Semiconductor devices
By optimizing the thickness and structure of TaN and TiN layers in Group III nitride semiconductor devices, the diffusion of metal atoms is suppressed, the problems of electrode degradation and current collapse are solved, and gate electrodes with low on-resistance and high reliability are achieved.
Patent Information
- Application Number
- CN202280051723.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-21
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-07-21
AI Technical Summary
Existing Group III nitride semiconductor devices are prone to electrode degradation and reverse leakage current under high temperature and high voltage conditions, and are prone to current collapse, resulting in an increase in on-resistance and affecting device reliability.
A semiconductor device is designed whose gate electrode is composed of TaN layer and TiN layer. By optimizing the thickness and structure of these layers, it ensures that metal atoms do not diffuse under high temperature conditions and reduces energy level generation and current collapse. Z1+ is used The structure of Z2≥50nm ensures that the first barrier layer and the second barrier layer inhibit the diffusion of metal atoms in the wiring layer.
It achieves low on-resistance and high reliability under high temperature and high voltage conditions, reduces reverse leakage current and current collapse, and improves the heat resistance and Schottky barrier of the gate electrode.
Smart Images

Figure CN117769762B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a semiconductor device, and in particular to a Group III nitride semiconductor device using a Group III nitride semiconductor. Background Art
[0002] A III-nitride semiconductor device using a III-nitride semiconductor, particularly gallium nitride (GaN) or aluminum gallium nitride (AlGaN), has a high dielectric breakdown voltage due to the width of the band gap of the material. In addition, in a III-nitride semiconductor device, a heterostructure such as AlGaN / GaN is easily formed.
[0003] In the AlGaN / GaN heterostructure, a channel with a high concentration of electrons (hereinafter referred to as a "two-dimensional electron gas layer") is formed on the GaN layer side of the AlGaN / GaN interface through piezoelectric polarization caused by the lattice constant difference between the materials and the spontaneous polarization of AlGaN and GaN. The III-nitride semiconductor device using the channel of the two-dimensional electron gas layer is used in high-frequency power devices because of its relatively high electron saturation velocity, high insulation resistance, and high thermal conductivity. In addition, an electrode that is Schottky-bonded to AlGaN needs to be used as the gate electrode.
[0004] Regarding these III-group nitride semiconductor devices, in order to improve the characteristics, for the gate electrode, it is necessary to reduce the degradation of the electrode during high temperature operation and reduce the reverse leakage current. Therefore, for the material used in the gate electrode, it is preferred to use a material with a high melting point and a high work function. Preferably, by using this material, the heat resistance of the gate electrode and the height of the Schottky barrier are as high as possible. In this way, the degradation of the electrode during high temperature operation and the reverse leakage current are reduced, so that the reliability can be higher.
[0005] In addition, it is necessary to alleviate the phenomenon called current collapse, which is a unique issue of III-nitride semiconductor devices. Current collapse is a phenomenon in which on-resistance increases by applying high current and high voltage stress. This phenomenon occurs when electrons accelerated by high voltage stress are captured by crystal defects inside the III-nitride semiconductor device and energy levels existing at the film interface.
[0006] Patent Document 1 discloses the following semiconductor device: <0001> On the n-type GaN layer (in the a-axis direction), a tantalum nitride (TaN) layer with a high melting point and a N / Ta ratio of 1.00 of a NaCl structure formed by sputtering is formed, and the n-type GaN layer and the TaN layer are Schottky bonded. Through this structure, the TaN with a N / Ta ratio of 1.00 in the NaCl structure not only has a higher work function of 5.4eV, but also has a smaller lattice constant difference with the n-type GaN layer in the a-axis direction, so the work function is the largest, that is, the Schottky barrier is the largest. Therefore, it is possible to improve heat resistance and Schottky barrier, and obtain a gate electrode with higher reliability.
[0007] Fig.29 2 is a cross-sectional view showing the structure near the gate electrode of the semiconductor device (III-nitride semiconductor device) of Patent Document 2. Fig.29 As shown, in the semiconductor device of Patent Document 2, a buffer layer 102, a GaN layer 103a, and an AlGaN layer 104a are sequentially provided on a substrate 101. The semiconductor device has a two-dimensional electron gas layer 105 on the GaN layer 103a side by a heterostructure. In addition, a first insulating layer 211 is provided on the AlGaN layer 104a, and a first opening 211a is provided in the first insulating layer 211, in which the first insulating layer 211 is removed so as to expose the AlGaN layer 104a. Furthermore, a gate insulating layer 204 is provided so as to cover the first insulating layer 211 and the first opening 211a, and a TaN layer 411a is provided on the gate insulating layer 204 so as to cover the first opening 211a. The second insulating layer 212 is provided so as to cover the gate insulating layer 204 and the TaN layer 411a, and the second opening 212b is provided in the second insulating layer 212, in which the second insulating layer 212 is removed so as to expose a part of the TaN layer 411a. The titanium nitride layer (TiN layer 411b) and the first wiring layer 411c are sequentially stacked so as to cover the second opening 212b, that is, the semiconductor device includes a gate electrode 411 composed of the TaN layer 411a, the TiN layer 411b and the first wiring layer 411c. The semiconductor device of Patent Document 2 is a MIS (Metal-Insulator-Semiconductor) structure having a gate insulating layer 204, but can also be used as a MES (Metal-Semiconductor) structure. In this case, the semiconductor device of Patent Document 2 can improve heat resistance and increase Schottky barrier as described in Patent Document 1 even if the TaN layer 411 a and the AlGaN layer 104 a form a Schottky junction, thereby obtaining a gate electrode with high reliability.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2006-190749
[0011] Patent Document 2: Japanese Patent Application Publication No. 2013-201370 Summary of the invention
[0012] Problems to be solved by the invention
[0013] According to the above-mentioned patent document 2, a gate electrode 411 composed of a TaN layer 411a, a TiN layer 411b and a first wiring layer 411c is shown. In the method described in patent document 2, according to the thermal process in the manufacturing process, if the metal atoms of the first wiring layer 411c diffuse into the inside of the AlGaN layer 104a or the first insulating layer 211, an energy level is generated. Through the generated energy level, the Schottky barrier height decreases, or when a high voltage is applied between the source electrode and the drain electrode, the current collapses and the electrons are captured, and the on-resistance increases. Therefore, it is necessary to consider the thickness of the TaN layer 411a and the thickness of the TiN layer 411b so that even if the temperature is about 250°C to 500°C due to the thermal process in the manufacturing process, the metal atoms of the first wiring layer 411c do not diffuse from the first wiring layer 411c to the AlGaN layer 104a or the first insulating layer 211. However, Patent Documents 1 and 2 do not specify the thickness of the TaN layer 411 a or the TiN layer 411 b , and the barrier property for suppressing diffusion of metal atoms of the first wiring layer 411 c into the AlGaN layer 104 a or the first insulating layer 211 is unclear.
[0014] The present disclosure has been made in view of such a problem, and an object of the present disclosure is to provide a semiconductor device having a gate electrode with high reliability and low on-resistance.
[0015] Means used to solve problems
[0016] To achieve the above object, a technical solution of the semiconductor device of the present disclosure includes: a substrate; a first nitride semiconductor layer provided on the substrate; a second nitride semiconductor layer having a larger bandgap than the first nitride semiconductor layer and provided on the first nitride semiconductor layer; a first insulating layer provided on the second nitride semiconductor layer; a source electrode and a drain electrode provided at an interval and respectively penetrating the first insulating layer and electrically connected to the first nitride semiconductor layer; an opening provided in the first insulating layer between the source electrode and the drain electrode to expose the second nitride semiconductor layer; and a gate electrode provided at an interval from the source electrode and the drain electrode and in contact with the second nitride semiconductor layer at the opening; the gate electrode includes: a first barrier layer made of TaN with a layer thickness of Z1 and in Schottky contact with the second nitride semiconductor layer; a second barrier layer provided in contact with the first barrier layer and made of TiN or WN with a layer thickness of Z2; and a wiring layer provided in contact with the second barrier layer; Z1 and Z2 satisfy 200nm ≥ Z1 + Z2 ≥ 50nm, Z1 < Z2, and 50nm > Z1 > 3nm.
[0017] Advantages of the Invention
[0018] According to the semiconductor device of the present disclosure, a semiconductor device having a gate electrode with high reliability and low on-resistance can be obtained. Description of the Drawings
[0019] Figure 1 It is a cross-sectional view showing the structure of the semiconductor device of Embodiment 1.
[0020] Figure 2 It is Figure 1 a cross-sectional view showing an enlarged view of Region II.
[0021] Figure 3 It is a cross-sectional view showing the vicinity of the gate electrode of the semiconductor device of the study example of Embodiment 1.
[0022] Figure 4 It is a graph showing the results of the thickness dependence of the reverse leakage current of the gate electrode of the semiconductor device of the study example of Embodiment 1 and the on-resistance at high voltage / on-resistance at low voltage of the TiN layer.
[0023] Figure 5 It is another graph showing the results of the thickness dependence of the reverse leakage current of the gate electrode of the semiconductor device of the study example of Embodiment 1 and the on-resistance at high voltage / on-resistance at low voltage of the TiN layer.
[0024] Figure 6 It is a cross-sectional view showing the process of the manufacturing method of the semiconductor device of Embodiment 1.
[0025] Figure 7The diagram is a cross-sectional view showing the steps of the method for manufacturing the semiconductor device according to the first embodiment.
[0026] Figure 8 The diagram is a cross-sectional view showing the steps of the method for manufacturing the semiconductor device according to the first embodiment.
[0027] Fig. 9 The diagram is a cross-sectional view showing the steps of the method for manufacturing the semiconductor device according to the first embodiment.
[0028] Fig.10 The diagram is a cross-sectional view showing the steps of the method for manufacturing the semiconductor device according to the first embodiment.
[0029] Fig.11 The diagram is a cross-sectional view showing the steps of the method for manufacturing the semiconductor device according to the first embodiment.
[0030] Fig.12 The diagram is a cross-sectional view showing the steps of the method for manufacturing the semiconductor device according to the first embodiment.
[0031] Fig.13 The diagram is a cross-sectional view showing the steps of the method for manufacturing the semiconductor device according to the first embodiment.
[0032] Fig.14 This is a cross-sectional view of a semiconductor device according to a second embodiment.
[0033] Fig.15 This is a cross-sectional view showing the structure of the semiconductor device in the vicinity of the gate electrode according to the first modification of the second embodiment.
[0034] Fig.16 This is a cross-sectional view showing a structure near a gate electrode of a semiconductor device according to a second variation of the second embodiment.
[0035] Fig.17 This is a cross-sectional view showing a structure near a gate electrode of a semiconductor device according to a third variation of the second embodiment.
[0036] Fig.18 Yes Fig.17 A cross-sectional view showing an enlarged view of region XVIII.
[0037] Fig.19 This is a cross-sectional view showing a structure near a gate electrode of a semiconductor device according to a fourth variation of the second embodiment.
[0038] Fig. 20 It is a cross-sectional view showing the steps of the method for manufacturing a semiconductor device according to the second embodiment.
[0039] Fig.21 It is a cross-sectional view showing the steps of the method for manufacturing a semiconductor device according to the second embodiment.
[0040] Fig. 22 It is a cross-sectional view showing the steps of the method for manufacturing a semiconductor device according to the second embodiment.
[0041] Fig.23 It is a cross-sectional view showing the steps of the method for manufacturing a semiconductor device according to the second embodiment.
[0042] Fig.24 It is a cross-sectional view showing the steps of the method for manufacturing a semiconductor device according to the second embodiment.
[0043] Fig.25 It is a cross-sectional view showing the steps of the method for manufacturing a semiconductor device according to the second embodiment.
[0044] Fig.26 It is a cross-sectional view showing the steps of the method for manufacturing a semiconductor device according to the second embodiment.
[0045] Fig. 27 It is a cross-sectional view showing the steps of the method for manufacturing a semiconductor device according to the second embodiment.
[0046] Fig.28 It is a cross-sectional view showing the steps of the method for manufacturing a semiconductor device according to the second embodiment.
[0047] Fig.29 This is a cross-sectional view showing the structure of the semiconductor device of Patent Document 2 near the gate electrode. DETAILED DESCRIPTION
[0048] The inventors have repeatedly conducted special studies and experiments to provide a semiconductor device having a gate electrode with high reliability and low on-resistance. As a result, the inventors have conceived the following semiconductor device and the like.
[0049] Hereinafter, a specific example of a semiconductor device or the like of a technical solution of the present disclosure is described with reference to the accompanying drawings. The embodiments described here all represent a specific example of the present disclosure. Therefore, the numerical values, shapes, constituent elements, configurations and connection forms of constituent elements, steps (processes) and the order of steps, etc. shown in the following embodiments are used as examples and are not intended to limit the present disclosure. Therefore, the constituent elements of the following embodiments that are not described in the independent claims are described as arbitrary constituent elements.
[0050] In addition, each figure is a schematic diagram and does not necessarily illustrate the exact figure. In each figure, the same reference numerals are given to substantially the same structure, and repeated descriptions are omitted or simplified.
[0051] In addition, in this specification, the terms "upper" and "lower" in the structure of the semiconductor device do not refer to the upper side (vertically above) and the lower side (vertically below) in absolute spatial identification, but are terms defined by relative positional relationships based on the stacking order in the stacking structure. In addition, the terms "upper" and "lower" are not only applied to the case where two components are arranged at a distance from each other and there is another component between the two components, but also to the case where two components are arranged closely to each other so that the two components are in contact.
[0052] In addition, in this specification and the drawings, the x-axis, y-axis, and z-axis represent three axes of a three-dimensional orthogonal coordinate system. In each embodiment, two axes parallel to the upper surface of the substrate of the semiconductor device are defined as the x-axis and the y-axis, and a direction orthogonal to the upper surface is defined as the z-axis direction. In the embodiments described below, the positive z-axis direction is sometimes referred to as the upper direction, and the negative z-axis direction is sometimes referred to as the lower direction.
[0053] In this specification, “planar observation” means observing a substrate included in a semiconductor device from the positive direction of the z-axis.
[0054] (Implementation Method 1)
[0055] First, use Figure 1 and Figure 2 The semiconductor device according to the first embodiment will be described. Figure 1 1 is a cross-sectional view showing the structure of the semiconductor device 100A according to the first embodiment. Figure 2 Yes Figure 1 A cross-sectional view showing an enlarged area II of FIG. 1 . In the present embodiment, a case where the semiconductor device 100A is a high electron mobility transistor (HEMT) having a Schottky junction gate structure will be described.
[0056] like Figure 1 As shown, the semiconductor device 100A includes a substrate 101, a buffer layer 102, a first nitride semiconductor layer 103, a second nitride semiconductor layer 104, a two-dimensional electron gas layer 105, a first insulating layer 201, an opening (here, the first opening 201a), a second insulating layer 202, a second opening 202b, a third opening 202c, a fourth opening 202d, a source electrode 301 composed of an ohmic electrode 301a and a second wiring layer 301b, a drain electrode 302 composed of the ohmic electrode 302a and the second wiring layer 302b, a gate electrode 401 including a first barrier layer 401a, a second barrier layer 401b and a wiring layer (here, the first wiring layer 401c), and a field plate electrode 501 composed of a third barrier layer 501b and a third wiring layer 501c.
[0057] In this embodiment, the substrate 101 is, for example, a substrate made of Si. The substrate 101 is not limited to a substrate made of Si, and may be a substrate made of sapphire, SiC, GaN, AlN, or the like.
[0058] The buffer layer 102 is provided on the substrate 101. In the present embodiment, the buffer layer 102 is, for example, a III-nitride semiconductor layer having a layer thickness of 2 μm, and more specifically, a III-nitride semiconductor layer formed by a plurality of stacked structures composed of AlN and AlGaN. In addition, the layer thickness is the thickness of the layer in the z-axis direction. The buffer layer 102 may also be composed of a single layer or multiple layers of a III-nitride semiconductor such as GaN, AlGaN, AlN, InGaN or AlInGaN.
[0059] The first nitride semiconductor layer 103 is provided on the substrate 101, more specifically, on the buffer layer 102. In the present embodiment, the first nitride semiconductor layer 103 is composed of GaN with a layer thickness of 200 nm, for example. In addition, the first nitride semiconductor layer 103 is not limited to GaN, and may also be composed of a group III nitride semiconductor such as InGaN, AlGaN or AlInGaN. In addition, the first nitride semiconductor layer 103 may contain n-type impurities.
[0060] The second nitride semiconductor layer 104 has a larger band gap than the first nitride semiconductor layer 103 and is provided on the first nitride semiconductor layer 103. In this embodiment, the second nitride semiconductor layer 104 is composed of, for example, AlGaN with a layer thickness of 20 nm and an Al composition ratio of 25%. In addition, "Al composition ratio of 25%" means that Al 0.25 Ga 0.75 N. A high-concentration two-dimensional electron gas is generated on the first nitride semiconductor layer 103 side of the heterointerface between the second nitride semiconductor layer 104 and the first nitride semiconductor layer 103 , and a channel of the two-dimensional electron gas layer 105 is formed.
[0061] In addition, the second nitride semiconductor layer 104 is not limited to AlGaN, and may be composed of a Group III nitride semiconductor such as AlInGaN. Furthermore, the second nitride semiconductor layer 104 may contain n-type impurities.
[0062] In addition, a cap layer composed of, for example, GaN and having a thickness of about 1 nm to about 2 nm may be provided as a cap layer on the second nitride semiconductor layer 104. That is, such a cap layer may be provided between the second nitride semiconductor layer 104 and the first insulating layer 201. In addition, a spacer layer composed of, for example, AlN and having a thickness of about 1 nm may be provided as a spacer layer between the first nitride semiconductor layer 103 and the second nitride semiconductor layer 104.
[0063] The ohmic electrodes 301a and 302a are disposed opposite to each other on the second nitride semiconductor layer 104. In the present embodiment, the ohmic electrodes 301a and 302a are, for example, multilayer electrode films having a stacked structure in which a Ti film and an Al film are stacked in sequence, but are not limited thereto. In addition, the ohmic electrodes 301a and 302a are electrically ohmically connected to the two-dimensional electron gas layer 105.
[0064] Alternatively, at least one of a groove in which a portion of the second nitride semiconductor layer 104 and the first nitride semiconductor layer 103 is removed and a contact layer containing n-type impurities including a donor such as Si may be provided under the ohmic electrodes 301a and 302a. The contact layer containing n-type impurities may be formed by plasma treatment, ion implantation, regrowth, or the like.
[0065] The first insulating layer 201 is provided on the second nitride semiconductor layer 104. In the present embodiment, the first insulating layer 201 is provided so as to cover the second nitride semiconductor layer 104, a part of the ohmic electrode 301a, and a part of the ohmic electrode 302a. In the present embodiment, the first insulating layer 201 is composed of SiN with a layer thickness of 100 nm, for example.
[0066] The first opening 201a is an example of an opening provided in the first insulating layer 201 between the source electrode 301 and the drain electrode 302 so as to expose the second nitride semiconductor layer 104. In the present embodiment, the first opening 201a is formed by removing the first insulating layer 201 between the ohmic electrodes 301a and 302a, and is provided so as to expose the second nitride semiconductor layer 104.
[0067] The first barrier layer 401a is provided on the second nitride semiconductor layer 104 and a portion of the first insulating layer 201 exposed by the first opening 201a so as to cover the first opening 201a and a portion of the first insulating layer 201. Figure 2As shown, the thickness t1 of the first barrier layer 401a is Z1. In this embodiment, the first barrier layer 401a is composed of, for example, TaN with a N / Ta ratio of 1.00 and a NaCl-type structure oriented only to the (111) plane, with a thickness t1 (Z1) of 30 nm. In addition, the first barrier layer 401a and the second nitride semiconductor layer 104 form a Schottky junction. Z1, which represents the thickness t1, satisfies 50 nm> Z1> 3 nm.
[0068] In addition, regarding Z1, when TaN (the first barrier layer 401a) is formed by sputtering, since the NaCl structure in which TaN is oriented only to the (111) plane is formed, Z1>10nm is preferred. In addition, when TaN (the first barrier layer 401a) is formed by atomic layer deposition, there is no limitation on the layer thickness, but there is a problem of reduced productivity.
[0069] Alternatively, the first barrier layer 401a may be made of TaN having a NaCl structure oriented only in the (111) plane and having an N / Ta ratio of 0.70 to 1.00. In this way, as described in Patent Document 1, the Schottky barrier height can be increased.
[0070] In addition, the distance between close metal atoms (i.e., lattice constant) of TaN with a NaCl-type structure having an N / Ta ratio of 0.70 to 1.00 is greater than 0.310 nm and less than 0.315 nm. The lattice constant of AlGaN is greater than 0.311 nm and less than 0.319 nm. Thus, the difference in the distance between atoms of the first barrier layer 401a composed of TaN and the second nitride semiconductor layer 104 composed of AlGaN can be reduced. Therefore, it is difficult to form dislocations in the first barrier layer 401a, so it is possible to reduce the diffusion of metal atoms of the first wiring layer 401c through dislocations in the first barrier layer 401a.
[0071] The second insulating layer 202 is provided so as to cover the first insulating layer 201 and the first barrier layer 401a. More specifically, the second insulating layer 202 is provided so as to cover the first insulating layer 201 and a portion of the first barrier layer 401a. In this embodiment, the second insulating layer 202 is preferably made of a material having an oxygen content of 1% or less, for example, SiN having a layer thickness of 150 nm. In addition, the second insulating layer 202 is not limited to SiN, and may also be SiC or SiCN.
[0072] The second opening 202b is formed by removing the second insulating layer 202, and is provided to cover the range of the first opening 201a when viewed in plan and to expose the first barrier layer 401a. In this case, the first opening 201a is arranged to be included in the second opening 202b of a larger size when viewed in plan.
[0073] In addition, the second opening 202b is provided so as to cover the range of the first opening 201a when viewed in plan, but the present invention is not limited thereto, and the end of the second opening 202b on the drain electrode 302 side may be located inside the first opening 201a. Figure 1 The second opening 202b is smaller than the semiconductor device 100A shown in FIG. 1. By making the second opening 202b, which can be a diffusion path for metal atoms of the first wiring layer 401c, smaller in size, diffusion of metal atoms of the first wiring layer 401c into the first insulating layer 201 and the second nitride semiconductor layer 104 on the drain electrode 302 side can be further reduced.
[0074] The second barrier layer 401b and the first wiring layer 401c are stacked in the order of the second barrier layer 401b and the first wiring layer 401c. The second barrier layer 401b is provided on the first barrier layer 401a and a part of the second insulating layer 202 exposed by the second opening 202b in a manner of covering the second opening 202b in contact with the first barrier layer 401a. Furthermore, the first wiring layer 401c is provided in contact with the second barrier layer 401b. In addition, the first wiring layer 401c is an example of a wiring layer provided in contact with the second barrier layer 401b. Thus, the gate electrode 401 including the first barrier layer 401a, the second barrier layer 401b and the first wiring layer 401c is formed.
[0075] In this embodiment, the second barrier layer 401b has a layer thickness t2 (see Figure 2 ) is a layer composed of TiN or WN with a thickness of 50 nm. In addition, the layer thickness t2 of the second barrier layer 401b is hereinafter referred to as Z2. The first wiring layer 401c is composed of Al with a layer thickness of 450 nm, for example.
[0076] In addition, the second barrier layer 401b is not limited to a single layer of TiN or WN, but may be a multi-layer structure composed of TiN and WN. In addition, the first wiring layer 401c is not limited to Al, but may be W, Au or Cu, a compound containing these elements, or a multi-layer electrode film formed by a multi-layer structure composed of these elements.
[0077] In addition, when the second barrier layer 401b is composed of TiN, it can be TiN with a NaCl type structure and a N / Ti ratio of 1.00 to 1.20. Alternatively, when the second barrier layer 401b is composed of WN, it can be WN with a NaCl type structure and a N / W ratio of 0.10. In this way, since the second barrier layer 401b is provided on the first barrier layer 401a composed of TaN with a N / Ta ratio of 1.00 oriented only to the (111) plane, the second barrier layer 401b can have a crystal structure oriented only to the (111) plane. In addition, the distance between the adjacent metal atoms (lattice constant) of the second barrier layer 401b composed of TiN or WN oriented only to the (111) plane is about 0.302nm or 0.298nm, respectively. In addition, the distance between adjacent metal atoms (lattice constant) of the first barrier layer 401a composed of TaN with an N / Ta ratio of 1.00 is 0.315 nm. Thus, the difference between the distance between adjacent metal atoms of the second barrier layer 401b and the first barrier layer 401a is small, so dislocations are less likely to form in the second barrier layer 401b. Therefore, metal diffusion of metal atoms of the first wiring layer 401c via dislocations of the second barrier layer 401b is reduced.
[0078] Furthermore, by making the crystal structure of the second barrier layer 401b into a NaCl type structure oriented only to the (111) plane, it is easy to make the crystal structure of the first wiring layer 401c provided on the second barrier layer 401b into a crystal structure oriented only to the (111) plane. In the case where the first wiring layer 401c is composed of Al with a layer thickness of 450nm, the crystal structure of the first wiring layer 401c is an FCC type structure oriented only to the (111) plane, and the distance between adjacent metal atoms is 0.286nm. In this way, the resistance of the first wiring layer 401c can be reduced, and the reliability can be improved.
[0079] Furthermore, since the distance between adjacent metal atoms gradually decreases from the lower layer to the upper layer, as in the first barrier layer 401a composed of TaN, the second barrier layer 401b composed of TiN or WN, and the first wiring layer 401c composed of Al, dislocations are less likely to form in the first wiring layer 401c. Therefore, the resistance of the first wiring layer 401c can be further reduced and the reliability can be improved.
[0080] As described above, the gate electrode 401 of this embodiment is an electrode including the first barrier layer 401a, the second barrier layer 401b, and the first wiring layer 401c. Figure 1As shown, the gate electrode 401 is provided at a distance from the source electrode 301 and the drain electrode 302 and is in contact with the second nitride semiconductor layer 104 in the first opening 201a. In other words, the gate electrode 401 is an electrode that penetrates the first insulating layer 201 and the second insulating layer 202 and is in contact with the second nitride semiconductor layer 104.
[0081] Here, the positional relationship among the first barrier layer 401 a , the second barrier layer 401 b , and the second insulating layer 202 will be described.
[0082] The first barrier layer 401a and the second barrier layer 401b are branched in the middle of the path from the first opening 201a toward the drain electrode 302. More specifically, the first barrier layer 401a and the second barrier layer 401b are branched in the middle of the path from the first opening 201a toward the drain electrode 302. Figure 2 The first barrier layer 401a branches at the branch point p2 of the circle indicated by the dotted line in FIG. The direction from the first opening 201a toward the drain electrode 302 is the positive direction of the x-axis. That is, the first barrier layer 401a and the second barrier layer 401b are connected at a portion closer to the negative side of the x-axis than the branch point p2, and branch and separate at a portion closer to the positive side of the x-axis than the branch point p2. In addition, the second insulating layer 202 can be said to be provided extending from above the first barrier layer 401a between the branch point p2 and the drain electrode 302 to above the first insulating layer 201. That is, at a portion closer to the positive side of the x-axis than the branch point p2, a portion of the second insulating layer 202 is sandwiched between the first barrier layer 401a and the second barrier layer 401b.
[0083] The field plate electrode 501 is an electrode provided on the second insulating layer 202 between the first opening 201a as an example of an opening and the drain electrode 302. The third barrier layer 501b and the third wiring layer 501c constituting the field plate electrode 501 are stacked in the order of the third barrier layer 501b and the third wiring layer 501c. The third barrier layer 501b is provided on a portion of the second insulating layer 202 between the second opening 202b and the drain electrode 302. Thus, the field plate electrode 501 composed of the third barrier layer 501b and the third wiring layer 501c is formed. In addition, the field plate electrode 501 is connected to the potential of the source electrode 301. In this case, the field plate electrode 501 exhibits the same potential as the source electrode 301.
[0084] The third barrier layer 501b preferably has the same structure as the second barrier layer 401b, but is not limited thereto. In addition, the third wiring layer 501c preferably has the same structure as the first wiring layer 401c, but is not limited thereto.
[0085] Although not shown in the figure, in the vertical direction (z-axis direction) of the upper surface (the main surface on the positive side of the z-axis) included in the substrate 101, the uppermost surface position of the field plate electrode 501 may be lower than the lower end position p1 of the side surface of the second barrier layer 401b closest to the drain electrode 302. Figure 2 The position of the uppermost surface 501t of the field plate electrode 501 is shown. In addition, the side surface of the second barrier layer 401b is the surface of the second barrier layer 401b parallel to the yz plane, and the side surface closest to the drain electrode 302 is the side surface with the shortest distance to the drain electrode 302. Figure 2 , the lower end position p1 of the side surface of the second barrier layer 401b is indicated by a dotted circle. In this case, although not shown in the figure, the position of the uppermost surface 501t may be lower (negative side of the z-axis) than the lower end position p1 of the side surface of the second barrier layer 401b. In this way, the area where the field plate electrode 501 and the gate electrode 401 face each other can be reduced, so the electrostatic capacitance between the field plate electrode 501 and the gate electrode 401 can be reduced. In addition, in this embodiment, as Figure 2 As shown, the uppermost surface position of the field plate electrode 501 is located above the lower end position p1 (on the positive side of the z axis).
[0086] In this embodiment, the lowest surface position of the field plate electrode 501 is located below the lower end position p1 of the side surface of the second barrier layer 401b closest to the drain electrode 302 in the vertical direction of the upper surface of the substrate 101. Figure 2 The position of the lowermost surface 501u of the field plate electrode 501 shown in FIG. Figure 2 As shown, the lowermost surface 501u is located below the lower end position p1 of the side surface of the second barrier layer 401b (negative side of the z axis). This can further reduce the electric field at the lower end of the first barrier layer 401a closest to the drain electrode 302.
[0087] In addition, in this embodiment, the material of a part of the field plate electrode 501 is the same as the material of the second barrier layer 401b. More specifically, the material of the second barrier layer 401b is the same as the material of the third barrier layer 501b, and the material of the first wiring layer 401c is the same as the material of the third wiring layer 501c. In this way, the gate electrode 401 and the field plate electrode 501 can be formed at the same time.
[0088] In addition, the field plate electrode 501 is composed of a plurality of layers including a lower layer and an upper layer. More specifically, the field plate electrode 501 is composed of a third barrier layer 501b as a lower layer and a third wiring layer 501c as an upper layer. As described above, the third barrier layer 501b and the third wiring layer 501c constituting the field plate electrode 501 are respectively made of the same material as the second barrier layer 401b and the first wiring layer 401c constituting the gate electrode 401. Furthermore, in the present embodiment, the resistivity of the upper layer is smaller than that of the lower layer. That is, the resistivity of the third wiring layer 501c of the upper layer composed of Al is smaller than that of the third barrier layer 501b of the lower layer composed of TiN. Therefore, the impedance of the field plate electrode 501 can be reduced.
[0089] The third opening 202 c and the fourth opening 202 d are formed by removing the first insulating layer 201 and the second insulating layer 202 , and are provided so as to expose a portion of the ohmic electrode 301 a and the ohmic electrode 302 a .
[0090] The second wiring layer 301b is provided on the ohmic electrode 301a and a part of the second insulating layer 202 exposed by the third opening 202c in a manner covering the third opening 202c. Similarly, the second wiring layer 302b is provided on the ohmic electrode 302a and a part of the second insulating layer 202 exposed by the fourth opening 202d in a manner covering the fourth opening 202d. In the present embodiment, the second wiring layer 301b and the second wiring layer 302b are respectively formed by stacking TiN with a layer thickness of 200nm, Al with a layer thickness of 3000nm, and TiN with a layer thickness of 50nm in sequence. In addition, the second wiring layer 301b and the second wiring layer 302b are not limited to Al, and Au or Cu may be used instead of Al, or a compound containing these elements, or a multilayer electrode film formed by a plurality of stacked structures composed of these elements.
[0091] The source electrode 301 composed of the ohmic electrode 301a and the second wiring layer 301b and the drain electrode 302 composed of the ohmic electrode 302a and the second wiring layer 302b are configured as described above. In addition, the source electrode 301 and the drain electrode 302 are arranged at a distance. The source electrode 301 and the drain electrode 302 penetrate the first insulating layer 201 and the second insulating layer 202, respectively, and are electrically connected to the first nitride semiconductor layer 103. That is, in the present embodiment, the source electrode 301 and the drain electrode 302 are in contact with the second nitride semiconductor layer 104 at the third opening 202c and the fourth opening 202d, respectively, and are electrically connected to the first nitride semiconductor layer 103.
[0092] Here, Z1 representing the layer thickness t1 of the first barrier layer 401a and Z2 representing the layer thickness t2 of the second barrier layer 401b are described. The Z1 and Z2 satisfy 200 nm ≥ Z1 + Z2 ≥ 50 nm, Z1 < Z2, and 50 nm > Z1 > 3 nm.
[0093] With the semiconductor device 100A having such a structure, the following effects can be expected as compared with the prior art of Patent Document 2. First, by setting Z1 + Z2 ≥ 50 nm, the diffusion of metal atoms in the first wiring layer 401c into the first insulating layer 201 and the second nitride semiconductor layer 104 is suppressed by the first barrier layer 401a and the second barrier layer 401b, and the generation of energy levels in the first insulating layer 201 and the second nitride semiconductor layer 104 can be reduced. Therefore, the reverse leakage current of the gate electrode 401 can be reduced and current collapse can be decreased. Further, by setting Z1 + Z2 ≥ 70 nm, the reverse leakage current of the gate electrode 401 can be reduced and current collapse can be further decreased. Thus, a semiconductor device 100A having a gate electrode 401 with high reliability and low on-resistance is obtained.
[0094] The reason why setting Z1 + Z2 ≥ 50 nm can reduce the reverse leakage current of the gate electrode 401 and decrease current collapse is described. Figure 3 It is a cross-sectional view near the gate electrode 401x of the semiconductor device having the research example of Embodiment 1. The semiconductor device of this research example mainly has the same structure as the semiconductor device 100A of the present embodiment except that it does not have the second insulating layer 202 and the gate electrode 401x is composed of a stacked structure of a TiN layer 401bx and an Al layer 401cx. Figure 4 It is a graph showing the results of the layer thickness dependence of the reverse leakage current of the gate electrode 401x and the on-resistance at high voltage / on-resistance at low voltage of the semiconductor device having the research example of Embodiment 1 with respect to the TiN layer 401bx. More specifically, in Figure 4 the first axis (left axis) of the graph shows the results of the layer thickness dependence of the reverse leakage current of the gate electrode 401x with respect to the TiN layer 401bx. Next, in Figure 4 the second axis (right axis) of the graph shows the results of the layer thickness dependence of the ratio of the on-resistance at high voltage (85 V) to the on-resistance at low voltage (30 V) when a voltage is applied between the source electrode 301 and the drain electrode 302 and a switching operation is performed as an index of current collapse with respect to the TiN layer 401bx.
[0095] Figure 54 is another diagram showing the results of the dependence of the reverse leakage current of the gate electrode 401x and the on-resistance at high voltage / on-resistance at low voltage on the thickness of the TiN layer 401bx of the semiconductor device of the research example of the first embodiment. More specifically, Figure 5 The horizontal axis of the graph represents the reverse leakage current of the gate electrode 401x. Figure 5 The vertical axis of the graph represents the ratio of the on-resistance at the high voltage (85 V) to the on-resistance at the low voltage (30 V). In addition, the thickness of the TiN layer 401bx is described outside the frame.
[0096] like Figure 4 As shown, according to the results of the thickness dependence of the TiN layer 401bx on the reverse leakage current of the gate electrode 401x, it can be seen that if the thickness of the TiN layer 401bx is 30nm or more, the reverse leakage current of the gate electrode 401x can be reduced. The change in the reverse leakage current of the gate electrode 401x when the thickness of the TiN layer 401bx is 30nm or more and 100nm or less is sufficiently smaller than the change range when the thickness of the TiN layer 401bx changes from 20nm to 30nm, so it can be considered as a manufacturing deviation. Next, according to the results of the thickness dependence of the TiN layer 401bx on the ratio of the on-resistance at high voltage and low voltage during the switching operation, it can be seen that if the thickness of the TiN layer 401bx is 50nm or more and 100nm or less, the ratio of the on-resistance becomes smaller, reducing the current collapse. Furthermore, when the thickness of the TiN layer 401bx is not less than 70 nm and not more than 100 nm, the ratio of the on-resistance is further reduced, and the current collapse is reduced.
[0097] Generally, if the reverse leakage current of the gate electrode 401x is large, the electrons captured by the energy level are released, so the reduction of the reverse leakage current of the gate electrode 401x and the increase of the current collapse are in a trade-off relationship. However, according to the results of this study, if the thickness of the TiN layer 401bx is made greater than 50nm, the reverse leakage current of the gate electrode 401x remains unchanged and the current collapse is reduced, eliminating the trade-off relationship. When the thickness of the TiN layer 401bx is greater than 70nm, the current collapse is significantly reduced. Figure 5 In FIG. 1 , a straight line with a dashed dot descending to the right is shown. The closer to the straight line with a dashed dot, the more the decrease in reverse leakage current and the increase in current collapse show a trade-off relationship. Figure 5 As shown, as the thickness of the TiN layer 401bx increases to 50 nm, 70 nm, and 100 nm, it moves away from the vicinity of the straight line of the single-dot chain line descending to the right, and the relationship of increase and decrease disappears.
[0098] When the thickness of the TiN layer 401bx is 20 nm, the diffusion of Al metal atoms causes the Schottky barrier to drop, increasing the reverse leakage current of the gate electrode 401x. Therefore, it is believed that the current collapse is reduced compared to when the thickness of the TiN layer 401bx is 50 nm.
[0099] Here, the semiconductor device 100A of the present embodiment is compared with the semiconductor device of the research example. The gate electrode 401 of the present embodiment is composed of the first barrier layer 401a (TaN), the second barrier layer 401b (TiN) and the first wiring layer 401c (Al). In addition, the gate electrode 401x of the research example is composed of the TiN layer 401bx and the Al layer 401cx. That is, if a part of the TiN layer 401bx of the research example is replaced with the first barrier layer 401a, the gate electrode 401x of the research example and the gate electrode 401 of the present embodiment have the same structure.
[0100] Here, TaN has a work function of 5.4 eV, a lattice constant of 0.310 nm to 0.315 nm, and a melting point of 3090° C. TiN has a work function of 4.7 eV, a lattice constant of 0.302 nm, and a melting point of 2930° C.
[0101] Therefore, in the structure in which a part of the TiN layer 401bx of the study example is replaced by the first barrier layer 401a (TaN), that is, the gate electrode 401, the work function is increased compared to the gate electrode 401x of the study example, and the lattice constant and the melting point are of the same level. Therefore, if the thickness of the TiN layer 401bx is equal to Z1+Z2 (the total thickness of the first barrier layer 401a and the second barrier layer 401b), for the gate electrode 401, the reverse leakage current can be suppressed and the current collapse can be reduced compared to the gate electrode 401x.
[0102] That is, in this embodiment, by setting Z1+Z2≥50nm, it is expected that the reverse leakage current can be suppressed and the current collapse can be reduced. More specifically, it can be considered that by setting Z1+Z2≥50nm, the diffusion of metal atoms of the first wiring layer 401c into the first insulating layer 201 and the second nitride semiconductor layer 104 can be suppressed by the first barrier layer 401a and the second barrier layer 401b, and the energy level in the first insulating layer 201 and the second nitride semiconductor layer 104 can be reduced. Therefore, the reverse leakage current of the gate electrode 401 can be reduced and the current collapse can be reduced. Furthermore, by setting Z1+Z2≥70nm, the reverse leakage current of the gate can be reduced and the current collapse can be further reduced. Therefore, a semiconductor device 100A having a gate electrode 401 with high reliability and low on-resistance is obtained.
[0103] In addition, WN has a work function of 4.6 eV and a lattice constant of 0.298 nm, which are equivalent to TiN. In addition, WN has a melting point of less than 2000° C., which is a sufficiently high melting point. Therefore, the same effect can be expected even when the second barrier layer 401 b of the gate electrode 401 is composed of WN instead of TiN.
[0104] In addition, from the viewpoint of processing and crystallinity of the first barrier layer 401a and the second barrier layer 401b, Z1+Z2≤200nm is preferred, Z1+Z2≤150nm is more preferred, and Z1+Z2≤100nm is further preferred.
[0105] In addition, in addition to the second barrier layer 401b composed of TiN or WN, the first barrier layer 401a is composed of TaN, which is a material with a higher melting point. By making the layer thickness t1 satisfy Z1>3nm, it is possible to suppress the diffusion of metal into the first insulating layer 201 and the second nitride semiconductor layer 104, compared with the case where the gate electrode 401 is composed only of the second barrier layer 401b. In the case where TaN is formed by sputtering, since it grows into an island shape of a discontinuous film in the initial process of film formation, it is easy to form a uniform film shape by setting Z1>3nm, so Z1>3nm is preferred. In addition, Z1>10nm is preferred, and Z1>15nm is more preferred. In addition, in the case where TaN is formed by atomic layer deposition, although there is no such restriction, there is a problem of low productivity. Furthermore, Z1, which represents the layer thickness t1 of the first barrier layer 401a, is 50nm>Z1. Z1 is more preferably 40nm>Z1, and Z1 is further preferably 30nm>Z1. TaN constituting the first barrier layer 401a exhibits high barrier properties, but has low dry etching processability. Therefore, by reducing the thickness t1 of the first barrier layer 401a to, for example, 50 nm>t1, the processability of the first barrier layer 401a can be improved.
[0106] In addition, TaN needs to be processed by dry etching. During the processing under dry etching, since TaN has a relatively high vapor pressure of halogen compounds, the selectivity between TaN and the first insulating layer 201 becomes low, and the residual film deviation of the first insulating layer 201 increases. Also, due to the increase in the residual film deviation of the first insulating layer 201, the capacitance deviation between the field plate electrode 501 and the drain electrode 302 increases. In contrast, since TiN or WN has a lower vapor pressure of halogen compounds than TaN, the selectivity between TiN or WN and the first insulating layer 201 becomes high. Therefore, by setting Z1 < Z2 as in the present embodiment, compared with the prior art of Patent Document 2, the diffusion of metal atoms in the first wiring layer 401c into the first insulating layer 201 and the second nitride semiconductor layer 104 is suppressed, and processing becomes easier. As a result, the residual film deviation of the first insulating layer 201 is reduced. Thus, the capacitance deviation between the field plate electrode 501 and the drain electrode 302 can be reduced.
[0107] In addition, as in the present embodiment, the first barrier layer 401a made of TaN is covered with the first insulating layer 201 and the second insulating layer 202 made of SiN, and the second barrier layer 401b. Further, the second insulating layer 202 is made of a material having an oxygen content of 1% or less. Therefore, the oxidation of the first barrier layer 401a made of TaN is suppressed. In addition, Figure 2 shows the closest distance d1 between the gate electrode 401 and the field plate electrode 501. The closest distance d1 refers to the shortest distance in the interval between the gate electrode 401 and the field plate electrode 501. For example, in the present embodiment, the closest distance d1 is Figure 2 the length in the x-axis direction in the cross-sectional view shown, and is the interval between the gate electrode 401 and the field plate electrode 501. The closest distance d1 is 100 nm or more. In addition, the closest distance d1 is preferably 200 nm or more, more preferably 300 nm or more. In this way, the ESD (Electrostatic Discharge) withstand voltage between the gate electrode 401 and the field plate electrode 501 can be sufficiently improved. In addition, the closest distance d1 may be 1000 nm or less, more preferably 900 nm or less, and further preferably 800 nm or less. Thereby, the miniaturization of the semiconductor device 100A becomes easy.
[0108] Hereinafter, with reference to Figure 6 to Figure 13 the manufacturing method of the semiconductor device 100A of the present embodiment will be described.
[0109] Figure 6 to Figure 13 are cross-sectional views showing the steps of the manufacturing method of the semiconductor device 100A of Embodiment 1, respectively.
[0110] First, as in Figure 6As shown, on a substrate 101 composed of Si, an organic metal vapor deposition method (MOCVD: Metal Organic Chemical Vapor Deposition) is used to grow a silicon layer in the +c plane direction ( <0001> The first nitride semiconductor layer 103 is formed by epitaxial growth in the direction of the first nitride semiconductor layer 104. The second nitride semiconductor layer 104 is formed by epitaxial growth in the direction of the first nitride semiconductor layer 104. The second nitride semiconductor layer 104 is formed by epitaxial growth in the direction of the first nitride semiconductor layer 103. The second nitride semiconductor layer 104 is formed by epitaxial growth in the direction of the first nitride semiconductor layer 103. The second nitride semiconductor layer 103 ...
[0111] Next, a pre-cleaning is performed on the second nitride semiconductor layer 104 using hydrochloric acid. Furthermore, after applying a resist, a mask is formed by patterning the resist using a photolithography method at locations other than the regions where the source electrode 301 and the drain electrode 302 are to be formed. Next, a Ti film and an Al film are deposited in sequence by vapor deposition. Figure 7 As shown, the ohmic electrode 301a and the ohmic electrode 302a are formed by a lift-off method. Then, by performing a heat treatment, the two-dimensional electron gas layer 105 and the ohmic electrode 301a and the ohmic electrode 302a are electrically ohmically connected. Alternatively, the ohmic electrode 301a and the ohmic electrode 302a may be formed by sequentially depositing a Ti film and an Al film by a sputtering method, and then sequentially applying a photolithography method and a dry etching method.
[0112] Then, if Figure 8 As shown, the first insulating layer 201 composed of SiN with a thickness of 100 nm is deposited by a plasma CVD (Chemical Vapor Deposition) method. Then, at a position other than the area where the gate electrode 401 is to be formed, after applying a resist, a mask is formed by patterning the resist using a photolithography method. Next, a first opening 201a is formed by a dry etching method to expose the second nitride semiconductor layer 104. In addition, in this embodiment, the first insulating layer 201 can be SiCN or SiN deposited by a reduced pressure CVD method. In addition, in this embodiment, a dry etching method is used, but a wet etching method can also be used to set the first opening 201a in the first insulating layer 201.
[0113] Then, if Fig. 9As shown, a sputtering device is used to sputter a Ta target with N2 gas, thereby depositing a first barrier layer 401a composed of TaN with a thickness of 30nm. Then, in the area where the gate electrode 401 is to be formed, after applying a resist, the resist is patterned using a photolithography method to form a mask. Next, the first barrier layer 401a is patterned using a dry etching method. At this time, a portion of the first insulating layer 201 is removed by over etching, but since the thickness of TaN (first barrier layer 401a) is as thin as 30nm, the amount of the first insulating layer 201 removed can be minimized, thereby reducing the residual film deviation of the first insulating layer 201.
[0114] Then, if Fig.10 As shown in FIG. 1 , a second insulating layer 202 made of SiN is deposited by plasma CVD to a thickness of 150 nm. Then, a resist is applied and patterned by photolithography to form a mask at a position other than the region where the gate electrode 401 is to be formed. Next, a second opening 202 b is formed by dry etching to expose the first barrier layer 401 a.
[0115] Next, TiN with a thickness of 50 nm and Al with a thickness of 450 nm were deposited in sequence by sputtering. Fig.11 As shown in FIG. 1 , TiN with a thickness of 50 nm corresponds to the second barrier layer 401 b and the third barrier layer 501 b, and Al with a thickness of 450 nm corresponds to the first wiring layer 401 c and the third wiring layer 501 c. Then, in the region where the gate electrode 401 and the field plate electrode 501 are to be formed, after applying a resist, the resist is patterned using a photolithography method to form a mask. Next, the second barrier layer 401 b and the third barrier layer 501 b and the first wiring layer 401 c and the third wiring layer 501 c are patterned using a dry etching method. In this way, the gate electrode 401 and the field plate electrode 501 are formed.
[0116] Then, if Fig.12 As shown, after applying a resist, a mask is formed by patterning the resist using photolithography at locations other than the regions where the source electrode 301 and the drain electrode 302 are formed. Next, a third opening 202c and a fourth opening 202d are formed using dry etching to expose the ohmic electrode 301a and the ohmic electrode 302a.
[0117] Then, if Fig.13As shown, TiN with a thickness of 200 nm, Al with a thickness of 3000 nm, and TiN with a thickness of 50 nm are sequentially deposited by sputtering. Then, in the regions where the source electrode 301 and the drain electrode 302 are formed, after applying a resist, photolithography is used to pattern the resist to form a mask. Next, dry etching is used to pattern the second wiring layer 301b and the second wiring layer 302b. In this way, the source electrode 301 and the drain electrode 302 are formed. In addition, not limited to the dry etching method, the second wiring layer 301b and the second wiring layer 302b can also be formed by a plating method or a Damascene method. In this case, the wiring can also be made of Au or Cu.
[0118] After the above series of processes, Figure 1 the semiconductor device 100A with the structure shown is completed.
[0119] In the semiconductor device 100A formed as above, by setting 200 nm ≥ Z1 + Z2 ≥ 50 nm, the metal atoms of the first wiring layer 401c can be inhibited from diffusing into the first insulating layer 201 and the second nitride semiconductor layer 104 by the first barrier layer 401a and the second barrier layer 401b, and the generation of energy levels in the first insulating layer 201 and the second nitride semiconductor layer 104 can be reduced. Therefore, the reverse leakage current of the gate electrode 401 can be reduced and current collapse can be decreased. Furthermore, by setting Z1 + Z2 ≥ 70 nm, the reverse leakage current of the gate can be reduced and current collapse can be further decreased. Thus, a semiconductor device 100A having a gate electrode 401 with high reliability and low on-resistance can be obtained.
[0120] In addition, by setting Z1 < Z2 as in the present embodiment, compared with the prior art of Patent Document 2, the diffusion of metal atoms in the first wiring layer 401c is suppressed, the processing becomes easier, and in addition, the residual film deviation of the first insulating layer 201 is reduced. Therefore, the electrostatic capacitance deviation between the field plate electrode 501 and the drain electrode 302 can be reduced.
[0121] In addition, in addition to the second barrier layer 401b of TiN or WN, by forming the first barrier layer 401a of TaN, which is a material with a higher melting point, and making the layer thickness t1 satisfy 50 nm > Z1 > 3 nm, metal diffusion can be suppressed compared with the case where the gate electrode 401 is composed only of the second barrier layer 401b.
[0122] (Embodiment 2)
[0123] Here, Fig.14 the semiconductor device of Embodiment 2 will be described.
[0124] Fig.141 is a cross-sectional view showing the structure of a semiconductor device 100B according to Embodiment 2. In this embodiment, detailed description of components common to those in Embodiment 1 will be omitted.
[0125] In the present embodiment, a case where the semiconductor device 100B is a HEMT including a Schottky junction gate electrode will be described.
[0126] like Fig.14 As shown, the semiconductor device 100B includes a substrate 101, a buffer layer 102, a first nitride semiconductor layer 103, a second nitride semiconductor layer 104, a two-dimensional electron gas layer 105, a first insulating layer 201, an opening (here, the first opening 201a), a second insulating layer 202, a third insulating layer 203, a second opening 203b, a third opening 203c, a fourth opening 203d, a source electrode 301 composed of an ohmic electrode 301a and a second wiring layer 301b, a drain electrode 302 composed of an ohmic electrode 302a and a second wiring layer 302b, a gate electrode 402 including a first barrier layer 401a, a second barrier layer 402b and a wiring layer (here, the first wiring layer 402c), and a field plate electrode 502.
[0127] The field plate electrode 502 is disposed on the second insulating layer 202 between the gate electrode 402 and the drain electrode 302. More specifically, the field plate electrode 502 is an electrode disposed on the second insulating layer 202 between the first opening 201a as an example of an opening and the drain electrode 302. In addition, the field plate electrode 502 is connected to the potential of the source electrode 301. In this case, the field plate electrode 502 exhibits the same potential as the source electrode 301. In this embodiment, the field plate electrode 502 is, for example, composed of TiN with a layer thickness of 50 nm. In addition, the field plate electrode 502 is not limited to TiN, and may also be composed of a plurality of layers including a lower layer and an upper layer. In this case, the resistivity of the upper layer may be smaller than the resistivity of the lower layer. The field plate electrode 502 may also be Al, Au, Cu, W, Ti, Ta, TiN, TaN, WN, Pt, etc., or a compound including these elements may be combined.
[0128] The third insulating layer 203 is provided on the second insulating layer 202 so as to cover the field plate electrode 502. More specifically, the third insulating layer 203 is provided on the second insulating layer 202 between the branch point p2 and the drain electrode 302 so as to cover the field plate electrode 502. In the present embodiment, the third insulating layer 203 is made of SiN with a layer thickness of 150 nm, for example.
[0129] The second opening 203b is formed by removing the second insulating layer 202 and the third insulating layer 203, and is provided so as to cover the range of the first opening 201a and expose the first barrier layer 401a when viewed in plan. In this case, the first opening 201a is arranged to be included in the second opening 203b of a larger size when viewed in plan.
[0130] In addition, the second opening 203b is provided so as to cover the range of the first opening 201a when viewed in plan, but the present invention is not limited thereto, and the end of the second opening 203b on the drain electrode 302 side may be located inside the first opening 201a. That is, in this case, the size of the second opening 203b is larger than that of the first opening 201a when viewed in plan. Fig.14 The semiconductor device 100B shown is smaller. By making the size of the second opening 203b, which may be a diffusion path for metal atoms of the first wiring layer 402c, smaller, diffusion of metal atoms of the first wiring layer 402c into the first insulating layer 201 and the second nitride semiconductor layer 104 on the drain electrode 302 side can be further reduced.
[0131] The second barrier layer 402b and the first wiring layer 402c are stacked in the order of the second barrier layer 402b and the first wiring layer 402c. The second barrier layer 402b is provided on the first barrier layer 401a and a part of the third insulating layer 203 exposed by the second opening 203b in a manner of covering the second opening 203b in contact with the first barrier layer 401a. Furthermore, the first wiring layer 402c is provided on the second barrier layer 402b in contact with the first wiring layer 402c. In addition, the first wiring layer 402c is an example of a wiring layer provided on the second barrier layer 402b in contact with the first wiring layer 402c. Thus, the gate electrode 402 including the first barrier layer 401a, the second barrier layer 402b and the first wiring layer 402c is formed.
[0132] In this embodiment, the second barrier layer 402b is made of, for example, TiN or WN with a thickness of 50 nm. The first wiring layer 402c is made of, for example, Al with a thickness of 450 nm.
[0133] In addition, the second barrier layer 402b is not limited to a single layer of TiN or WN, but may be a multi-layer structure composed of TiN and WN. In addition, the first wiring layer 402c is not limited to Al, but may be W, Au or Cu, a compound containing these elements, or a multi-layer electrode film formed by a multi-layer structure composed of these elements.
[0134] In addition, when the second barrier layer 402b is composed of TiN, it can be TiN with a NaCl type structure and a N / Ti ratio of 1.00 to 1.20. Alternatively, when the second barrier layer 402b is composed of WN, it can be WN with a NaCl type structure and a N / W ratio of 0.10. In this way, since the second barrier layer 402b is provided on the first barrier layer 401a composed of TaN with a NaCl type structure and a N / Ta ratio of 1.00 oriented only to the (111) plane, the second barrier layer 402b can have a crystal structure oriented only to the (111) plane. In addition, the distance between the adjacent metal atoms (lattice constant) of the second barrier layer 402b composed of TiN or WN oriented only to the (111) plane is about 0.302nm or 0.298nm, respectively. In addition, the distance between adjacent metal atoms (lattice constant) of the first barrier layer 401a composed of TaN with an N / Ta ratio of 1.00 is 0.315 nm. As a result, the difference between the distance between adjacent metal atoms of the second barrier layer 402b and the first barrier layer 401a is small, so dislocations are less likely to form in the second barrier layer 402b. Therefore, metal diffusion of metal atoms of the first wiring layer 402c via dislocations of the second barrier layer 402b is reduced.
[0135] Furthermore, by making the crystal structure of the second barrier layer 402b into a NaCl type structure oriented only to the (111) plane, the crystal structure of the first wiring layer 402c provided on the second barrier layer 402b is easily made into a crystal structure oriented only to the (111) plane. When the layer thickness of the first wiring layer 402c is 450nm and the first wiring layer 402c is composed of Al, the crystal structure of the first wiring layer 402c is made into an FCC type structure oriented only to the (111) plane, and the distance between the adjacent metal atoms is 0.286nm. In this way, the resistance of the first wiring layer 402c can be reduced and the reliability can be improved.
[0136] Furthermore, since the distance between adjacent metal atoms gradually decreases from the lower layer to the upper layer, as in the first barrier layer 401a composed of TaN, the second barrier layer 402b composed of TiN or WN, and the first wiring layer 402c composed of Al, dislocations are less likely to form in the first wiring layer 402c. Therefore, the resistance of the first wiring layer 402c can be further reduced, and the reliability can be improved.
[0137] Here, the positional relationship among the first barrier layer 401 a , the second barrier layer 402 b , the second insulating layer 202 , and the third insulating layer 203 will be described.
[0138] The first barrier layer 401a and the second barrier layer 402b branch from a branch point p2 located halfway from the first opening 201a toward the drain electrode 302. At this time, the second insulating layer 202 and the third insulating layer 203 are sandwiched by the first barrier layer 401a and the second barrier layer 402b on the positive side of the x-axis relative to the branch point p2. More specifically, a portion of the stacked body composed of the second insulating layer 202 and the third insulating layer 203 is sandwiched by the first barrier layer 401a and the second barrier layer 402b.
[0139] In addition, in the vertical direction of the upper surface of the substrate 101, the uppermost surface position of the field plate electrode 502 is set below the lower end position p1 of the side surface of the second barrier layer 402b closest to the drain electrode 302. Fig.14 The position of the uppermost surface 502t of the field plate electrode 502 is shown. In addition, the side surface of the second barrier layer 402b is the surface of the second barrier layer 402b parallel to the yz plane, and the side surface closest to the drain electrode 302 is the side surface with the shortest distance to the drain electrode 302. Fig.14 In FIG. 4 , the lower end position p1 of the side surface of the second barrier layer 402b is indicated by a dotted circle. Fig.14 As shown, the uppermost surface 502t is located below the lower end position p1 of the side surface of the second barrier layer 402b (negative side of the z axis). This can reduce the area where the field plate electrode 502 faces the gate electrode 402, thereby reducing the capacitance between the field plate electrode 502 and the gate electrode 402.
[0140] In addition, the first barrier layer 401a composed of TaN is covered by the first insulating layer 201 and the second insulating layer 202 composed of SiN, and the second barrier layer 402b. Furthermore, the second insulating layer 202 is composed of a material with an oxygen content of 1% or less. Therefore, oxidation of the first barrier layer 401a composed of TaN is suppressed. Fig.14 The closest distance d1 between the gate electrode 402 and the field plate electrode 502 is shown in FIG. The closest distance d1 refers to the shortest distance between the gate electrode 402 and the field plate electrode 502. For example, in this embodiment, the closest distance d1 is Fig.14 The length in the x-axis direction in the cross-sectional view shown is the interval between the gate electrode 402 and the field plate electrode 502. The closest distance d1 is greater than 100 nm. In addition, the closest distance d1 is preferably greater than 200 nm, and more preferably greater than 300 nm. In this way, the ESD withstand voltage of the gate electrode 402 and the field plate electrode 502 can be sufficiently improved. In addition, the closest distance d1 is less than 1000 nm, more preferably less than 900 nm, and further preferably less than 800 nm. As a result, the compactness of the semiconductor device 100B becomes easy.
[0141] In this embodiment, the lowest surface position of the field plate electrode 502 is set below the lower end position p1 of the side surface of the second barrier layer 402b closest to the drain electrode 302 in the vertical direction of the upper surface of the substrate 101. Fig.14 The position of the lowermost surface 502u of the field plate electrode 502 is shown. That is, in this case, Fig.14 As shown, the lowermost surface 502u is located below the lower end position p1 of the side surface of the second barrier layer 402b (negative side of the z axis). This can further reduce the electric field at the lower end of the first barrier layer 401a closest to the drain electrode 302.
[0142] The third opening 203 c and the fourth opening 203 d are formed by removing the first insulating layer 201 , the second insulating layer 202 , and the third insulating layer 203 , and are provided to expose a portion of the ohmic electrode 301 a and the ohmic electrode 302 a .
[0143] The second wiring layer 301b is provided on the ohmic electrode 301a and a part of the third insulating layer 203 exposed by the third opening 203c in a manner covering the third opening 203c. Similarly, the second wiring layer 302b is provided on the ohmic electrode 302a and a part of the third insulating layer 203 exposed by the fourth opening 203d in a manner covering the fourth opening 203d. In the present embodiment, the second wiring layer 301b and the second wiring layer 302b are respectively composed of, for example, TiN with a layer thickness of 200nm, Al with a layer thickness of 3000nm, and TiN with a layer thickness of 50nm. In addition, the second wiring layer 301b and the second wiring layer 302b are not limited to Al, and may be W, Au, or Cu instead of Al, or may be a compound containing these elements, or may be a multilayer electrode film formed by a plurality of stacked structures composed of these elements.
[0144] As described above, the semiconductor device 100B of the present embodiment has the third insulating layer 203, and the second insulating layer 202 and the third insulating layer 203 are sandwiched by the first barrier layer 401a and the second barrier layer 402b. With the semiconductor device 100B having such a structure, the second insulating layer 202 and the third insulating layer 203 are independently designed, so the degree of freedom of the structural design of the semiconductor device 100B is high from the viewpoint of ESD withstand voltage and electric field design. Furthermore, since the third insulating layer 203 is inserted between the first barrier layer 401a and the second barrier layer 402b, the electrostatic capacitance between the field plate electrode 502 and the gate electrode 402 is small, and a gate electrode 402 having high reliability and low on-resistance is obtained.
[0145] In addition, the dielectric constant of the material constituting the third insulating layer 203 may be smaller than the dielectric constant of the material constituting the second insulating layer 202. The material constituting the third insulating layer 203 may be, for example, SiO2, SiON, SiC, or SiCN, and is preferably selected according to the dielectric constant of the material constituting the second insulating layer 202. In this way, the electrostatic capacitance of the field plate electrode 502 and the gate electrode 402 can be reduced.
[0146] In addition, the thickness of the second insulating layer 202 may be thinner than the thickness of the third insulating layer 203. In this way, the electric field can be relaxed at the end of the first barrier layer 401a on the drain electrode 302 side.
[0147] In addition, at least one of the first barrier layer 401a and the second barrier layer 402b may be bilaterally asymmetric. That is, at least one of the shapes of the first barrier layer 401a and the second barrier layer 402b may not be linearly symmetric about a symmetry line passing through the center of the opening (here, the first opening 201a) and parallel to the z-axis. In this way, the degree of freedom in the structural design of the field plate electrode 502 is increased.
[0148] use Figure 15 to Figure 19 Such a shape will be described.
[0149] First, use Fig.15 Provide explanation.
[0150] Fig.15 1 is a cross-sectional view showing a structure near the gate electrode 402 of the semiconductor device 100B according to the first modification of the second embodiment.
[0151] The semiconductor device 100B according to the first modification of the second embodiment has the same structure as the semiconductor device 100B according to the second embodiment, except that the field plate electrode 502 has a stepped shape and the second barrier layer 402 b has an asymmetric shape.
[0152] exist Fig.15 , a symmetry line L1 passing through the center of the first opening 201a and parallel to the z-axis is shown. With the symmetry line L1 as the axis, the shape of the second barrier layer 402b is, for example, Fig.15In the cross-sectional view shown, the second barrier layer 402b is not line symmetrical. In this case, in the second barrier layer 402b, the extension length from the center of the first opening 201a toward the source electrode 301 is different from the extension length from the center toward the drain electrode 302. In addition, the direction from the center toward the source electrode 301 is the negative direction of the x-axis, and the extension length in the negative direction of the x-axis is the length from the symmetry line L1 to the end of the second barrier layer 402b on the source electrode 301 side. In addition, the direction from the center toward the drain electrode 302 is the positive direction of the x-axis, and the extension length in the positive direction of the x-axis is the length from the symmetry line L1 to the end of the second barrier layer 402b on the drain electrode 302 side. In this way, in at least one of the first barrier layer 401a and the second barrier layer 402b (here, the second barrier layer 402b), the extension length from the center of the first opening 201a toward the source electrode 301 is different from the extension length from the center toward the drain electrode 302. This improves the degree of freedom in structural design of the field plate electrode 502 .
[0153] Furthermore, in a planar view of the substrate 101, the distance between the first barrier layer 401a and the field plate electrode 502 may be shorter than the distance d2 between the second barrier layer 402b and the field plate electrode 502. More specifically, the distance d2 between the second barrier layer 402b and the field plate electrode 502 is Fig.15 In addition, in the plan view, since the end of the first barrier layer 401a on the positive side of the x-axis overlaps the end of the field plate electrode 502 on the negative side of the x-axis, the interval between the first barrier layer 401a and the field plate electrode 502 is 0 here. In this way, the interval between the second barrier layer 402b and the drain electrode 302 is enlarged, so that the electrostatic capacitance between the drain electrode 302 and the gate electrode 402 can be reduced.
[0154] Furthermore, use Fig.16 Provide explanation.
[0155] Fig.16 1 is a cross-sectional view showing a structure near a gate electrode 402 of a semiconductor device 100B according to a second modification of the second embodiment.
[0156] The semiconductor device 100B according to the second modification of the second embodiment has the same structure as the semiconductor device 100B according to the first modification of the second embodiment, except that the shape of the second barrier layer 402 b is mainly different.
[0157] like Fig.16 As shown, the shape of the second barrier layer 402b is, for example, Fig.16In the cross-sectional view shown, the second barrier layer 402b is not linearly symmetrical about the symmetry line L1. In addition, the second barrier layer 402b has a step shape on the negative side of the x-axis from the center of the first opening 201a (e.g., the symmetry line L1) and on the positive side of the x-axis from the center of the first opening 201a (e.g., the symmetry line L1). Here, the step shape on the negative side of the x-axis from the center of the first opening 201a and the step shape on the positive side of the x-axis from the center of the first opening 201a are different in the number of steps.
[0158] In addition, Fig.15 Similarly, in the semiconductor device 100B of the variation 1 of the embodiment 2 shown in FIG. 1 , in the semiconductor device 100B of the variation 2 of the embodiment 2, the interval between the first barrier layer 401a and the field plate electrode 502 can be shorter than the interval d2 between the second barrier layer 402b and the field plate electrode 502 in a plan view of the substrate 101. In this way, the interval between the second barrier layer 402b and the drain electrode 302 is increased, so that the electrostatic capacitance between the drain electrode 302 and the gate electrode 402 can be reduced.
[0159] Furthermore, use Fig.17 and Fig.18 Provide explanation.
[0160] Fig.17 1 is a cross-sectional view showing a structure near a gate electrode 402 of a semiconductor device 100B according to a third modification of the second embodiment. Fig.18 Yes Fig.17 A cross-sectional view showing an enlarged view of region XVIII.
[0161] The semiconductor device 100B according to the third modification of the second embodiment has the same structure as the semiconductor device 100B according to the second embodiment, except that the shape of the first barrier layer 401 a is bilaterally asymmetric.
[0162] exist Fig.17 and Fig.18 The symmetry line L1 is shown in FIG. The shape of the first barrier layer 401a is, for example, Fig.17 and Fig.18 More specifically, in the first barrier layer 401a, the extension length from the center of the first opening 201a toward the source electrode 301 (hereinafter referred to as the first extension length) is different from the extension length from the center toward the drain electrode 302 (hereinafter referred to as the second extension length). As an example, Fig.18As shown, the first extension length and the second extension length are length d4 and length d5, respectively. In this case, the first extension length is the length d4 along the negative direction of the x-axis, which is the direction from the center of the first opening 201a (e.g., the symmetry line L1) toward the source electrode 301, and the second extension length is the length d5 along the positive direction of the x-axis, which is the direction from the center of the first opening 201a (e.g., the symmetry line L1) toward the drain electrode 302. In addition, as another example, as Fig.18 As shown in FIG. 1 , the first extension length and the second extension length are length d6 and length d7, respectively. In this case, the first extension length is the length of the step difference of the step shape of the first barrier layer 401a on the negative side of the x-axis relative to the symmetry line L1, i.e., length d6, and the second extension length is the length of the step difference of the step shape of the first barrier layer 401a on the positive side of the x-axis relative to the symmetry line L1, i.e., length d7. Thus, the first extension length and the second extension length preferably satisfy the relationship of length d4>length d5 or length d6>length d7. Fig.17 and Fig.18 As shown, in the first barrier layer 401a, the extension length (first extension length) from the center of the first opening 201a toward the source electrode 301 is different from the extension length (second extension length) from the center toward the drain electrode 302. Thus, the structural design freedom of the field plate electrode 502 is improved.
[0163] Furthermore, in a planar view of the substrate 101, the interval d3 between the first barrier layer 401a and the field plate electrode 502 may be longer than the interval between the second barrier layer 402b and the field plate electrode 502. More specifically, the interval d3 between the first barrier layer 401a and the field plate electrode 502 is Fig.17 4. In addition, in the plane view, since the end of the second barrier layer 402b on the positive side of the x-axis overlaps the end of the field plate electrode 502 on the negative side of the x-axis, the interval between the second barrier layer 402b and the field plate electrode 502 is 0 here. In this way, the width of the second barrier layer 402b and the first wiring layer 402c is expanded toward the drain electrode 302 side, which can reduce the wiring resistance of the gate electrode 402. Furthermore, since the shape of the field plate electrode 502 becomes flat, the electrostatic capacitance between the field plate electrode 502 and the gate electrode 402 can be reduced.
[0164] Further Use Fig.19 Provide explanation.
[0165] Fig.19 1 is a cross-sectional view showing a structure near a gate electrode 402 of a semiconductor device 100B according to a fourth modification of the second embodiment.
[0166] The semiconductor device 100B according to the fourth variation of the second embodiment has the same structure as the semiconductor device 100B according to the third variation of the second embodiment, except that the shape of the second barrier layer 402b is different. Fig.19 As shown in FIG. 2 , the interval d3 between the first barrier layer 401a and the field plate electrode 502 can be longer than the interval d2 between the second barrier layer 402b and the field plate electrode 502. In this case, the width of the second barrier layer 402b and the first wiring layer 402c is further expanded toward the drain electrode 302 side, and the wiring resistance of the gate electrode 402 can be reduced. In this way, when it is desired to reduce the wiring resistance of the gate electrode 402, the electrostatic capacitance of the field plate electrode 502 and the gate electrode 402 increases. For this reason, by making the layer thickness of the third insulating layer 203 thicker, the structure can be designed in a manner that the electrostatic capacitance of the field plate electrode 502 and the gate electrode 402 does not increase.
[0167] Below, refer to Figure 20 to Figure 28 A method for manufacturing the semiconductor device 100B according to the present embodiment will be described. Figure 20 to Figure 28 Each of them is a cross-sectional view showing the structure of the semiconductor device 100B in the process of being manufactured.
[0168] first, Figure 20 to Figure 23 Compared with the embodiment 1 Figure 6 to Figure 9 It is the same, so the detailed description is omitted.
[0169] Then, if Fig.24 As shown in FIG. 1 , after a second insulating layer 202 made of SiN with a thickness of 150 nm is deposited by plasma CVD, TiN with a thickness of 50 nm is deposited in sequence by sputtering. Then, in the region where the field plate electrode 502 is to be formed, a resist is applied and then patterned by photolithography to form a mask. Next, the field plate electrode 502 is formed by dry etching.
[0170] Then, if Fig.25 As shown in FIG. 1 , a third insulating layer 203 made of SiN is deposited by plasma CVD to a thickness of 150 nm. Then, a resist is applied and patterned by photolithography to form a mask at a position other than the region where the gate electrode 402 is to be formed. Next, a second opening 203 b is formed by dry etching to expose the first barrier layer 401 a.
[0171] Then, if Fig.26As shown in FIG. 1 , a second barrier layer 402b made of TiN with a thickness of 50 nm and a first wiring layer 402c made of Al with a thickness of 450 nm are sequentially deposited by sputtering. Then, in the region where the gate electrode 402 is to be formed, a resist is applied and then patterned using photolithography to form a mask. Next, the second barrier layer 402b and the first wiring layer 402c are patterned using a dry etching method. In this way, the gate electrode 402 is formed.
[0172] Then, if Fig. 27 As shown, after applying a resist, a mask is formed by patterning the resist using photolithography at locations other than the regions where the source electrode 301 and the drain electrode 302 are formed. Next, a third opening 203c and a fourth opening 203d are formed using dry etching to expose the ohmic electrode 301a and the ohmic electrode 302a.
[0173] Then, if Fig.28 As shown, TiN with a layer thickness of 200 nm, Al with a layer thickness of 3000 nm, and TiN with a layer thickness of 50 nm are sequentially deposited by sputtering. Then, in the area where the source electrode 301 and the drain electrode 302 are formed, after applying a resist, the resist is patterned using a photolithography method to form a mask. Next, the second wiring layer 301b and the second wiring layer 302b are patterned using a dry etching method. In this way, the source electrode 301 and the drain electrode 302 are formed. In addition, the second wiring layer 301b and the second wiring layer 302b are not limited to the dry etching method, and can also be formed as wiring using Au or Cu by a plating method or a damascene method.
[0174] After the above series of processes, Fig.14 The semiconductor device 100B having the structure shown is completed.
[0175] In the semiconductor device 100B formed as described above, the area where the field plate electrode 502 and the gate electrode 402 face each other can be reduced, so that the electrostatic capacitance between the field plate electrode 502 and the gate electrode 402 can be reduced. Therefore, the semiconductor device 100B can be obtained in which the electrostatic capacitance between the field plate electrode 502 and the gate electrode 402 is small, and the gate electrode 402 has high reliability and low on-resistance.
[0176] (Other embodiments)
[0177] As mentioned above, the semiconductor device of the present disclosure has been described based on the respective embodiments, but the present disclosure is not limited to the above-described respective embodiments.
[0178] For example, as in Embodiment 2, Figure 15 to Figure 19As shown, at least one of the first barrier layer 401a and the second barrier layer 402b may be asymmetric. In addition, in Embodiment 1, at least one of the first barrier layer 401a and the second barrier layer 401b may be asymmetric. In this way, the degree of freedom in the structural design of the field plate electrode 501 is improved.
[0179] In addition, for example, Fig.15 As shown in FIG. 1 , the interval between the first barrier layer 401a and the field plate electrode 502 may be shorter than the interval d2 between the second barrier layer 402b and the field plate electrode 502. In addition, in Embodiment 1, the interval between the first barrier layer 401a and the field plate electrode 501 may be shorter than the interval between the second barrier layer 401b and the field plate electrode 501. In this way, the interval between the second barrier layer 401b and the drain electrode 302 is increased, so that the electrostatic capacitance between the drain electrode 302 and the gate electrode 401 can be reduced.
[0180] In addition, for example, Fig.17 As shown in the figure, the interval d3 between the first barrier layer 401a and the field plate electrode 502 can be longer than the interval between the second barrier layer 402b and the field plate electrode 502. In addition, in the first embodiment, the interval between the first barrier layer 401a and the field plate electrode 501 can be longer than the interval between the second barrier layer 402b and the field plate electrode 501. In this way, the width of the gate electrode 401 is expanded toward the drain electrode 302 side, and the wiring resistance of the gate electrode 401 can be reduced. Furthermore, since the shape of the field plate electrode 501 becomes flat, the electrostatic capacitance between the field plate electrode 501 and the gate electrode 401 can be reduced.
[0181] In addition, for example, as long as it does not depart from the main purpose of the present disclosure, the present disclosure also includes forms obtained by implementing various modifications that a person skilled in the art would think of to each embodiment, or forms achieved by arbitrarily combining the constituent elements and functions of the embodiments within the scope that does not depart from the main purpose of the present disclosure.
[0182] In addition, various changes, substitutions, additions, omissions, etc. can be made to the above-mentioned embodiments within the scope of the claims or their equivalents.
[0183] Industrial Applicability
[0184] The semiconductor device of the present disclosure is useful as a power switching element or the like used in communication equipment, inverters, power supply circuits, and the like that require high-speed operation.
[0185] Description of symbols
[0186] 100A, 100B semiconductor device
[0187] 101 Substrate
[0188] 102 Buffer layer
[0189] 103 first nitride semiconductor layer
[0190] 103a GaN layer
[0191] 104 second nitride semiconductor layer
[0192] 104a AlGaN layer
[0193] 105 Two-dimensional electron gas
[0194] 201, 211 1st insulation layer
[0195] 201a, 211a first opening
[0196] 202, 212 second insulation layer
[0197] 202b, 203b, 212b second opening
[0198] 202c, 203c third opening
[0199] 202d, 203d Fourth opening
[0200] 203 3rd insulation layer
[0201] 204 Gate insulation layer
[0202] 301 source electrode
[0203] 301a, 302a Ohm electrodes
[0204] 301b, 302b: second wiring layer
[0205] 302 drain electrode
[0206] 401, 401x, 402, 411 gate electrodes
[0207] 401a1st barrier layer
[0208] 401b, 402b second barrier layer
[0209] 401c, 402c, 411c 1st wiring layer
[0210] 411a TaN layer
[0211] 401bx, 411b TiN layer
[0212] 401cx Al layer
[0213] 501, 502 field plate electrode
[0214] 501b 3rd barrier layer
[0215] 501c 3rd wiring layer
[0216] 501t, 502t top surface
[0217] The bottom surface of 501u and 502u
[0218] p1 bottom position
[0219] p2 branch point
[0220] d1 closest distance
[0221] d2, d3 interval
[0222] Length of d4, d5, d6, d7
[0223] L1 symmetry line
[0224] t1, t2 layer thickness
Claims
1. A semiconductor device, characterized in that: comprises: a substrate; a first nitride semiconductor layer provided on the substrate; a second nitride semiconductor layer having a larger bandgap than the first nitride semiconductor layer and provided on the first nitride semiconductor layer; a first insulating layer provided on the second nitride semiconductor layer; a source electrode and a drain electrode spaced apart from each other, each penetrating the first insulating layer and being electrically connected to the first nitride semiconductor layer; an opening provided in the first insulating layer between the source electrode and the drain electrode so as to expose the second nitride semiconductor layer; and a gate electrode spaced apart from the source electrode and the drain electrode and in contact with the second nitride semiconductor layer at the opening; the gate electrode includes: a first barrier layer made of TaN with a layer thickness of Z1, which forms a Schottky junction with the second nitride semiconductor layer; a second barrier layer provided in contact with the first barrier layer and made of TiN or WN with a layer thickness of Z2; and a wiring layer provided in contact with the second barrier layer; the Z1 and the Z2 satisfy 200nm ≥ Z1 + Z2 ≥ 50nm, Z1 < Z2, and 50nm > Z1 > 3nm, the first barrier layer covers the opening and a part of the first insulating layer.
2. The semiconductor device according to claim 1, wherein the Z1 and the Z2 satisfy Z1 + Z2 ≥ 70nm.
3. The semiconductor device according to claim 1 or 2, wherein: the Z1 satisfies Z1 > 10nm.
4. The semiconductor device according to claim 3, wherein: the first barrier layer and the second barrier layer branch from a branch point, and the branch point is located midway from the opening toward the drain electrode; the semiconductor device further comprises: a second insulating layer extending from above the first barrier layer between the branch point and the drain electrode to above the first insulating layer, with an oxygen content rate of 1% or less; and a field plate electrode provided on the second insulating layer between the opening and the drain electrode and having the same potential as the source electrode; the closest distance between the field plate electrode and the gate electrode is 100nm or more and 1000nm or less.
5. A semiconductor device, characterized in that: comprises: a substrate; a first nitride semiconductor layer provided on the substrate; a second nitride semiconductor layer having a larger bandgap than the first nitride semiconductor layer and provided on the first nitride semiconductor layer; a first insulating layer provided on the second nitride semiconductor layer; a source electrode and a drain electrode spaced apart from each other, each penetrating the first insulating layer and being electrically connected to the first nitride semiconductor layer; an opening provided in the first insulating layer between the source electrode and the drain electrode so as to expose the second nitride semiconductor layer; and a gate electrode spaced apart from the source electrode and the drain electrode and in contact with the second nitride semiconductor layer at the opening; the gate electrode includes: a first barrier layer made of TaN with a layer thickness of Z1, which forms a Schottky junction with the second nitride semiconductor layer; a second barrier layer provided in contact with the first barrier layer and made of TiN or WN with a layer thickness of Z2; and a wiring layer provided in contact with the second barrier layer; The above-mentioned Z1 and the above-mentioned Z2 satisfy 200 nm ≥ Z1 + Z2 ≥ 50 nm, Z1 < Z2, and 50 nm > Z1 > 3 nm. The above-mentioned first barrier layer and the above-mentioned second barrier layer branch from a branch point, and the branch point is located midway from the above-mentioned opening toward the above-mentioned drain electrode. The above-mentioned semiconductor device further includes: A second insulating layer that extends from above the above-mentioned first barrier layer between the above-mentioned branch point and the above-mentioned drain electrode to above the above-mentioned first insulating layer, and has an oxygen content rate of 1% or less; and A field plate electrode that is provided above the above-mentioned second insulating layer between the above-mentioned opening and the above-mentioned drain electrode and has the same potential as the above-mentioned source electrode; The closest distance between the above-mentioned field plate electrode and the above-mentioned gate electrode is 100 nm or more and 1000 nm or less.
6. The semiconductor device according to claim 5, wherein: In the vertical direction of the upper surface included in the above-mentioned substrate, the lowermost surface position of the above-mentioned field plate electrode is lower than the lower end position of the side surface of the above-mentioned second barrier layer closest to the above-mentioned drain electrode.
7. The semiconductor device according to claim 5, wherein: The material of a part of the above-mentioned field plate electrode is the same as the material of the above-mentioned second barrier layer.
8. The semiconductor device according to claim 5, wherein: In the vertical direction of the upper surface included in the above-mentioned substrate, the uppermost surface position of the above-mentioned field plate electrode is lower than the lower end position of the side surface of the above-mentioned second barrier layer closest to the above-mentioned drain electrode.
9. The semiconductor device according to claim 5, wherein: The above-mentioned field plate electrode is composed of a plurality of layers including a lower layer and an upper layer, and the resistivity of the above-mentioned upper layer is smaller than the resistivity of the above-mentioned lower layer.
10. The semiconductor device according to claim 5, wherein: There is also a third insulating layer that is provided above the above-mentioned second insulating layer between the above-mentioned branch point and the above-mentioned drain electrode so as to cover the above-mentioned field plate electrode; The above-mentioned second insulating layer and the above-mentioned third insulating layer are sandwiched by the above-mentioned first barrier layer and the above-mentioned second barrier layer.
11. The semiconductor device according to claim 10, wherein: The dielectric constant of the material constituting the above-mentioned third insulating layer is smaller than the dielectric constant of the material constituting the above-mentioned second insulating layer.
12. The semiconductor device according to claim 11, wherein The layer thickness of the above-mentioned second insulating layer is thinner than the layer thickness of the above-mentioned third insulating layer.
13. The semiconductor device according to claim 5, wherein: In at least one of the above-mentioned first barrier layer and the above-mentioned second barrier layer, the extension length in the direction from the center of the above-mentioned opening toward the above-mentioned source electrode is different from the extension length in the direction from the center toward the above-mentioned drain electrode.
14. The semiconductor device according to claim 11, wherein In at least one of the above-mentioned first barrier layer and the above-mentioned second barrier layer, the extension length in the direction from the center of the above-mentioned opening toward the above-mentioned source electrode is different from the extension length in the direction from the center toward the above-mentioned drain electrode.
15. The semiconductor device according to claim 13, wherein: In a plan view of the above-mentioned substrate, the interval between the above-mentioned first barrier layer and the above-mentioned field plate electrode is shorter than the interval between the above-mentioned second barrier layer and the above-mentioned field plate electrode.
16. The semiconductor device according to claim 14, wherein: In a plan view of the above-mentioned substrate, the interval between the above-mentioned first barrier layer and the above-mentioned field plate electrode is shorter than the interval between the above-mentioned second barrier layer and the above-mentioned field plate electrode.
17. The semiconductor device according to claim 13, wherein: In a plan view of the above-mentioned substrate, the interval between the above-mentioned first barrier layer and the above-mentioned field plate electrode is longer than the interval between the above-mentioned second barrier layer and the above-mentioned field plate electrode.
18. The semiconductor device according to claim 14, wherein: In a plan view of the above-mentioned substrate, the interval between the above-mentioned first barrier layer and the above-mentioned field plate electrode is longer than the interval between the above-mentioned second barrier layer and the above-mentioned field plate electrode.
Citation Information
Patent Citations
Semiconductor element and field effect transistor
JP2006190749A
Nitride semiconductor device and manufacturing method of the same
JP2013201370A
Damascene contacts on iii-v CMOS devices
US20100176421A1
Method of manufacturing a HEMT device with reduced gate leakage current, and HEMT device
US20200051823A1