Modified cyclized vinyl silicone oil and preparation method thereof

By controlling the structure and composition of modified cyclized vinyl silicone oil and combining specific reaction conditions, a modified cyclized vinyl silicone oil with high light transmittance and good flowability was prepared, solving the problem of uncontrollable product structure in the prior art and improving the storage stability and mechanical properties of the product.

CN117777453BActive Publication Date: 2024-11-19四川大学青岛研究院
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311856460.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-29
Publication Date
2024-11-19
Estimated Expiration
2043-12-29

AI Technical Summary

Technical Problem

Existing methods for synthesizing phenyl silicone oils have poor reaction controllability, resulting in uncontrollable product structure, unstable light transmittance, storage stability and color issues, making it difficult to obtain products with high phenyl content and suitable viscosity.

Method used

By controlling the ratio of methylphenylsiloxane units to methylsiloxane units in the modified cyclized vinyl silicone oil, and adjusting the molar ratio of silicon atoms to phenyl groups, combined with the use of end-capping agents and alkaline catalysts, dehydration and end-capping reactions were carried out to prepare a modified cyclized vinyl silicone oil with high refractive index, high light transmittance and good flowability.

Benefits of technology

The modified cyclized vinyl silicone oil achieved high light transmittance and fluidity, while improving the mechanical properties after curing. The preparation process is controllable, and the product has good performance uniformity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117777453B_ABST
    Figure CN117777453B_ABST
Patent Text Reader

Abstract

A modified cyclized vinyl silicone oil and a preparation method thereof, belonging to the technical field of silicone oil preparation. The modified cyclized vinyl silicone oil has a structure shown in formula (1): #imgabs0# wherein Vi represents vinyl, m>0, n>0, 0.6≤n / m+n≤0.8, and m and n are both positive integers. The modified cyclized vinyl silicone oil of the present invention has a high refractive index and high light transmittance, and at the same time has good fluidity and good mechanical properties after curing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of silicone oil preparation, and specifically relates to a modified cyclized vinyl silicone oil and a preparation method thereof. Background Art

[0002] Silicone oil usually refers to linear polysiloxane products that remain in liquid state at room temperature, which are generally divided into two categories: methyl silicone oil and modified silicone oil. Methyl silicone oil is the most commonly used silicone oil, also known as ordinary silicone oil. Its organic groups are all methyl. Methyl silicone oil has good chemical stability, insulation, and good hydrophobicity. In recent years, organic modified silicone oil has developed rapidly, and many organic modified silicone oils with special properties have emerged, such as: hydrogen silicone oil, ethyl silicone oil, phenyl silicone oil, chlorophenyl silicone oil, trifluoropropyl silicone oil, etc. Among them, phenyl silicone oil has good high temperature resistance, radiation resistance, lubrication and compatibility due to the introduction of phenyl groups in the molecular chain. In addition, phenyl silicone oil shows a certain absorption of ultraviolet light, and the working temperature is -50-250℃. Therefore, phenyl silicone oil is widely used in daily chemical products, electronics, machinery and other fields.

[0003] Existing phenyl silicone oils are mainly produced by hydrolysis and polycondensation of vinyl chlorosilane and non-vinyl chlorosilane, and the reaction controllability is poor. The composition of the product (i.e., phenyl vinyl silicone oil) obtained under different raw material ratios and hydrolysis conditions varies greatly, resulting in uncontrollable product structure and unstable product transmittance.

[0004] Patent CN1569925A discloses a method for synthesizing phenyl silicone oil using tetramethylammonium hydroxide or its silicon alkoxide as catalyst. Since tetramethylammonium hydroxide or its silicon alkoxide cannot withstand high temperatures, it can only be used at low temperatures. However, the rearrangement reaction of siloxane units containing phenyl segments at low temperatures is insufficient. Therefore, the storage stability of the synthesized phenyl silicone oil is unreliable and is easily turbid. In addition, the color of the phenyl silicone oil synthesized by this method is yellowish, which affects the light transmittance.

[0005] Patent CN103012797B discloses a method for preparing modified silicone oil by hydrolysis condensation polymerization of phenylalkoxysilane and alkyldialkoxysilane, the molecular structure of which is difficult to control, which will affect the storage stability and light transmittance of the product. At the same time, the silicone oil containing diphenyl chain segments prepared by the above preparation method is not easy to obtain a product with high phenyl content and moderate viscosity. Summary of the invention

[0006] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a modified cyclized vinyl silicone oil and a preparation method and application thereof, wherein the modified cyclized vinyl silicone oil has a high refractive index and high light transmittance, as well as good fluidity and good mechanical properties after curing.

[0007] In order to achieve the above object, according to one aspect of the present invention, a modified cyclized vinyl silicone oil is provided, having a structure shown in formula (1):

[0008]

[0009] Wherein, Vi represents vinyl, m>0, n>0, 0.6≤n / m+n≤0.8, and m and n are both positive integers.

[0010] In some embodiments, the number average molecular weight of the modified cyclized vinyl silicone oil is 3500-35000, and the molecular weight distribution index PDI is 1.4-1.6.

[0011] In some embodiments, in the modified cyclized vinyl silicone oil, the molar ratio of silicon atoms to phenyl groups is 1.4 to 1.7.

[0012] According to another aspect of the present invention, there is also provided a method for preparing the above-mentioned modified cyclized vinyl silicone oil, comprising the following steps:

[0013] (1) mixing methylphenylcyclosiloxane and methylcyclosiloxane, and performing a dehydration reaction to obtain a mixed solution;

[0014] (2) adding a capping agent and an alkaline catalyst to the mixed solution obtained in step (1), and reacting at a temperature of 130 to 140° C. to obtain a reaction solution;

[0015] (3) The reaction solution obtained in step (2) is heated to 170-180° C., the catalyst and low-boiling substances are removed, and the product modified cyclized vinyl silicone oil is obtained.

[0016] In some embodiments, in step (1), the methylphenylcyclosiloxane is selected from one or more of trimethyltriphenylcyclotrisiloxane, tetramethyltetraphenylcyclotetrasiloxane and pentamethylpentaphenylcyclopentasiloxane.

[0017] In some embodiments, in step (1), the methylcyclosiloxane is selected from octamethylcyclotetrasiloxane and / or decamethylcyclopentasiloxane.

[0018] In some embodiments, in step (1), the conditions for the dehydration reaction are: dehydration reaction at a temperature of 45 to 55° C. and a vacuum degree of -0.075 to -0.096 MPa for 0.5 to 2 hours.

[0019] In some embodiments, in step (2), the catalyst is one or more of sodium hydroxide, potassium hydroxide, and sodium carbonate solution, and the amount of the catalyst added is 0.1 to 0.5 mol‰ of the total amount of methylphenylcyclosiloxane and methylcyclosiloxane.

[0020] In some embodiments, in step (2), the end-capping agent is a vinyl double-capping agent, and the amount of the end-capping agent added is 0.5 to 1 mol% of the total amount of methylphenylcyclosiloxane and methylcyclosiloxane.

[0021] According to another aspect of the present invention, there is also provided the use of the modified cyclized vinyl silicone oil or the modified cyclized vinyl silicone oil prepared according to the above preparation method in silicone rubber.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] (1) The present invention provides a modified cyclized vinyl silicone oil. By controlling the ratio of methylphenylsiloxane segments to methylsiloxane segments in the modified cyclized vinyl silicone oil and further controlling the molar ratio of silicon atoms to phenyl groups in the modified cyclized vinyl silicone oil, the modified cyclized vinyl silicone oil of the present invention has a high refractive index and high light transmittance, as well as good fluidity and better mechanical properties after curing.

[0024] (2) The preparation method of the modified cyclized vinyl silicone oil of the present invention is simple, and the amount of the end-capping agent is further controlled during the preparation process, so that the product structure is controllable, the molecular weight distribution is narrow, the product performance is more uniform, and it has a good industrial application prospect. DETAILED DESCRIPTION

[0025] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.

[0026] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.

[0027] Herein, when describing embodiments or examples, it should be understood that they are not used to limit the present invention to these embodiments or examples. On the contrary, all substitutes, improvements and equivalents of the methods and materials described in the present invention can be included in the scope limited by the claims.

[0028] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.

[0029] The present invention provides a modified cyclized vinyl silicone oil having a structure shown in formula (1):

[0030]

[0031] Wherein, Vi represents vinyl, m>0, n>0, 0.6≤n / m+n≤0.8, and m and n are both positive integers.

[0032] Preferably, m is preferably 20 to 100; n is preferably 20 to 200; and the value of n / m+n is preferably greater than or equal to 0.65 and less than or equal to 0.7. The inventors of the present invention have found that the proportion of methylphenylsiloxane segments in the modified cyclized vinyl silicone oil is critical to the refractive index and light transmittance. Further, by controlling the ratio of n / m+n within a suitable range, the prepared modified cyclized vinyl silicone oil has excellent refractive index and light transmittance. If the ratio of n / m+n is lower than 0.6, the refractive index will be greatly reduced. If the ratio of n / m+n is higher than 0.8, the light transmittance of the modified cyclized vinyl silicone oil will be greatly reduced, and the polymer tends to be unclear.

[0033] In some embodiments, the number average molecular weight of the modified cyclized vinyl silicone oil is 3500-35000, preferably 5000-20000; the molecular weight distribution index PDI is 1.4-1.6.

[0034] In some embodiments, in the modified cyclized vinyl silicone oil, the molar ratio of silicon atoms to phenyl groups is 1.4 to 1.7, preferably 1.5 to 1.6. To the surprise of the inventors of the present invention, the inventors of the present invention found that by further controlling the molar ratio of silicon atoms to phenyl groups in the modified cyclized vinyl silicone oil within the range, the prepared modified cyclized vinyl silicone oil has better fluidity and mechanical properties after curing. If the molar ratio of silicon atoms to phenyl groups is lower than 1.4, although the hardness after curing is higher, the viscosity of the modified cyclized vinyl silicone oil is larger, the fluidity is poor, and the flexibility of the cured product is poor; if the molar ratio of silicon atoms to phenyl groups is higher than 1.7, the fluidity of the modified cyclized vinyl silicone oil is better, but the hardness of the cured product is lower.

[0035] According to another aspect of the present invention, there is also provided a method for preparing the above-mentioned modified cyclized vinyl silicone oil, comprising the following steps:

[0036] (1) mixing methylphenylcyclosiloxane and methylcyclosiloxane, and performing a dehydration reaction to obtain a mixed solution;

[0037] (2) adding a capping agent and an alkaline catalyst to the mixed solution obtained in step (1), and reacting at a temperature of 130 to 140° C. to obtain a reaction solution;

[0038] (3) The reaction solution obtained in step (2) is heated to 170-180° C., the catalyst and low-boiling substances are removed, and the product modified cyclized vinyl silicone oil is obtained.

[0039] According to the preparation method of the present invention, methylphenylcyclosiloxane and methylcyclosiloxane are first mixed, dehydrated, and a mixed solution is obtained. In some embodiments, the methylphenylcyclosiloxane is selected from one or more of trimethyltriphenylcyclotrisiloxane, tetramethyltetraphenylcyclotetrasiloxane and pentamethylpentaphenylcyclopentasiloxane. In some embodiments, the methylcyclosiloxane is selected from octamethylcyclotetrasiloxane and / or decamethylcyclopentasiloxane. In some embodiments, the conditions of the dehydration reaction are: dehydration reaction for 0.5 to 2 hours at a temperature of 45 to 55° C. and a vacuum degree of -0.075 to -0.096 MPa. Preferably, in some embodiments, the conditions of the dehydration reaction are preferably: dehydration reaction for 1 to 1.5 hours at a temperature of 50 to 55° C. and a vacuum degree of -0.08 to -0.09 MPa.

[0040] According to the preparation method of the present invention, it also includes adding a capping agent and an alkaline catalyst to the mixed solution obtained by the dehydration reaction, reacting at a temperature of 130 to 140°C to obtain a reaction solution. In some embodiments, the catalyst is one or more of sodium hydroxide, potassium hydroxide, and sodium carbonate solution, and the amount of the catalyst added is 0.1 to 0.5 mol‰ of the total amount of methylphenylcyclosiloxane and methylcyclosiloxane. In some embodiments, the capping agent is a vinyl double cap, and the amount of the capping agent added is 0.5 to 1 mol% of the total amount of methylphenylcyclosiloxane and methylcyclosiloxane. In some embodiments, after adding the capping agent and the alkaline catalyst to the mixed solution obtained by the dehydration reaction, react at a temperature of 130 to 140°C for 2-5h.

[0041] The inventors of the present invention have found that the end-capping agent has a crucial influence on the molecular weight and distribution of the polymer. As the amount of the end-capping agent increases, the molecular weight decreases. And as the amount of the end-capping agent increases, the molecular weight distribution shows the characteristics of first decreasing and then increasing. When the content of the end-capping agent is too little, the end-capping effect is not obvious and the molecular weight distribution is wide. When the amount of the end-capping agent is increased to a certain extent, the end-capping effect is good in the area with high concentration, and the end-capping effect is slightly poor in the area with low concentration, so it will also cause the molecular weight distribution to become wider. Therefore, in the present invention, by controlling the amount of the end-capping agent within the range, the molecular weight and molecular weight distribution of the polymer can be better regulated, and the molecular weight distribution of the modified cyclized vinyl silicone oil prepared according to the preparation method of the present invention is narrow, and the performance of the polymer is more uniform.

[0042] The preparation method according to the present invention further comprises heating the reaction solution obtained after the reaction to 170-180°C, removing the catalyst and low-boiling substances, and obtaining the product modified cyclized vinyl silicone oil. Preferably, in some embodiments, the catalyst and low-boiling substances are removed at a temperature of 170-180°C and a vacuum degree of -0.075 to -0.096 MPa to finally obtain a clear and transparent modified cyclized vinyl silicone oil.

[0043] According to another aspect of the present invention, there is also provided the use of the modified cyclized vinyl silicone oil or the modified cyclized vinyl silicone oil prepared according to the above preparation method in silicone rubber.

[0044] The present invention will be described in detail below by way of examples. It should be understood that the following examples are only used to further explain and illustrate the content of the present invention by way of example, and are not intended to limit the present invention.

[0045] Unless otherwise specified, the raw materials in the examples and comparative examples of the present invention are all commercially available, and the specific information is as follows:

[0046] Vinyl double head (99%), Shandong Qufu Chenguang Co., Ltd.; trimethyltriphenylcyclotrisiloxane, tetramethyltetraphenylcyclotetrasiloxane, pentamethylpentaphenylcyclopentasiloxane (99%), Shandong Qufu Chenguang Co., Ltd.; octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane (99%), Shandong Qufu Chenguang Co., Ltd.; potassium hydroxide, analytical grade; sodium hydroxide, analytical grade.

[0047] Example 1

[0048] The preparation method of the modified cyclized vinyl silicone oil described in this embodiment comprises the following steps:

[0049] (1) Tetramethyltetraphenylcyclotetrasiloxane and octamethylcyclotetrasiloxane were added into a three-necked flask at a molar ratio of 7:3, and mixed, and dehydrated for 1 hour at a temperature of 45° C. and a vacuum degree of -0.08 MPa to obtain a mixed solution;

[0050] (2) adding 1 mol% of vinyl double end cap and 0.5 mol‰ of potassium hydroxide to the obtained mixed solution, and reacting at 130°C for 5 hours to obtain a reaction solution;

[0051] (3) The obtained reaction solution is heated to 180° C., and the catalyst and low-boiling substances are removed under a vacuum condition of -0.08 MPa to obtain the product modified cyclized vinyl silicone oil.

[0052] Example 2

[0053] The preparation method of the modified cyclized vinyl silicone oil described in this embodiment comprises the following steps:

[0054] (1) adding trimethyltriphenylcyclotrisiloxane and octamethylcyclotetrasiloxane in a molar ratio of 3:1 into a three-necked flask and mixing, and dehydrating and reacting for 1.5 hours at a temperature of 55° C. and a vacuum degree of −0.09 MPa to obtain a mixed solution;

[0055] (2) adding 0.5 mol% of vinyl double end cap and 0.1 mol‰ of potassium hydroxide to the obtained mixed solution, and reacting at 140°C for 2 hours to obtain a reaction solution;

[0056] (3) The obtained reaction solution is heated to 170° C., and the catalyst and low-boiling substances are removed under a vacuum condition of −0.096 MPa to obtain a product, a modified cyclized vinyl silicone oil.

[0057] Example 3

[0058] The preparation method of the modified cyclized vinyl silicone oil described in this embodiment comprises the following steps:

[0059] (1) adding pentamethylpentaphenylcyclopentasiloxane and decamethylcyclopentasiloxane in a molar ratio of 13:7 into a three-necked flask and mixing them, and dehydrating and reacting them for 1.5 hours at a temperature of 50° C. and a vacuum degree of −0.096 MPa to obtain a mixed solution;

[0060] (2) adding 0.8 mol% of vinyl double-capped end cap and 0.3 mol‰ of sodium hydroxide to the obtained mixed solution, and reacting at 135°C for 3 hours to obtain a reaction solution;

[0061] (3) The obtained reaction solution was heated to 175° C., and the catalyst and low-boiling substances were removed under a vacuum condition of −0.09 MPa to obtain a product, a modified cyclized vinyl silicone oil.

[0062] Example 4

[0063] The preparation method of the modified cyclized vinyl silicone oil described in this embodiment comprises the following steps:

[0064] (1) Tetramethyltetraphenylcyclotetrasiloxane and octamethylcyclotetrasiloxane were added into a three-necked flask at a molar ratio of 3:2, and mixed, and dehydrated for 1 hour at a temperature of 45° C. and a vacuum degree of -0.08 MPa to obtain a mixed solution;

[0065] (2) adding 1 mol% of vinyl double end cap and 0.5 mol‰ of potassium hydroxide to the obtained mixed solution, and reacting at 130°C for 5 hours to obtain a reaction solution;

[0066] (3) The obtained reaction solution is heated to 180° C., and the catalyst and low-boiling substances are removed under a vacuum condition of -0.08 MPa to obtain the product modified cyclized vinyl silicone oil.

[0067] Comparative Example 1

[0068] The preparation method of this comparative example is the same as that of Example 1, except that the molar ratio of tetramethyltetraphenylcyclotetrasiloxane to octamethylcyclotetrasiloxane is 1:1.

[0069] Comparative Example 2

[0070] The preparation method of this comparative example is the same as that of Example 1, except that the molar ratio of tetramethyltetraphenylcyclotetrasiloxane to octamethylcyclotetrasiloxane is 9:1.

[0071] Comparative Example 3

[0072] The preparation method of this comparative example is the same as that of Example 1, except that the amount of vinyl double cap added is 0.3 mol% of the total amount of tetramethyltetraphenylcyclotetrasiloxane and octamethylcyclotetrasiloxane.

[0073] Comparative Example 4

[0074] The preparation method of this comparative example is the same as that of Example 1, except that the amount of vinyl double-capped end added is 1.2 mol% of the total amount of tetramethyltetraphenylcyclotetrasiloxane and octamethylcyclotetrasiloxane.

[0075] Performance Testing

[0076] The modified cyclized vinyl silicone oils described in Examples 1-4 of the present invention and Comparative Examples 1-4 were tested for performance according to the following test methods. The specific performance indicators are shown in Table 1.

[0077] Number average molecular weight Mn and molecular weight distribution index PDI: Agilent PL-GPC50 gel permeation chromatograph (GPC) was used with toluene as the mobile phase, polysiloxane sample as the standard sample, column temperature set to 35°C, separation column model HT2 (size 7.8×300mm), to determine the number average molecular weight Mn and molecular weight distribution index PDI of each sample.

[0078] The molar ratio of silicon atoms / phenyl groups and the proportion of methylphenylsiloxane chains in the modified cyclized vinyl silicone oil were analyzed by adding deuterated chloroform to the sample for dissolution. 1 HNMR test, by 1 The peak area of ​​the characteristic peaks of the HNMR spectrum determines the molar ratio of silicon atoms / phenyl groups and the proportion of the methylphenylsiloxane chain content in the modified cyclized vinyl silicone oil.

[0079] Light transmittance: Observe the color of the solution with the naked eye. Clear and transparent indicates good light transmittance, slightly clear indicates poor light transmittance, and milky turbid indicates extremely poor light transmittance.

[0080] Refractive index: The refractive index of the modified cyclized vinyl silicone oil was measured at 25°C using a WYA-2S digital Abbe refractometer.

[0081] Viscosity: The viscosity (mPa·s) of the modified cyclized vinyl silicone oil was tested according to GB / T22235-2008 “Determination of viscosity of liquids”.

[0082] Hardness of the cured product: 50g of modified cyclized vinyl silicone oil and 22.5g of hydrogen-containing silicone oil (produced by Dongguan Beiteli New Materials Co., Ltd.) were mixed, and then 2ppm of Karstedt catalyst was added, stirred evenly, vacuum degassed until no bubbles appeared, and placed in an oven at 150°C for 3h to obtain a cured product. The hardness of the cured product was tested using a Shore A durometer, and at least 3 parallel samples were tested to obtain the average value (D).

[0083] Table 1 Performance data of the modified cyclized vinyl silicone oils described in Examples 1-4 and Comparative Examples 1-4

[0084]

[0085]

[0086] As shown in Table 1, the refractive index and light transmittance of the modified cyclized vinyl silicone oils obtained in Examples 1-4 of the present application are relatively excellent, and the viscosity is moderate, the flowability is good, and the hardness of the cured product is appropriate. It can be seen from Example 1 and Comparative Examples 1-2 that the silicon atom / phenyl group molar ratio and the methylphenylsiloxane segment content ratio in the modified cyclized vinyl silicone oil are different. The silicon atom / phenyl group molar ratio in the modified cyclized vinyl silicone oil obtained in Comparative Example 1 is high, and the methylphenylsiloxane segment content ratio is low. It can be found that the refractive index and light transmittance are significantly reduced. The silicon atom / phenyl group molar ratio in the modified cyclized vinyl silicone oil obtained in Comparative Example 2 is low, and the methylphenylsiloxane segment content ratio is high. It can be found that its light transmittance is very low, and it is milky and turbid when observed with the naked eye. It can be seen from Example 1 and Comparative Examples 3-4 that the amount of the end-capping agent is very critical to the molecular weight and molecular weight distribution of the polymer. If the amount of the end-capping agent is too high or too low within a certain range, the molecular weight of the obtained modified cyclized vinyl silicone oil will decrease, and the molecular weight distribution index will increase significantly. The product performance uniformity is poor, and the light transmittance and refractive index will also decrease.

[0087] In summary, the present invention controls the ratio of methylphenylsiloxane chain segments to methylsiloxane chain segments in the modified cyclized vinyl silicone oil, and further controls the molar ratio of silicon atoms to phenyl groups in the modified cyclized vinyl silicone oil, so that the modified cyclized vinyl silicone oil of the present invention has a high refractive index and high light transmittance, and at the same time has good fluidity and better mechanical properties after curing.

[0088] Obviously, the above embodiments of the present invention are only examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made on the basis of the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.

Claims

1. A modified cyclized vinyl silicone oil having a structure as shown in formula (1): Formula (1) in, Vi represents vinyl, m>0, n>0, 0.6≤n / m+n≤0.8, m and n are both positive integers; In the modified cyclized vinyl silicone oil, the molar ratio of silicon atoms to phenyl groups is 1.4 to 1.7; The number average molecular weight of the modified cyclized vinyl silicone oil is 3500-35000, and the molecular weight distribution index PDI is 1.4-1.6; The preparation method of the modified cyclized vinyl silicone oil comprises the following steps: (1) Mix methylphenyl cyclosiloxane and methyl cyclosiloxane, and perform a dehydration reaction at a temperature of 45 to 55°C and a vacuum degree of -0.075 to -0.096 MPa for 0.5 to 2 h to obtain a mixed solution; (2) adding a capping agent and an alkaline catalyst to the mixed solution obtained in step (1), and reacting at a temperature of 130-140° C. for 2-5 hours to obtain a reaction solution; The end-capping agent is a vinyl double end-capping agent, and the amount of the end-capping agent added is 0.5-1 mol% of the total amount of methylphenyl cyclosiloxane and methyl cyclosiloxane; The alkaline catalyst is sodium hydroxide or potassium hydroxide, and the amount of the alkaline catalyst added is 0.1-0.5 mol‰ of the total amount of methylphenylcyclosiloxane and methylcyclosiloxane; (3) The reaction solution obtained in step (2) is heated to 170-180° C., the catalyst and low-boiling substances are removed, and the product modified cyclized vinyl silicone oil is obtained.

2. The modified cyclized vinyl silicone oil according to claim 1, characterized in that: In step (1), the methylphenylcyclosiloxane is selected from one or more of trimethyltriphenylcyclotrisiloxane, tetramethyltetraphenylcyclotetrasiloxane and pentamethylpentaphenylcyclopentasiloxane.

3. The modified cyclized vinyl silicone oil according to claim 1, characterized in that: In step (1), the methylcyclosiloxane is selected from octamethylcyclotetrasiloxane and / or decamethylcyclopentasiloxane.

4. Use of the modified cyclized vinyl silicone oil according to any one of claims 1 to 3 in silicone rubber.