A homogenization method for positive electrode slurry and its application

By controlling the solid content of the slurry through a multi-step dispersion process, the problems of equipment wear and foreign matter introduction during the homogenization process of lithium-ion battery cathode slurry were solved, thereby extending equipment life and improving product quality.

CN117797672BActive Publication Date: 2026-11-17HONEYCOMB ENERGY TECH (SHANGRAO) CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202311857645.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-29
Publication Date
2026-11-17
Estimated Expiration
2043-12-29

AI Technical Summary

Technical Problem

In the current process of homogenizing lithium-ion battery cathode slurry, the high viscosity of the slurry leads to a heavy load on the equipment, easy wear, shortened equipment service life, and risk of foreign matter introduction, which affects product quality.

Method used

The pure dispersion process is adopted, eliminating the kneading step with high solid content and high viscosity. The solid content of the slurry is controlled through a multi-step dispersion process to avoid equipment wear. Low-speed dispersion and stirring are used to adjust the viscosity and ensure uniform mixing of materials.

Benefits of technology

This achieves thorough dispersion of the slurry, reduces equipment load, extends equipment lifespan, reduces the risk of foreign matter introduction, and improves product quality and production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117797672B_ABST
    Figure CN117797672B_ABST
Patent Text Reader

Abstract

This invention provides a homogenization method for positive electrode slurry and its application. The homogenization method includes the following steps: (1) mixing a first conductive agent, a binder, and a first portion of solvent, and dispersing them in one step to obtain a first dispersion; (2) mixing the first dispersion and a second conductive agent, and dispersing them in two steps to obtain a second dispersion; (3) mixing the second dispersion, positive electrode material, and a second portion of solvent, and dispersing them in three steps to obtain a third dispersion; (4) dispersing the third dispersion in four steps and adjusting the viscosity to obtain the positive electrode slurry. This invention eliminates the high-solids-content, high-viscosity kneading step through a pure dispersion process, and controls the solids content of the slurry in each step of the process. This ensures the dispersion of the slurry and avoids excessive wear and load on the equipment caused by high-solids-content, high-viscosity slurry, which has a positive effect on reducing product manufacturing costs and improving product quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of battery materials technology, and relates to a homogenization method for positive electrode slurry and its application. Background Technology

[0002] With the rapid development of the new energy industry, the number of lithium-ion battery companies has gradually increased, leading to fierce competition. In order to save costs and increase the price advantage of products, the positive electrode slurry process in the current lithium-ion battery manufacturing process mostly adopts the dry mixing process.

[0003] The dry mixing process eliminates the initial preparation of the adhesive solution. The main materials, binders, conductive agents, and other materials are directly added to the homogenizing tank for dispersion, thereby saving on equipment and space investment, while also speeding up the production cycle and increasing capacity.

[0004] CN111632509A discloses a homogenization method for lithium-ion battery positive electrode slurry, with the following steps: S1, using an automatic feeding system, positive electrode active material, conductive agent dry powder, and binder dry powder are fed into a double planetary mixer in proportion to premix the powders and obtain a dry powder mixture; S2, the solvent is divided into two parts, and conductive agent slurry and one part of solvent are added to the dry powder mixture prepared in step S1 in proportion to perform the first mixing to obtain a semi-finished slurry; S3, a high-speed mixer is turned on, and the semi-finished slurry obtained in step S2 and the other part of solvent are fed into the high-speed mixer for high-speed mixing and dispersion, and the mixed slurry is pumped into circulation tank A; S4, the slurry in circulation tank A is fed into the high-speed mixer again for high-speed mixing and dispersion, and the mixed slurry is pumped into circulation tank B.

[0005] CN112687872A discloses a lithium-sulfur battery positive electrode slurry, its homogenization method, and its uses. The homogenization method includes: mixing positive electrode material powder and conductive agent powder, adding a binder and mixing again, and finally adding a dispersant to obtain the lithium-sulfur battery positive electrode slurry. This invention utilizes a dry mixing method, pre-mixing the positive electrode material powder and conductive agent powder, and then sequentially adding the binder and dispersant to ensure uniform mixing of the positive electrode material, conductive agent, and binder.

[0006] During the homogenization process described above, the high viscosity of the slurry leads to a heavy load on the equipment, making it prone to wear and tear. This results in frequent equipment downtime, shortening the equipment's service life. Furthermore, the wear and tear poses a risk of introducing foreign matter, which can affect product quality. Summary of the Invention

[0007] The purpose of this invention is to provide a homogenization method for positive electrode slurry and its application. This invention eliminates the kneading step with high solid content and high viscosity through a pure dispersion process. The solid content of the slurry is controlled in each step of the process, which not only ensures the dispersion of the slurry, but also avoids excessive wear and load on the equipment caused by high solid content and high viscosity slurry. This has a positive effect on reducing product manufacturing costs and improving product quality.

[0008] To achieve this objective, the present invention adopts the following technical solution:

[0009] In a first aspect, the present invention provides a method for homogenizing a positive electrode slurry, the homogenization method comprising the following steps:

[0010] (1) The first conductive agent, the binder and the first portion of the solvent are mixed and dispersed in one step to obtain the first dispersion;

[0011] (2) The first dispersion and the second conductive agent are mixed and dispersed in two steps to obtain the second dispersion;

[0012] (3) Mix the second dispersion, the positive electrode material, and the second solvent, and disperse them in three steps to obtain the third dispersion;

[0013] (4) The third dispersion is dispersed in four steps and the viscosity is adjusted to obtain the positive electrode slurry.

[0014] This invention employs a pure dispersion process, eliminating the kneading step involved in high-viscosity, high-solids-content processes. It directly disperses the various materials in the positive electrode, controlling the slurry solids content during the process. This avoids equipment load alarms and wear risks caused by the kneading process, thereby improving equipment lifespan and product quality.

[0015] Preferably, the adhesive in step (1) comprises polyvinylidene fluoride.

[0016] Preferably, the solvent comprises N-methylpyrrolidone.

[0017] Preferably, the first conductive agent comprises carbon nanotubes.

[0018] Preferably, the first portion of solvent accounts for 60-70% of the total solvent, for example: 60%, 62%, 65%, 68% or 70%, etc.

[0019] Preferably, the solid content of the mixed solution obtained after mixing is <10%.

[0020] Preferably, the revolution speed of the one-step dispersion in step (1) is 20 to 40 rpm, for example: 20 rpm, 25 rpm, 30 rpm, 35 rpm or 40 rpm, etc.

[0021] Preferably, the rotation speed of the one-step dispersion is 700-1000 rpm, for example: 700 rpm, 750 rpm, 800 rpm, 900 rpm or 1000 rpm, etc.

[0022] Preferably, the dispersion time in the first step is 20 to 60 minutes, for example: 20 minutes, 30 minutes, 40 minutes, 50 minutes or 60 minutes.

[0023] Preferably, in step (2), the second conductive agent comprises conductive carbon black.

[0024] Preferably, the solid content of the mixed solution obtained after mixing is <15%.

[0025] Preferably, the two-step dispersion revolution speed in step (2) is 20 to 40 rpm, for example: 20 rpm, 25 rpm, 30 rpm, 35 rpm or 40 rpm, etc.

[0026] Preferably, the rotation speed of the two-step dispersion is 800-1100 rpm, for example: 800 rpm, 850 rpm, 900 rpm, 1000 rpm or 1100 rpm, etc.

[0027] Preferably, the two-step dispersion time is 60 to 90 minutes, for example: 60 minutes, 65 minutes, 70 minutes, 80 minutes or 90 minutes.

[0028] Preferably, the cathode material in step (3) includes any one or a combination of at least two of the following: ternary cathode material, lithium iron phosphate cathode material, lithium manganese iron phosphate cathode material, lithium manganese oxide cathode material, or lithium cobalt oxide cathode material.

[0029] Preferably, the second portion of solvent accounts for 30-40% of the total solvent, for example: 30%, 32%, 35%, 38% or 40%, etc.

[0030] Preferably, the three-step dispersion revolution speed in step (3) is 10 to 30 rpm, for example: 10 rpm, 15 rpm, 20 rpm, 25 rpm or 30 rpm, etc.

[0031] Preferably, the rotation speed of the three-step dispersion is 200-500 rpm, for example: 20 rpm, 25 rpm, 30 rpm, 40 rpm or 50 rpm.

[0032] The three-step dispersion method described in this invention employs low-speed dispersion with a low rotation speed to prevent material splashing and equipment wear, and primarily ensures sufficient wetting of the material.

[0033] Preferably, the three-step dispersion time is 10 to 20 minutes, for example: 10 rpm, 12 rpm, 15 rpm, 18 rpm or 20 rpm, etc.

[0034] Preferably, the solid content of the third dispersion in step (4) is ≤75%.

[0035] Preferably, the revolution speed of the four steps is 30 to 50 rpm, for example: 30 rpm, 35 rpm, 40 rpm, 45 rpm or 50 rpm.

[0036] Preferably, the rotation speed of the four-step dispersion is 1000-1400 rpm, for example: 1000 rpm, 1100 rpm, 1200 rpm, 1300 rpm or 1400 rpm, etc.

[0037] Preferably, the dispersion time for the four steps is 90 to 120 minutes, for example: 90 minutes, 95 minutes, 100 minutes, 110 minutes or 120 minutes.

[0038] Preferably, the method of adjusting viscosity in step (4) includes adding solvent and then stirring.

[0039] Preferably, the rotation speed of the stirring is 500 to 800 rpm, for example: 500 rpm, 550 rpm, 600 rpm, 700 rpm or 800 rpm.

[0040] Preferably, the revolution speed of the stirring is 20 to 40 rpm, for example: 20 rpm, 25 rpm, 30 rpm, 35 rpm or 40 rpm.

[0041] Preferably, the stirring time is 10 to 30 minutes, for example: 10 minutes, 15 minutes, 20 minutes, 25 minutes or 30 minutes.

[0042] In a second aspect, the present invention provides a positive electrode slurry, which is prepared by the homogenization method described in the first aspect.

[0043] The homogenization method described in this invention produces a slurry with good dispersion, and the coated electrode has no abnormal appearance. The load current during the homogenization process is much lower than the rated maximum current of the equipment, and the slurry has low solid content and low viscosity, resulting in less wear on the equipment.

[0044] Compared with the prior art, the present invention has the following beneficial effects:

[0045] (1) The present invention can achieve full dispersion of positive electrode slurry, and the processing effect is no different from that of conventional process, but can reduce the equipment load during the stirring process, thereby reducing the wear on the homogenizing equipment, preventing the rapid reduction of equipment service life and the risk of foreign matter introduction.

[0046] (2) The maximum limit average current of the equipment during the homogenization process of the homogenization method of the present invention can be as low as 133.7A, which is significantly lower than that of conventional process (195A). Attached Figure Description

[0047] Figure 1 This is a process flow diagram of the homogenization method according to an embodiment of the present invention.

[0048] Figure 2 This is a SEM image of the positive electrode slurry described in Embodiment 1 of the present invention.

[0049] Figure 3 This is a SEM image of the positive electrode slurry described in Comparative Example 1.

[0050] Figure 4 This is a coating appearance diagram of the positive electrode slurry described in Embodiment 1 of the present invention.

[0051] Figure 5 This is a coating appearance diagram of the positive electrode slurry described in Comparative Example 1. Detailed Implementation

[0052] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.

[0053] Example 1

[0054] This embodiment provides a homogenization method for positive electrode slurry, and the process flow diagram of the homogenization method is as follows. Figure 1 As shown, the homogenization method includes the following steps:

[0055] (1) Mix polyvinylidene fluoride, carbon nanotubes and 65% NMP, and disperse at a revolution speed of 30 rpm and a rotation speed of 800 rpm for 40 min to obtain the first dispersion (solid content <10%).

[0056] (2) After adding conductive carbon black, disperse it for 60 min at a revolution speed of 30 rpm and a rotation speed of 900 rpm to obtain a second dispersion (solid content <15%).

[0057] (3) Add ternary cathode material and the remaining 35% NMP, disperse at a revolution speed of 20 rpm and a rotation speed of 500 rpm for 10 min to obtain the third dispersion (solid content <75%).

[0058] (4) The third dispersion was dispersed at a revolution speed of 40 rpm and a rotation speed of 1200 rpm for 90 min. NMP was added to adjust the viscosity, and the mixture was stirred at a revolution speed of 30 rpm and a rotation speed of 600 rpm to obtain the positive electrode slurry. The SEM image of the slurry is shown below. Figure 1 As shown.

[0059] Example 2

[0060] This embodiment provides a homogenization method for positive electrode slurry, and the process flow diagram of the homogenization method is as follows. Figure 1 As shown, the homogenization method includes the following steps:

[0061] (1) Mix polyvinylidene fluoride, carbon nanotubes and 60% NMP, and disperse at a revolution speed of 20 rpm and a rotation speed of 700 rpm for 60 min to obtain the first dispersion (solid content <10%).

[0062] (2) After adding conductive carbon black, disperse it for 90 minutes at a revolution speed of 20 rpm and a rotation speed of 800 rpm to obtain a second dispersion (solid content <15%).

[0063] (3) Add ternary cathode material and the remaining 40% NMP, disperse at a revolution speed of 10 rpm and a rotation speed of 200 rpm for 20 min to obtain the third dispersion (solid content <75%).

[0064] (4) The third dispersion was dispersed for 120 minutes at a revolution speed of 30 rpm and a rotation speed of 1000 rpm. NMP was added to adjust the viscosity. The mixture was stirred at a revolution speed of 20 rpm and a rotation speed of 500 rpm to obtain the positive electrode slurry.

[0065] Example 3

[0066] This embodiment provides a homogenization method for positive electrode slurry, and the process flow diagram of the homogenization method is as follows. Figure 1 As shown, the homogenization method includes the following steps:

[0067] (1) Mix polyvinylidene fluoride, carbon nanotubes and 70% NMP, and disperse at a revolution speed of 40 rpm and a rotation speed of 1000 rpm for 20 min to obtain the first dispersion (solid content <10%).

[0068] (2) After adding conductive carbon black, disperse it for 90 min at a revolution speed of 40 rpm and a rotation speed of 1100 rpm to obtain a second dispersion (solid content <15%).

[0069] (3) Add ternary cathode material and the remaining 30% NMP, disperse at a revolution speed of 30 rpm and a rotation speed of 500 rpm for 10 min to obtain the third dispersion (solid content <75%).

[0070] (4) The third dispersion was dispersed at a revolution speed of 50 rpm and a rotation speed of 1400 rpm for 90 min. NMP was added to adjust the viscosity. The mixture was stirred at a revolution speed of 30 rpm and a rotation speed of 600 rpm to obtain the positive electrode slurry.

[0071] Example 4

[0072] The only difference between this embodiment and embodiment 1 is that the solid content of the first dispersion in step (1) is 12%, while the other conditions and parameters are exactly the same as in embodiment 1.

[0073] Example 5

[0074] The only difference between this embodiment and embodiment 1 is that the solid content of the second dispersion in step (2) is 18%, while the other conditions and parameters are exactly the same as in embodiment 1.

[0075] Example 6

[0076] The only difference between this embodiment and Embodiment 1 is that the solid content of the third dispersion in step (3) is 78%, while the other conditions and parameters are exactly the same as in Embodiment 1.

[0077] Comparative Example 1

[0078] This comparative example provides a method for homogenizing a positive electrode slurry, the method comprising the following steps:

[0079] (1) Mix polyvinylidene fluoride and conductive carbon black, and disperse them for 30 minutes at a revolution speed of 20 rpm and a rotation speed of 200 rpm to obtain a mixture.

[0080] (2) After adding carbon nanotubes and 40% NMP, kneading with high solid content and high viscosity was carried out at a revolution speed of 30 rpm for 60 min.

[0081] (3) Add the ternary cathode material and the remaining 60% NMP, disperse at a revolution speed of 35 rpm and a rotation speed of 1100 rpm for 90 min, then disperse at a revolution speed of 40 rpm and a rotation speed of 1200 rpm for 90 min. Add NMP to adjust the viscosity, and stir at a revolution speed of 30 rpm and a rotation speed of 600 rpm to obtain the cathode slurry. The SEM image of the cathode slurry is shown below. Figure 3 As shown.

[0082] Performance testing:

[0083] The maximum limiting current of the equipment during the homogenization process of the examples and comparative examples was recorded. Data was collected three times, and the test results are shown in Table 1.

[0084] Table 1

[0085]

[0086]

[0087] As can be seen from Table 1, and from Examples 1-3, the maximum limit average current of the equipment during the homogenization process of the homogenization method of the present invention can reach below 133.7A, which is significantly lower than that of the conventional process (195A).

[0088] A comparison of Examples 1 and 4-6 shows that the solid content of the dispersion in each step of the homogenization process of the present invention affects the homogenization effect. By controlling the solid content of the first dispersion to below 10%, the solid content of the second dispersion to below 15%, and the solid content of the third dispersion to below 75%, the homogenization effect of the slurry is better, the instrument load current is smaller, the damage to the instrument is less, and the rapid reduction of equipment lifespan and the risk of foreign matter introduction can be effectively prevented.

[0089] The coating appearance of the positive electrode slurry described in Example 1 and Comparative Example 1 is shown in the following figures. Figure 4-5 As shown, a comparison between Example 1 and Comparative Example 1 reveals that the present invention employs a pure dispersion process, eliminating the kneading step involving high viscosity and high solids content, and directly dispersing the various materials of the positive electrode. This process controls the solids content of the slurry, thereby avoiding equipment load alarms and wear risks caused by the kneading process. The method achieves thorough dispersion of the positive electrode slurry, with processing results no different from conventional processes, but reduces the equipment load during the stirring process, thus minimizing wear on the homogenizing equipment.

[0090] The applicant declares that the above description is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention fall within the protection and disclosure scope of the present invention.

Claims

1. A method for homogenizing a positive electrode slurry, characterized in that, The homogenization method includes the following steps: (1) The first conductive agent, the binder and the first portion of the solvent are mixed and dispersed in one step to obtain the first dispersion; (2) The first dispersion and the second conductive agent are mixed and dispersed in two steps to obtain the second dispersion; (3) Mix the second dispersion, the positive electrode material, and the second solvent, and disperse them in three steps to obtain the third dispersion; (4) The third dispersion is dispersed in four steps, and the viscosity is adjusted to obtain the positive electrode slurry; The solid content of the mixed solution obtained after mixing in step (1) is <10%; The solid content of the mixed solution obtained after mixing in step (2) is <15%; The solid content of the third dispersion in step (4) is ≤75%; The first portion of solvent accounts for 60-70% of the total solvent volume; The second part of the solvent accounts for 30-40% of the total solvent.

2. The homogenization method as described in claim 1, characterized in that, The adhesive in step (1) includes polyvinylidene fluoride.

3. The homogenization method as described in claim 1, characterized in that, The first conductive agent includes carbon nanotubes.

4. The homogenization method as described in claim 1, characterized in that, The solvent includes N-methylpyrrolidone.

5. The homogenization method as described in claim 1, characterized in that, The orbital speed of the one-step dispersion in step (1) is 20~40 rpm.

6. The homogenization method as described in claim 5, characterized in that, The rotation speed of the first-step dispersion is 700~1000 rpm.

7. The homogenization method as described in claim 5, characterized in that, The dispersion time for this step is 20-60 minutes.

8. The homogenization method as described in claim 1, characterized in that, Step (2) The second conductive agent includes conductive carbon black.

9. The homogenization method as described in claim 1, characterized in that, The orbital speed of the two-step dispersion in step (2) is 20~40 rpm.

10. The homogenization method as described in claim 9, characterized in that, The rotation speed of the two-step dispersion is 800~1100 rpm.

11. The homogenization method as described in claim 9, characterized in that, The two-step dispersion takes 60-90 minutes.

12. The homogenization method as described in claim 1, characterized in that, The cathode material in step (3) includes any one or a combination of at least two of the following: ternary cathode material, lithium iron phosphate cathode material, lithium manganese iron phosphate cathode material, lithium manganese oxide cathode material, or lithium cobalt oxide cathode material.

13. The homogenization method as described in claim 1, characterized in that, The revolution speed of the three steps in step (3) is 10~30 rpm.

14. The homogenization method as described in claim 13, characterized in that, The rotation speed of the three-step dispersion is 200~500 rpm.

15. The homogenization method as described in claim 13, characterized in that, The three-step dispersion process takes 10-20 minutes.

16. The homogenization method as described in claim 1, characterized in that, The revolution speed of the four-step dispersion is 30~50 rpm.

17. The homogenization method as described in claim 16, characterized in that, The rotation speed of the four-step dispersion is 1000~1400 rpm.

18. The homogenization method as described in claim 16, characterized in that, The time for the four-step dispersion is 90~120 minutes.

19. The homogenization method as described in claim 1, characterized in that, The method of adjusting viscosity in step (4) includes adding solvent and then stirring.

20. The homogenization method as described in claim 19, characterized in that, The stirring mechanism rotates at a speed of 500-800 rpm.

21. The homogenization method as described in claim 19, characterized in that, The stirring speed is 20~40 rpm.

22. The homogenization method as described in claim 19, characterized in that, The stirring time is 10-30 minutes.

23. A positive electrode slurry, characterized in that, The positive electrode slurry is prepared by the homogenization method as described in any one of claims 1-22.

Citation Information

Patent Citations

  • Homogenizing method of lithium ion battery positive electrode slurry

    CN111632509A

  • Lithium-sulfur battery positive electrode slurry as well as homogenizing method and application thereof

    CN112687872A

  • Homogenizing process and application thereof

    CN116407992A

  • Lithium ion battery positive electrode homogenizing process

    CN116705996A