Copper-molybdenum alloy wire for electronic devices, manganese plating process and manganese plating solution
By preparing a copper-molybdenum alloy wire containing Mo and Cu and plating a Mn layer on its surface, the problem of insufficient coating process and service life of MuCu alloy in the field of electronic devices in the existing technology is solved, and the control of high-voltage and high-power current is realized. The tolerance and coating life are significantly improved.
Patent Information
- Application Number
- CN202311838079.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-28
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-12-28
AI Technical Summary
In the application of existing MuCu alloys in the field of electronic devices, especially in the field of high-performance and high-power electronic devices, the process and service life of the plating layer have not been effectively improved, and it is difficult to meet the impact requirements of long-term high-density current and high voltage. .
A copper-molybdenum alloy wire containing 10-30% Mo element and 70-90% Cu element is used, and the Mn layer is plated on the surface. Molybdenum powder is prepared through a specific preparation process including screening, mixing powder granulation, and pressing. Molding, sintering, wire drawing and manganese plating processes control the distribution of Mo and Cu and the quality of the coating.
Significantly improve the thermal shock resistance and service life of copper-molybdenum alloy wire, improve the ability to withstand high voltage and high power current, extend the life of the plating layer and maintain high conductivity and strength.
Smart Images

Figure CN117758104B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a high-performance copper alloy for electronics and a method for manufacturing the same, and more particularly to a molybdenum-copper alloy, and more particularly to a copper-molybdenum alloy wire for electronic devices, a manganese plating process thereof, and a manganese plating solution used in manufacturing the molybdenum-copper alloy. Background Art
[0002] With the country's emphasis on high-tech industries, research on electronic devices, chips and semiconductor devices has received widespread attention in recent years. In the use of high-power semiconductor electronic devices, such as IGBT, due to the long-term high-load operation of high-power and high-current devices, higher and higher requirements are placed on the use of their metal accessories. For example, the wiring used by IGBT requires good protection for the wiring to be suitable for long-term high-density current and high-voltage impact.
[0003] MuCu alloys have been widely used in conductor materials for high-intensity magnetic fields, heat exchange materials, lead frame materials, contact wires, etc. With the development of high-tech industries, the comprehensive performance requirements for copper and molybdenum-copper alloys are getting higher and higher.
[0004] There have been reports on the research of MuCu alloy. For example, Chinese patent publication CN117051283A proposes a low-molybdenum-content molybdenum-copper alloy and a preparation method thereof, comprising the following steps: selecting molybdenum and copper by weight percentage and crushing them, wherein the particle size of the molybdenum powder is selected to be 5 microns, and the particle size of the copper powder is selected to be 5 microns; mixing the molybdenum powder and the copper powder evenly to obtain a mixed powder; pressing the mixed powder into a predetermined shape; sintering the mixed powder of the predetermined shape; performing staged heat preservation during sintering heating and cooling to obtain the low-molybdenum-content molybdenum-copper alloy. The present invention effectively controls the diffusion and migration of molybdenum and copper during the sintering process, thereby optimizing the microstructure of the alloy and improving its uniformity; by gradually heating and cooling during the sintering process, the cracks and defects caused by thermal stress in the sintered body can be effectively reduced, thereby improving the thermal shock resistance of the alloy. However, this type of research has not made research on the application needs in the field of electronic devices, especially in the field of high-performance and high-power electronic devices (such as IGBT power devices), nor has it made further improvements on the process and service life of the MoCu alloy coating.
[0005] Therefore, there is still a need for improvement and development of the existing related technologies. Summary of the invention
[0006] The present invention focuses on improving one or more of the above-mentioned deficiencies in the prior art. The first aspect of the present invention relates to a copper-molybdenum alloy wire for electronic devices, the copper-molybdenum alloy wire comprising 10-30% by mass of Mo element and 70-90% by mass of Cu element, and the surface of the copper-molybdenum alloy wire has a Mn coating, and the copper-molybdenum alloy wire is prepared by the following method:
[0007] Step 1) Screening and preparing molybdenum powder: Mo powder with a particle size of 2.5 to 3.0 μm is selected, and a pneumatic crushing device is used to de-agglomerate the powder;
[0008] Step 2) Preparation of alloy powder: taking copper powder with a particle size of 4.0-5.0 μm, mixing it with the molybdenum powder of step 1), adding water and a binder to mix into a slurry; wherein the mass ratio of molybdenum powder to copper powder is controlled to be (1-3):(9-7), followed by granulation, and drying to obtain spherical molybdenum-copper powder with a diameter of 100 μm to 200 μm;
[0009] Step 3) pressing: the spherical molybdenum copper powder prepared in step 2) is pressed using a pressing machine to obtain a compact;
[0010] Step 4) removing the binder: placing the green compact prepared in step 3) into a furnace and heating it to remove the binder to obtain a green compact;
[0011] Step 5) sintering: sintering in a furnace, the atmosphere is hydrogen, the sintering temperature is controlled at 900-1000° C., the heating rate is 10-30° C. / min, and the sintering time is 30-90 minutes to obtain an alloy columnar blank;
[0012] Step 6) The alloy columnar blank in step 5) is subjected to unidirectional wire drawing and annealing to obtain a MoCu alloy wire body; thereafter, the surface of the MoCu alloy wire is plated with Mn to obtain the copper-molybdenum alloy wire for electronic devices.
[0013] In a further preferred technical solution, the surface of the MoCu alloy wire is plated with Mn by the following steps:
[0014] Prepare a CuMo alloy plating solution, the CuMo alloy plating solution is composed of: 50-200 g / L manganese sulfate, 50-150 g / L ammonium sulfate, 5-15 g / L selenium dioxide, 1-5 g / L first auxiliary agent, 1-5 g / L second auxiliary agent, the plating solution is prepared with deionized water, and the pH value is controlled between 5 and 7;
[0015] The alloy wire in step 6) is placed in the prepared CuMo alloy plating solution for Mn plating; wherein,
[0016] The first auxiliary agent is selected from one imidazole compound or a combination of multiple imidazole compounds, and the second auxiliary agent is selected from soluble persulfate.
[0017] In a further optional technical solution, steps 1) to 6) are implemented by the following process:
[0018] Step 1) Screening and preparing molybdenum powder: Select Mo powder with a particle size of 2.5 to 3.0 μm and a loose bulk density of about 1.20-1.30 g / cm 3 ; Thereafter, the powder is subjected to a deagglomeration step using a jet crushing device to render it in an unagglomerated state;
[0019] Step 2) Preparation of alloy powder: particle size of 4.0-5.0 μm, bulk density of 2.0-2.5 g / cm 3 The fine copper powder is mixed with the non-agglomerated molybdenum powder in step 1), and water and PEG20000 are added as a binder to form a slurry; wherein the mass ratio of molybdenum powder: copper powder is controlled to be 3:7, the amount of water added is 20-50% of the total mass of the non-agglomerated molybdenum powder and the copper powder; the amount of the binder added is 0.5-2% of the total mass of the non-agglomerated molybdenum powder and the copper powder; the slurry is spray-dried and granulated under a nitrogen protective atmosphere, wherein the nozzle diameter used for spray granulation is 1-3mm, the slurry pressure is 500-1000KPa, the drying temperature is 150-200°C, and after drying, spherical molybdenum-copper powder with a diameter of 110μm to 160μm is obtained;
[0020] Step 3) pressing: the spherical molybdenum copper powder prepared in step 2) is pressed using an automatic pressing machine with a pressure of 50-70 tons and a speed of 10-20 Hz to obtain a compact;
[0021] Step 4) removing the binder: placing the green compact prepared in step 3 into a furnace and heating it to remove the binder, the atmosphere is nitrogen, the temperature is 500 to 550° C., and the debinding time is 0.5 to 2 hours to obtain a green compact;
[0022] Step 5) sintering: placing the blank in a furnace for sintering, the atmosphere is hydrogen, the sintering temperature is controlled at 900-980° C., the heating rate is 20-50° C. / min, and the sintering time is 30-90 minutes to obtain an alloy columnar blank;
[0023] Step 6) The alloy columnar blank described in step 5 is subjected to unidirectional wire drawing, and an online annealing process is implemented during the wire drawing process. The annealing temperature is controlled at 200-250°C to achieve an aging effect. After wire drawing, it is wound to obtain a MoCu alloy wire body; thereafter, the surface of the MoCu alloy wire is plated with Mn to obtain the copper-molybdenum alloy wire for electronic devices.
[0024] In a further optional technical solution, the surface of the MoCu alloy wire is plated with Mn by the following steps:
[0025] A CuMo alloy plating solution is prepared, which is composed of the following components: 150 g / L manganese sulfate, 100 g / L ammonium sulfate, 15 g / L selenium dioxide, 5 g / L first auxiliary agent, and 5 g / L second auxiliary agent, prepared with deionized water; wherein ammonia and / or boric acid (HBO 3 ) Adjust the pH value to 5-7;
[0026] The MoCu alloy wire is polished, alkaline washed for degreasing, and acid washed for activation, and then immersed in a manganese plating solution for 3-5 minutes, followed by electrolytic plating; during the electrolytic plating process, the deposition current density is 1-5A / dm 2 , the deposition temperature is 30-60°C, and the deposition time is 5-20min; then the electroplated coiled copper wire is placed in a tubular atmosphere furnace, argon gas is passed in advance to replace the air in the system, and then the temperature is increased at a heating rate of 1-10°C / min, and heat treated at 500-600°C for 1-3h. During the whole process, the argon flow rate is maintained at 10-100mL / min to obtain the copper-molybdenum alloy wire for electronic devices.
[0027] In a further optional technical scheme, the first auxiliary agent is selected from a mixture of a triazole compound and a tetrazole compound, the triazole compound is selected from one or more of 1,2,3-triazole, 1,2,4-triazole, tolyltriazole, and 4-amino-1,2,4-triazole; the tetrazole compound is an aminotetrazole compound, which is selected from one or more of 5-aminotetrazole, 5-amino-1-phenyltetrazole, 5-amino-1-(1-naphthyl)tetrazole, 1-methyl-5-aminotetrazole, and 1,5-diaminotetrazole.
[0028] In a further preferred technical solution, the first auxiliary agent is a mixture of 1,2,4-triazole and 5-aminotetrazole, and preferably, the mass ratio of 1,2,4-triazole to 5-aminotetrazole is 1:1.
[0029] In a second aspect of the present invention, a process for manufacturing a copper-molybdenum alloy wire for electronic devices is provided, wherein a Mn coating is plated on a substrate of the copper-molybdenum alloy wire, and the method comprises the following steps:
[0030] Step 1) Screening and preparing molybdenum powder: Mo powder with a particle size of 2.5 to 3.0 μm is selected, and a pneumatic crushing device is used to de-agglomerate the powder;
[0031] Step 2) Preparation of alloy powder: taking copper powder with a particle size of 4.0-5.0 μm, mixing it with the molybdenum powder of step 1), adding water and a binder to mix into a slurry; wherein the mass ratio of molybdenum powder to copper powder is controlled to be (1-3):(9-7), followed by granulation, and drying to obtain spherical molybdenum-copper powder with a diameter of 100 μm to 200 μm;
[0032] Step 3) pressing: the spherical molybdenum copper powder prepared in step 2) is pressed using a pressing machine to obtain a compact;
[0033] Step 4) removing the binder: placing the green compact prepared in step 3) into a furnace and heating it to remove the binder to obtain a green compact;
[0034] Step 5) sintering: sintering in a furnace, the atmosphere is hydrogen, the sintering temperature is controlled at 900-1000° C., the heating rate is 10-30° C. / min, and the sintering time is 30-90 minutes to obtain an alloy columnar blank;
[0035] Step 6) The alloy columnar blank in step 5) is subjected to unidirectional wire drawing and annealing to obtain a MoCu alloy wire; thereafter, the surface of the MoCu alloy wire is plated with Mn to obtain the copper-molybdenum alloy wire for electronic devices.
[0036] In a preferred technical solution, the surface of the MoCu alloy wire is plated with Mn by the following steps:
[0037] A CuMo alloy plating solution is prepared, which is composed of the following components: 150 g / L manganese sulfate, 100 g / L ammonium sulfate, 15 g / L selenium dioxide, 5 g / L first auxiliary agent, and 5 g / L second auxiliary agent, prepared with deionized water; wherein ammonia or boric acid (HBO 3 ) Adjust the pH value to 5-7;
[0038] The MoCu alloy wire is polished, alkaline washed for degreasing, and acid washed for activation, and then immersed in a manganese plating solution for 3-5 minutes, followed by electrolytic plating; during the electrolytic plating process, the deposition current density is 1-5A / dm 2 , the deposition temperature is 30-60°C, and the deposition time is 5-20min; then the electroplated coiled copper wire is placed in a tubular atmosphere furnace, argon gas is passed in advance to replace the air in the system, and then the temperature is increased at a heating rate of 1-10°C / min, and heat treated at 500-600°C for 1-3h. During the whole process, the argon flow rate is maintained at 10-100mL / min to obtain the copper-molybdenum alloy wire for electronic devices.
[0039] In a preferred technical solution, the process produces the copper-molybdenum alloy wire for electronic devices described in any one of the first aspects of the present invention.
[0040] In another aspect of the present invention, a manganese plating solution suitable for preparing a copper-molybdenum alloy wire for electronic devices is also provided, the manganese plating solution comprising:
[0041] Manganese sulfate 50-200g / L, ammonium sulfate 50-150g / L, selenium dioxide 5-15g / L, first auxiliary agent 1-5g / L, second auxiliary agent 1-5g / L; the pH value of the manganese plating solution is between 5-7; wherein
[0042] The first auxiliary agent is selected from a mixture of a triazole compound and a tetrazole compound, the triazole compound is selected from one or more of 1,2,3-triazole, 1,2,4-triazole, tolyltriazole, 4-amino-1,2,4-triazole; the tetrazole compound is an aminotetrazole compound, which is selected from one or more of 5-aminotetrazole, 5-amino-1-phenyltetrazole, 5-amino-1-(1-naphthyl)tetrazole, 1-methyl-5-aminotetrazole, and 1,5-diaminotetrazole.
[0043] According to the copper-molybdenum alloy, preparation method and process for applying Mn coating provided by the present invention, a copper-molybdenum alloy wire suitable for high-end electronic devices, especially for IGBT semiconductor module (high-power IGBT) wiring is provided. The wire effectively controls the Mo particles and distribution in the CuMo alloy through a specific static pressure preparation process, and significantly improves the protection of the Mn coating on the wire and its service life through a specific Mn plating and appropriate surface corrosion process. In the application of high-voltage and high-power current IGBT semiconductor modules, the overall service life and efficiency of the IGBT semiconductor module are effectively improved, and the strength of the wire and the coating are maintained for a long time without cracking, blistering or discoloration while maintaining high conductivity.
[0044] It should be noted that the product and process of the present invention may include the above steps and other related steps. In an optional or preferred scheme, the scheme of the present invention may only include the above steps or components, no longer include other steps and components, or do not significantly include other main steps or main components. In addition, the steps should be performed in a sequential order in the optional scheme, and the components and steps of the present invention can be implemented independently or arbitrarily superimposed and combined with each other.
[0045] In the following, the technical solutions and advantages of the present invention will be explained and described in more detail in conjunction with specific implementation methods. It should be understood that the contents presented in the specification and specific implementation methods are only for the purpose of more clearly illustrating the technical solutions and advantages of the present invention, and do not limit the protection scope of the present invention. Those skilled in the art can obtain the changed technical solutions based on the disclosure of the specification for various reasonable transformations. As long as they do not deviate from the spirit of the present invention, the various changed technical solutions should be understood to be included in the protection scope of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] The accompanying drawings are used to provide a further understanding of the technical solution of the present disclosure and constitute a part of the specification. Together with the specific embodiments of the present application, they are used to explain the technical solution of the present disclosure and do not constitute a limitation on the technical solution of the present disclosure.
[0047] Figure 1 It is the X-ray diffraction pattern of the CuMo manganese-plated wire prepared in Example 1 and Example 2 of the present invention;
[0048] Figure 2 is a cross-sectional view of the CuMo manganese-plated wire used in Examples 1 and 2 of the present invention;
[0049] Figure 3 is a schematic diagram of an IGBT device using the wire material of Example 2;
[0050] Figure 4 is a SEM scanning electron microscope photograph of a longitudinal section of a CuMo-plated Mn wire prepared according to a comparative example.
[0051] Description of the accompanying drawings of the present invention:
[0052] 1-Silicon carbide IGBT module body; 2-CuMo coated Mn wire 2; 3-CuMo wire body; 4-Mn coating; 5-wear-resistant insulation layer; 6-protective film layer; 7-wire protection structure. DETAILED DESCRIPTION
[0053] The present invention is described in more detail hereinafter to facilitate understanding of the invention.
[0054] Before describing the specific implementation scheme, it should be noted that those skilled in the art can select appropriate raw materials according to the enlightenment and teaching of the present disclosure, and use relevant testing equipment to perform relevant tests and obtain corresponding results. For raw materials without specific manufacturers or pathways, those skilled in the art can select raw materials that meet corresponding requirements as reaction starting materials according to the disclosure and requirements of this specification. The reaction raw materials of the process part compounds are derived from the initial products synthesized in the preamble step of the present invention, which can also be understood according to the present disclosure.
[0055] The press used in the powder preparation was an automatic press machine using the 0PC-60TG model fully automatic powder press produced by Nanjing Dongtian Precision Machinery Co., Ltd.;
[0056] The silicon carbide IGBT module used in the embodiment comes from Infineon The FZ600R65KF2 module.
[0057] In the electron microscope test of the embodiment of the present invention, a scanning electron microscope JSM-IT200 of JEOL Company of Japan was used for testing;
[0058] X-ray diffraction was performed using an X-ray analyzer model Rigaku R-AXIS-SPIDER manufactured by Rigaku Corporation.
[0059] This embodiment will describe the treatment process of electrophoretic paint wastewater, and the important equipment and devices used in the related process. For equipment or devices that can be obtained in the existing technology, or equipment and devices that the skilled person in the art knows should be used, the specific description will be omitted in order to omit unnecessary length of the specification. The skilled person in the art can obtain the specific process or equipment for the corresponding implementation based on the description of the specification of the present invention and the relevant professional and technical knowledge in the field.
[0060] Example 1
[0061] This embodiment describes a process for preparing a MoCu alloy wire, wherein specifically an alloy wire whose main component is Mo10Cu90 is prepared.
[0062] Step 1) Screening and preparing molybdenum powder: Mo powder with a particle size of 2.5 to 3.0 μm (measured by Fisher particle size measurement method) and a loose bulk density of about 1.25-1.28 g / cm 3 The powder is deagglomerated using air flow crushing equipment to keep it in an unagglomerated state as much as possible.
[0063] The inventors found that selecting molybdenum powder within the above-mentioned particle size range is beneficial to the distribution of Mo particles and Cu in the subsequent MoCu wire, especially on the surface of the wire; if the particle size is too large, the surface of the wire is prone to excessive roughness during long-term high-intensity use; if the particle size is too small, it cannot be guaranteed that the wire body is effectively and firmly combined with the Mn coating.
[0064] Step 2) Preparation of alloy powder: The particle size is 4.0-5.0 μm (Fisher particle size) and the bulk density is 2.3 g / cm 3 The fine copper powder is mixed with the non-agglomerated molybdenum powder of step 1, and water and PEG20000 binder are added to form a slurry. The mass ratio of molybdenum powder: copper powder is controlled to be 1:9, the amount of water added is 40% of the total mass of the non-agglomerated molybdenum powder and copper powder; the amount of binder added is 1% of the total mass of the non-agglomerated molybdenum powder and copper powder. The slurry is spray-dried and granulated under a nitrogen protective atmosphere, wherein the nozzle diameter used for spray granulation is 1.00mm, the slurry pressure is 950KPa, the drying temperature is 180℃, and spherical molybdenum-copper powder with a diameter of 110μm to 160μm is obtained after drying.
[0065] Step 3) pressing: the spherical molybdenum copper powder prepared in step 2 is pressed by an automatic pressing machine, the pressure of the pressing machine is 60 tons, the speed is 20Hz, and a pressed blank is obtained; the specific pressing steps are: the spherical molybdenum copper powder is added to the feed bin; the spherical molybdenum copper powder in the feed bin flows into the mold through the pipeline under the action of gravity; the automatic pressing machine presses according to the set speed and pressure, here 10 pieces are pressed per minute, the pressure is 60t (single piece press time is 2s, the pressure holding time is 2s, and the pressure relief and unloading time is 2s); wherein the blank is automatically demolded after the pressing is completed;
[0066] Step 4) removing the binder: placing the green compact prepared in step 3 into a furnace and heating it to remove the binder, the atmosphere is nitrogen, the temperature is 550°C, and the debinding time is 1 hour to obtain a green compact;
[0067] Step 5) Sintering: Sintering in a furnace, the atmosphere is hydrogen, the sintering temperature is controlled at 950°C, the heating rate is 30°C / min, and the sintering time is 60 minutes. The Mo10Cu90 alloy columnar blank with a diameter of φ20*10mm is produced by the method, and the density can reach more than 99.5%. 100 finished products are sampled, and the diameter range is 20.00±0.02mm, the height range is 10.00±0.01mm, and the density can reach 9.31g / cm 3 .
[0068] Step 6) The alloy columnar blank in step 5 is subjected to unidirectional wire drawing, and an online annealing method is used during the wire drawing process to achieve an aging effect. The online annealing voltage is 80V, the annealing temperature is 220°C, and the speed is 300m / min. After wire drawing, winding is performed to obtain a MoCu alloy wire, which is ready to enter the following manganese plating process.
[0069] Example 2
[0070] This embodiment describes the preparation of a manganese plating solution and the process of Mn plating on a MoCu alloy wire.
[0071] First, it is necessary to prepare a CuMo alloy plating solution. The preferred manganese plating solution of this embodiment is composed of the following components:
[0072] Manganese sulfate 150g / L, ammonium sulfate 100g / L, selenium dioxide 15g / L, first auxiliary agent 5g / L, second auxiliary agent 5g / L. Use ammonia or boric acid (HBO 3 ) adjust the pH value to 5-7, and the manganese plating solution is prepared using deionized water.
[0073] The inventors describe the first auxiliary agent and the second auxiliary agent in detail in this embodiment.
[0074] The first auxiliary agent is composed of an organic compound that controls alloy corrosion. Specifically, in Example 1, a triazole compound (1,2,4-triazole) and an aminotetrazole compound (5-aminotetrazole) are used in a mass ratio of 1:1.
[0075] The second auxiliary agent is composed of persulfate which affects the etching rate. In this embodiment, the second auxiliary agent is selected from ammonium persulfate (NH 4 ) 2 S 2 O 8 ).
[0076] Thereafter, the CuMo alloy was plated with manganese in the following process. The MoCu alloy wire in Example 1 was polished, alkali washed to remove oil, and acid washed to activate (using 5%wt dilute sulfuric acid), then immersed in a manganese plating solution, immersed in the manganese plating solution for 5 minutes, and then electrolytically plated. During the electroplating process, the deposition current density was 3A / dm 2 The deposition temperature is 45°C and the deposition time is 15min. The electroplated coiled copper wire is placed in a tubular atmosphere furnace. After the air in the system is replaced by argon gas in advance, the temperature is increased at a rate of 5°C / min and heat treated at 550°C for 1h. The argon flow rate is maintained at 30-50mL / min during the whole process.
[0077] The CuMo-plated Mn sample completed in Example 2 was subjected to X-ray detection. The results are as follows: Figure 1As shown. The CuMo-plated Mn sample with good crystallization performance was obtained. The resistivity test showed 0.050Ω.mm 2 .m -1 , can be used as a good Cu-based high-performance wire.
[0078] The cross-section of the CuMo-plated Mn sample of Example 2 (including the boundary between the Mn plating layer and the copper wire substrate) was used to prepare a cross-section polished alloy sample, and a SEM scanning electron microscope test was performed. The results are as follows: Figure 2 shown.
[0079] exist Figure 2 In the sample shown, the inventor found that after the electroplating process of the Mn plating solution of the present invention, an obvious interface layer of Mn and CuMo alloy appeared at the interface of Mn and CuMo alloy (the bright part in the figure, the upper part of the interface is mainly the Mn coating, and the lower part of the interface is mainly the CuMo substrate part). In the interface layer, a small part of the substrate part protrudes upward (as shown by the arrow in the figure) and enters the interface layer part. In this regard, the inventor does not want to be bound by any theoretical explanation. However, it is possible that the surface of the CuMo alloy of the present invention is micro-corroded during the initial immersion process in the electroplating solution, a small amount of Cu is etched and some Mo particles are protruded, and micro-protrusions are formed at the interface of Mn and the alloy wire formed in the subsequent electroplating process, which promotes the combination of the Mn coating and the Cu-Mo alloy wire. This wire is used in semiconductor devices, especially in the wire application of high-power devices (such as IGBT) devices, and the quality of the coating and the wire is significantly maintained, and the service life of the coating is extended.
[0080] Example 3
[0081] This embodiment will briefly describe the application of the CuMo-plated Mn wire of embodiment 2 in an IGBT module. Specifically, the CuMo-plated Mn wire of embodiment 2 is applied to the copper busbar structure of the silicon carbide IGBT module. Figure 3 This structure is briefly shown in Figure 3 In the schematic diagram, the silicon carbide IGBT module and its copper busbar structure include a silicon carbide IGBT module body 1, a CuMo-plated Mn wire 2 (CuMo alloy wire body) is provided on one side of the high-performance silicon carbide IGBT module body 1, as described in embodiments 1 and 2 of the present invention, the CuMo-plated Mn wire 2 of the embodiment of the present invention is composed of a CuMo wire body 3 and a Mn coating 4 (schematic diagram, the thickness of which does not necessarily represent the actual thickness ratio of the two). Of course, the CuMo-plated Mn wire 2 can also be provided with a wear-resistant insulating layer 5, a protective film layer 6 and other structures according to the needs of semiconductor engineering. A wire protection structure 7 can also be provided at the interface between the CuMo-plated Mn wire 2 and the silicon carbide IGBT module body 1.
[0082] In the implementation scheme of the CuMo-plated Mn wire of the present invention, after long-term device testing by the inventors, the surface of the CuMo-plated Mn wire 2 can be free of blistering for more than 300 days, the Mn coating does not change color, and the Cu-Mo wire body always maintains a close bond with the Mn coating.
[0083] Comparative Example 1
[0084] In this experiment, different Mn plating solutions are mainly used to plate the CuMo body. In the following examples, the operation process is basically the same as that of Examples 1 and 2, except that the various implementation schemes of Comparative Example 1 use the following CuMo alloy plating solution components (the components in the plating solution are g / L), and then the corresponding CuMo alloy wire is applied to the wiring of the IGBT module of Example 3, and the corresponding test is performed:
[0085] Table 1: Different Mn plating solution compositions
[0086]
[0087]
[0088] It can be seen from the relevant experiments implemented by the inventor that the content of the first auxiliary and the second auxiliary components has an impact on the flat quality of the coating and the high quality of the Mn coating. When the content of the azole compound of the first auxiliary component increases, the coating causes blistering after a period of use, and the degree of maintaining the color of the Mn coating is limited. In the use of IGBT high-power devices, high temperature and high current put forward higher requirements for the protection of the wire body and the high quality of the Mn coating. The inventor does not want to be bound by any theory, but after research, the inventor believes that the combination of the first auxiliary and the second auxiliary components is conducive to the slight corrosion of the surface of the CuMo alloy wire, especially Cu is significantly more susceptible to corrosion than Mo (or Mo is almost not corroded), and the micro-corrosion phenomenon causes the Mo particles on the surface of the Cu-Mo alloy to have the opportunity to protrude slightly, thereby better combining with the Mn coating. When the azole compound of the first auxiliary component is increased, the corrosion rate rises, resulting in the surface of the wire body being too concave and convex, and the subsequent Mn coating may appear discontinuous or protruding in a large range, which is not conducive to protecting the quality and flatness of the Mn coating during the use of the IGBT wire with high temperature, high voltage and high current. In addition, when the content of the first auxiliary component is too low, although the etching effect may still be implemented, it may not lead to an effective micro-corrosion effect leading to micro-protrusions. Although it can maintain flatness and service life to a certain extent, it also leads to the problem of insufficient life in the long-term application of power devices. When there are too many persulfates in the second component, the inventors found that excessive corrosion may also occur, resulting in insufficient use efficiency and life. It is worth noting that when the component does not contain sulfate (such as ammonium sulfate) but only contains persulfate, the problem of insufficient protection of the Mn coating also occurs. The inventors realize that the presence of the sulfate solution component may have a buffering effect on the second component, which slows down the etching effect of the second auxiliary component. Of course, in the technical solution that does not use the first auxiliary component and the second auxiliary component (such as C-3), it is impossible to provide an effective process and product for improving the quality of the Mn coating.
[0089] The inventors conducted SEM tests on typical C-1 and C-2 samples. The results are shown in Figure 4 . Figure 4 The left side corresponds to sample C-1. In this sample, there is a large and discontinuous interface layer between CuMo and Mn, and there is no interface layer in some locations, resulting in the mixing of Mn, Cu-Mo matrix and Mn coating. This may be caused by the unevenness caused by the excessive etching rate. Sample C-2 ( Figure 4 The right side shows a very small cross-section with almost no protrusions and unevenness, which may be caused by insufficient difference in the degree of CuMo etching.
[0090] Example 4
[0091] This example mainly tests different auxiliary preparation components. In this experimental example, the technical scheme composed of Example 1 to Example 3 is basically implemented. The difference is that the specific first auxiliary agent and the second auxiliary agent are adjusted.
[0092]
[0093]
[0094] As can be seen from the test results of Example 4, the composite use of two structures of azole compounds is a relatively more optimal technical solution. When using auxiliary preparations of other structures (such as pyrroline compounds), the protective effect for the Mn coating decreases. This may be related to the Cu etching mechanism of different compounds. The change and use of the specific type of persulfate are not much different for the protective effect of the sample coating. In an embodiment of the present invention, a combination of a triazole compound and a tetrazolium compound is preferably used as the first auxiliary component, and the auxiliary components of sulfate and persulfate are matched.
[0095] According to the implementation scheme and technical contents recorded in the specification of the present invention, the present invention can at least provide the following technical solutions: Although the present disclosure includes specific embodiments, it is obvious to those skilled in the art that various formal and detailed replacements or changes can be made to these embodiments without departing from the gist and scope of the invention of the present claims and their equivalent technical solutions. The embodiments described herein should be considered to be illustrative only and not for the purpose of limitation. The description of the features and aspects in each embodiment is considered to be applicable to similar features and aspects in other embodiments. Therefore, the scope of the present disclosure should not be limited by the specific description, but by the technical solutions of the claims, and all changes within the scope of the claims and their equivalents are interpreted as being included in the technical solutions of the present disclosure.
Claims
1. A process for manufacturing a copper-molybdenum alloy wire for electronic devices, wherein a Mn coating is plated on a substrate of the copper-molybdenum alloy wire, It is characterized in that The process comprises the following steps: Step 1) Screening and preparing molybdenum powder: Mo powder with a particle size of 2.5 μm is selected, and the powder is deagglomerated using a jet crushing device; Step 2) Preparation of alloy powder: taking copper powder with a particle size of 4.0-5.0 μm, mixing it with the molybdenum powder of step 1), adding water and a binder to mix into a slurry; wherein the mass ratio of molybdenum powder to copper powder is controlled to be (1-3):(9-7), followed by granulation, and drying to obtain spherical molybdenum-copper powder with a diameter of 100 μm to 200 μm; Step 3) pressing: the spherical molybdenum copper powder prepared in step 2) is pressed using a pressing machine to obtain a compact; Step 4) removing the binder: placing the green compact prepared in step 3) into a furnace and heating it to remove the binder to obtain a green compact; Step 5) sintering: sintering in a furnace, the atmosphere is hydrogen, the sintering temperature is controlled at 900-1000° C., the heating rate is 10-30° C. / min, and the sintering time is 30-90 minutes to obtain an alloy columnar blank; Step 6) unidirectionally drawing the alloy columnar blank in step 5) and annealing it to obtain a MoCu alloy wire; thereafter, Mn is plated on the surface of the MoCu alloy wire to obtain the copper-molybdenum alloy wire for electronic devices; and The surface of the MoCu alloy wire is plated with Mn by the following steps: Prepare a CuMo alloy plating solution, the CuMo alloy plating solution is composed of: 50-200 g / L manganese sulfate, 50-150 g / L ammonium sulfate, 5-15 g / L selenium dioxide, 1-5 g / L first auxiliary agent, 1-5 g / L second auxiliary agent, the plating solution is prepared with deionized water, and the pH value is controlled between 5 and 7; wherein the first auxiliary agent is a mixture of 1,2,4-triazole and 5-aminotetrazole, and the mass ratio of 1,2,4-triazole to 5-aminotetrazole is 1:1, and the second auxiliary agent is selected from soluble persulfate; The alloy wire in step 6) is placed in the prepared CuMo alloy plating solution for Mn plating.
2. The manufacturing process of the copper-molybdenum alloy wire for electronic devices according to claim 1, wherein the surface of the MoCu alloy wire is plated with Mn, which is carried out by the following steps: A CuMo alloy plating solution is prepared, which is composed of the following components: 150 g / L manganese sulfate, 100 g / L ammonium sulfate, 15 g / L selenium dioxide, 5 g / L first auxiliary agent, and 5 g / L second auxiliary agent, and is prepared with deionized water; wherein the pH value is adjusted to 5-7 with ammonia water or boric acid; The MoCu alloy wire is polished, alkaline washed for degreasing, and acid washed for activation, and then immersed in a manganese plating solution for 3-5 minutes, followed by electrolytic plating; during the electrolytic plating process, the deposition current density is 1-5A / dm 2 , the deposition temperature is 30-60°C, and the deposition time is 5-20min; then the electroplated coiled copper wire is placed in a tubular atmosphere furnace, argon gas is passed in advance to replace the air in the system, and then the temperature is increased at a heating rate of 1-10°C / min, and heat treated at 500-600°C for 1-3h. During the whole process, the argon flow rate is maintained at 10-100mL / min to obtain the copper-molybdenum alloy wire for electronic devices.
3. The manufacturing process of the copper-molybdenum alloy wire for electronic devices according to claim 1 or 2, wherein the copper-molybdenum alloy wire comprises 10-30% by mass of the Mo element and 70-90% by mass of the Cu element, and the surface of the copper-molybdenum alloy wire has a Mn coating.