An accelerometer based on a two-dimensional thin film and its fabrication method
By using two-dimensional thin film materials such as graphene and MoS2 as sensing materials and combining them with wafer bonding technology to fabricate MEMS accelerometers, the problem of excessively large sensor chip size has been solved, and a high-performance and high-yield accelerometer has been realized.
Patent Information
- Application Number
- CN202311729727.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-15
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-12-15
AI Technical Summary
How to further reduce the size of MEMS accelerometer chips while ensuring good performance?
Two-dimensional thin films such as graphene, molybdenum disulfide (MoS2) and other transition metal sulfide (TMDC) materials, as well as graphene/TMDC heterolayers, are used as sensitive thin films for piezoresistive and resonant accelerometers. Accelerometers are fabricated using wafer bonding and micro/nano fabrication techniques, and the conversion of acceleration signals is achieved by utilizing the deformation and piezoresistive effect of the two-dimensional thin film.
This significantly reduces the size of the accelerometer chip, improves sensor performance (sensitivity, etc.), and increases device yield.
Smart Images

Figure CN117805436B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of acceleration sensor design and manufacturing, specifically relating to novel acceleration sensor sensitive materials, sensitive structures and their preparation methods. Background Technology
[0002] MEMS accelerometers are small devices manufactured using micro-nano fabrication technology that convert acceleration signals into other detectable signals. Compared to other accelerometers, MEMS accelerometers offer advantages such as miniaturization, low cost, and ease of use. Based on their detection principles, MEMS accelerometers can be categorized into piezoresistive, capacitive, and resonant types, among others. Currently, traditional MEMS accelerometers are generally based on silicon materials. However, due to the inherent physical properties of silicon, silicon-based accelerometers face the technical challenge of balancing miniaturization and high performance. Furthermore, as the demands on accelerometers continue to increase, this problem becomes increasingly prominent. Therefore, the development of novel accelerometers is of great significance.
[0003] Novel two-dimensional materials, represented by graphene, possess excellent electromechanical properties. Graphene, in particular, exhibits a Young's modulus of up to 1 TPa, a tensile strength of 130 GPa, a strain capacity of 25%, and a piezoresistive effect, with its piezoresistive strain coefficient (GF) typically reported to be 2–6. Graphene's atomic-layer thickness allows it to undergo significant deformation under stress, resulting in highly sensitive accelerometers based on it. Furthermore, graphene's chemical stability makes it compatible with micro / nano fabrication technologies. On the other hand, reports indicate that two-dimensional transition metal sulfides (TMDCs), such as molybdenum disulfide (MoS2), tungsten disulfide (WuS2), molybdenum diselenide (MoSe2), tungsten diselenide (WuSe2), and platinum diselenide (PtSe2), also possess good electromechanical properties, with theoretically predicted piezoresistive strain coefficients reaching hundreds or even thousands. The sensitivity of piezoresistive accelerometers is closely related to the piezoresistive strain coefficient of the sensitive material. Therefore, TMDC materials such as MoS2, WuS2, MoSe2, and WuSe2 have the potential to significantly improve the sensitivity of MEMS accelerometers.
[0004] Given the above, further miniaturizing the size of accelerometer chips while maintaining high device performance is a pressing technical challenge. To address this challenge, this invention proposes using two-dimensional thin films such as graphene, MoS2, and other TMDC materials, as well as graphene / TMDC heterolayers, as the sensitive films for piezoresistive and resonant accelerometers. A fabrication method for accelerometers based on these two-dimensional thin films is also proposed. This will significantly reduce the size of the accelerometer chip, substantially improve the performance (sensitivity, etc.) of the accelerometer, and greatly improve device yield. Summary of the Invention
[0005] The technical problem this invention aims to solve is how to further reduce the size of MEMS accelerometer chips while maintaining good performance. This invention proposes using two-dimensional thin films such as graphene, molybdenum disulfide (MoS2) and other transition metal sulfide (TMDC) materials, and graphene / TMDC heterolayers as sensitive materials for piezoresistive and resonant accelerometer sensors. A method for fabricating accelerometer sensors based on two-dimensional thin films is also proposed. The specific technical solution is as follows: An accelerometer based on a two-dimensional thin film is integrated with a silicon MEMS substrate, with a Si / SiO2 mass suspended by the two-dimensional thin film. The device is composed of two wafers bonded together. The upper wafer has a cavity with a silicon support frame at the upper edge of the cavity. A two-dimensional sensitive film supported by the silicon support frame is placed above the cavity, and a Si / SiO2 mass is suspended below the two-dimensional sensitive film. The lower wafer has a through-hole cavity that communicates with the cavity of the upper wafer. Under the action of acceleration, the Si / SiO2 mass causes the two-dimensional sensitive film to deform. The deformed two-dimensional sensitive film can convert the acceleration signal into other detectable signals. The cavity and the through-hole cavity enable the Si / SiO2 mass to move in a direction perpendicular to the plane of the silicon support frame when subjected to acceleration.
[0006] The two-dimensional sensitive film can be a two-dimensional film such as graphene, molybdenum disulfide (MoS2) transition metal sulfide (TMDC) material, or graphene / TMDC heterolayer.
[0007] The SiO2 layer on the surface of the Si / SiO2 mass block can enhance the adhesion between the two-dimensional sensitive film and the Si / SiO2 mass block.
[0008] When an external acceleration is applied to a mass block suspended in a two-dimensional thin film, a resonant frequency detection device connected to an external device, such as a laser Doppler vibrometer (LDV), is used to detect the shift in the resonant frequency of the sensitive structure of the suspended mass block in the two-dimensional thin film, thus forming a resonant acceleration sensor. When the device is subjected to acceleration, the two-dimensional sensitive film deforms, causing a change in the stress of the two-dimensional sensitive film, which in turn causes a change in the resonant frequency of the two-dimensional sensitive film. By detecting the change in the resonant frequency, the acceleration can be detected.
[0009] A piezoresistive accelerometer is constructed by connecting a two-dimensional sensitive thin film to a circuit via electrodes. When the device is subjected to acceleration, the two-dimensional sensitive thin film deforms. Due to the piezoresistive effect of the two-dimensional material, the resistance of the two-dimensional sensitive thin film changes. By applying a constant current to the two-dimensional sensitive thin film through electrodes or by placing the two-dimensional sensitive thin film in a circuit structure such as a Wheatstone bridge, the change in resistance of the two-dimensional sensitive thin film can be converted into a change in voltage, so as to collect the signal.
[0010] The types of two-dimensional sensitive thin film materials can be graphene, TMDC materials such as MoS2, hexagonal boron nitride, MXene, graphene / TMDC heterolayer, hexagonal boron nitride / graphene heterolayer, graphene / MXene heterolayer, hexagonal boron nitride / TMDC heterolayer, TMDC / MXene heterolayer, metal thin films (gold, silver, platinum, aluminum) and their heterolayers with two-dimensional materials such as graphene, metal oxide thin films and their heterolayers with two-dimensional materials such as graphene (alumina / graphene heterolayer, etc.), organic polymers and their heterolayers with two-dimensional materials such as graphene (polymethyl methacrylate / graphene heterolayer, etc.), silicon nitride and graphene heterolayers, etc.
[0011] The thickness of the two-dimensional sensitive film can be a single atomic layer, two atomic layers, three atomic layers, four atomic layers, five atomic layers, six atomic layers, seven atomic layers, eight atomic layers, nine atomic layers, ten atomic layers, and thicker two-dimensional material films (0~1000nm).
[0012] The bottom shape of the Si / SiO2 mass block can be square, rectangular, circular, etc. If the bottom surface is rectangular, the dimensions include 100nm*100nm to 1mm*1mm, and the height includes 100nm to 1mm; if the bottom surface is circular, the diameter includes 10nm to 1mm, and the height includes 100nm to 1mm.
[0013] The width of the cavity ranges from 100nm to 1mm, and the size of the through-hole cavity ranges from 150nm*150nm to 1.5mm*1.5mm.
[0014] The accelerometer is composed of two bonded structures. The upper structure includes a silicon support frame, a two-dimensional sensitive film, a Si / SiO2 mass block, and a cavity. The lower structure includes a through-hole cavity that communicates with the upper cavity.
[0015] A method for fabricating a two-dimensional thin-film accelerometer includes the following steps: (1) Thermal oxidation (first Si substrate) A silicon wafer is thermally oxidized to grow a layer of SiO2 on the upper and lower surfaces of the wafer.
[0016] (2) SiO2 etching Based on step (1), photoresist is coated onto the wafer and exposed and developed. The SiO2 layer is etched using reactive ion beam (RIE) technology.
[0017] (3) Electrode preparation Based on step (2), electrodes are fabricated using metal deposition processes such as evaporation and sputtering. After electrode deposition, photoresist residue is removed using a metal lift-off process.
[0018] (4) Back etching Based on step (3), a layer of photoresist is coated on the back side of the wafer, and it is exposed and developed to define the location of the cavity. The SiO2 layer on the back side of the wafer is etched using RIE (Reactive Ion Etching) process, and the Si layer on the wafer is etched using Deep Reactive Ion Beam (DRIE) process. When etching reaches the SiO2 layer on the upper surface, the etching is stopped. At this point, the cavity has been initially formed.
[0019] (5) Thermal oxidation (second Si substrate) Take a second silicon wafer and perform thermal oxidation to grow a layer of SiO2 on its upper and lower surfaces.
[0020] (6) Etching the Si / SiO2 substrate to form through-hole cavities Based on step (5), the silicon wafer is coated with photoresist, exposed and developed, etc. The position of the via cavity in the wafer is defined according to the cavity formed in step (4). Then, the SiO2 layer and Si layer of the second silicon wafer are etched by RIE and DRIE processes respectively to form the via cavity.
[0021] (7) Bonding the two processed silicon substrates (step (4) + step (6)) The structures formed in steps (4) and (6) are then wafer-bonded.
[0022] (8) Transfer of two-dimensional thin films such as graphene, MoS2 and other TMDC materials, and graphene / TMDC heterolayers. Based on step (7), various two-dimensional material transfer methods, such as wet transfer based on organic polymers such as PMMA as support layers and dry transfer represented by mechanical exfoliation, are used to transfer two-dimensional thin films such as graphene, MoS2 and other TMDC materials, and graphene / TMDC heterolayers to the surface of the device formed in step (7).
[0023] (9) Patterned etching of two-dimensional thin films such as graphene, MoS2 and other TMDC materials, and graphene / TMDC heterolayers. Based on step (8), traditional photolithography, laser etching or focused ion beam etching processes are used to pattern the transferred graphene, MoS2 and other TMDC materials, graphene / TMDC heterolayer and other two-dimensional thin films.
[0024] (10) Etch the SiO2 sacrificial layer to release the Si / SiO2 mass block. Based on step (9), the SiO2 layer in the cavity surrounding the Si / SiO2 mass block is etched using a gas phase hydrofluoric acid (HF) process to release the Si / SiO2 mass block.
[0025] In steps (1) and (5), the wafer size can be 2 inches, 4 inches, 6 inches, 8 inches, etc., and its thickness can be selected according to the size of the device to be manufactured.
[0026] Step (3) is used to prepare a piezoresistive accelerometer, wherein the deposited electrode includes two layers, one of which is a metal Ti in contact with the silicon substrate, and the other of which is a metal Au in contact with the metal Ti.
[0027] The bonding methods in step (7) include, but are not limited to, direct wafer bonding, anodic wafer bonding, binder wafer bonding, glass frit wafer bonding, eutectic wafer bonding, transient liquid phase (TLP) wafer bonding, metal hot pressing wafer bonding, etc.
[0028] The transfer methods in step (8) include wet transfer (transfer method with PMMA as support layer, transfer method without support layer), electrostatic transfer method, bubbling transfer method (electrochemical reaction transfer method, non-electrochemical bubbling assisted transfer method), heat release tape method, polydimethylsiloxane (PDMS) imprinting method and dry transfer (roll-to-roll transfer method, metal-assisted peeling method).
[0029] The etching process in step (9) includes: traditional photolithography, laser etching, and focused ion beam etching, etc. Attached Figure Description
[0030] Figure 1 This is a three-dimensional structural schematic diagram of the accelerometer sensor of the present invention. Figure 2 This is a three-dimensional cross-sectional view of the accelerometer sensor of the present invention. Figure 3 For graphene-based accelerometers, Figure 4 An accelerometer based on TMDC material, Figure 5 This is a process flow diagram of the accelerometer sensor of the present invention. Figure 6This is a cross-sectional view of the piezoresistive accelerometer sensor described in this invention. Figure 7 This is a cross-sectional view of the resonant accelerometer sensor described in this invention. Detailed Implementation
[0031] The present invention will now be described in detail with reference to specific embodiments. These embodiments will help those skilled in the art to further understand the present invention, but do not limit the invention in any way. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention. These all fall within the scope of protection of the present invention.
[0032] A two-dimensional thin-film accelerometer, such as Figure 1 The device includes a silicon support frame, a Si / SiO2 mass block, a two-dimensional sensitive film (including TMDC materials such as graphene and MoS2, and 2D films such as graphene / TMDC heterolayers), a cavity, a through-hole cavity, and electrodes. The silicon support frame suspends the sensitive film containing the Si / SiO2 mass block. Due to the presence of the cavity and through-hole cavity, when the device is subjected to acceleration, the Si / SiO2 mass block moves in a direction perpendicular to the plane of the silicon support frame. This movement of the Si / SiO2 mass block further deforms the two-dimensional sensitive film (including TMDC materials such as graphene and MoS2, and 2D films such as graphene / TMDC heterolayers), generating stress and strain. Because graphene and TMDC materials have a piezoresistive effect, the resistance of the sensitive film changes when stress is generated. For a piezoresistive accelerometer, by applying a constant current to the device through the electrodes at both ends of the two-dimensional sensitive film or through a circuit structure such as a Wheatstone bridge, the change in the resistance of the sensitive film can be converted into a change in voltage. The working principle of a resonant accelerometer is that when a Si / SiO2 mass block is subjected to acceleration, the two-dimensional sensitive film (including TMDC materials such as graphene and MoS2 and graphene / TMDC heterolayers) generates stress, and its resonant frequency will change. At this time, the change in acceleration can be read out by the change in the resonant frequency of the two-dimensional sensitive film.
[0033] 1. This invention relates to a two-dimensional thin-film accelerometer based on graphene. The Si / SiO2 mass block has a square bottom with dimensions of 100 μm x 100 μm and a height of 102 μm. The cavity size is 4 μm. The through-hole cavity has dimensions of 200 μm x 200 μm and a height of 302 μm. The two-dimensional sensitive film is made of a graphene / MoS2 heterolayer with dimensions of 150 μm wide and 200 μm long. The center of the two-dimensional sensitive film overlaps with the center of the Si / SiO2 mass block. The electrode has dimensions of 150 μm x 150 μm.
[0034] 2. For example Figure 5 As shown, the fabrication method for a two-dimensional thin-film accelerometer based on graphene and other materials in this embodiment includes the following steps: (1) For example Figure 5 As shown in (a), a silicon wafer with a thickness of 100 μm was cleaned and thermally oxidized to grow a 2 μm thick SiO2 layer on both the upper and lower surfaces of the wafer. The thermal oxidation conditions were: oxygen gas, temperature 1100℃, and time 100 min.
[0035] (2) For example Figure 5 As shown in (b), the silicon wafer in step (1) was spin-coated with photoresist, exposed and developed, and then etched with RIE (Rapid Etching) to determine the electrode positions. The photoresist was a PC solution, and the spin speeds were set sequentially as follows: 500 rpm for 5 seconds; 4000 rpm for 30 seconds; and 500 rpm for 5 seconds. The exposure method was ultraviolet exposure, and the etching machine model was MA 8.
[0036] (3) For example Figure 5 As shown in (c), a metal deposition process is performed at the SiO2 etching location in step (2) to fabricate the electrode. Subsequently, the photoresist is removed using a metal lift-off process. The photoresist used for electrode spin-coating should be applied in two separate spin-coating processes at different speeds. This is to ensure that the cross-sectional shape of the photoresist is trapezoidal after exposure and development, which facilitates its removal after metal deposition. The metal deposition should also be performed in two stages: first, Ti metal is deposited, and second, Au metal is deposited.
[0037] (4) For example Figure 5 As shown in (d), a layer of photoresist is spin-coated onto the back side of the silicon wafer and then exposed and developed to determine the location of the cavity. The SiO2 layer is etched using the RIE process, followed by the Si layer being etched using the DRIE process. After the Si layer is completely etched, the back side of the SiO2 layer on the silicon wafer surface will be exposed to the atmosphere to facilitate the release of the Si / SiO2 mass. Since the etched SiO2 and Si layers are relatively deep, the thickness of the spin-coated photoresist should be as thick as possible. The purpose of using the DRIE process for the Si layer etching is to ensure that the etched cavity is as perpendicular as possible.
[0038] (5) For example Figure 5 As shown in (e), another 300 μm thick silicon wafer was thermally oxidized to grow a 2 μm thick SiO2 layer on both the upper and lower surfaces of the wafer. The thermal oxidation conditions were: oxygen gas, temperature 1100℃, and time 100 min.
[0039] (6) For example Figure 5As shown in (f), in step (5), a layer of photoresist is spin-coated onto the surface of the silicon wafer and exposed and developed to determine the location of the via cavity. First, the surface SiO2 layer is etched using the RIE process. After the surface SiO2 layer is completely etched, the Si layer is etched using the DRIE process. After the Si layer is completely etched, the back SiO2 layer is etched using the RIE process. After the back SiO2 layer is completely etched, the final via cavity is formed. In this step, because the etching depth is relatively deep, the spin-coated photoresist should be as thick as possible.
[0040] (7) For example Figure 5 As shown in (g), the structures formed in steps (4) and (6) are bonded using a wafer direct bonding process.
[0041] (8) For example Figure 5 As shown in (h), two-dimensional films such as graphene, MoS2 and other TMDC materials, and graphene / TMDC heterolayers are transferred to the surface of the structure formed in step (7). The material transferred in this step is a graphene / MoS2 heterolayer. The specific steps are as follows: Take a piece of CVD copper-based graphene and spin-coat a layer of PMMA. The PMMA model is (AR-P 649.04, ALLRESIST). The spin-coating process is: 500 rpm, 5s; 2000 rpm, 30s. After spin-coating, bake at 100℃ for 4min. The graphite residue on the back of the copper-based graphene is removed using an oxygen plasma etching process. The graphene / PMMA film is placed in FeCl3 solution to remove the copper substrate. After the copper substrate is removed, in order to remove Fe 3+ Ions and Cl -1 The graphene / PMMA film was sequentially immersed in deionized water, HCl solution, and then in deionized water. A separate CVD copper-based MoS2 substrate was taken, and the graphene / PMMA film prepared in the above process was placed on the surface of the copper-based MoS2. The back side of the copper-based MoS2 was treated using oxygen plasma etching. The PMMA / graphene / MoS2 film was then immersed in FeCl3 solution to remove the copper substrate. After the copper substrate was removed, the PMMA / graphene / MoS2 film was sequentially immersed in deionized water, HCl solution, and then in deionized water to remove Fe. 3+ Ions and Cl -1 Ions. The PMMA / graphene / MoS2 film can then be transferred to a silicon substrate, and the PMMA is removed by immersion in an acetone solution. After PMMA removal, the graphene / MoS2 / silicon composite is then sequentially placed in isopropanol and deionized water.
[0042] (9) For example Figure 5 As shown in (i), based on the device fabricated in step 8, the graphene / MoS2 heterolayer transferred in step 8 is patterned and etched using a laser etching process.
[0043] (10) For example Figure 5 As shown in (j), based on step 9, vapor phase HF etching is performed to etch away the SiO2 layer on top of the cavity around the Si / SiO2 mass block, thereby releasing the Si / SiO2 mass block.
Claims
1. A method for fabricating an accelerometer based on a two-dimensional thin film, characterized in that, The sensor is composed of two wafers bonded together, with a two-dimensional thin film integrated onto a silicon MEMS substrate and a Si / SiO2 mass suspended beneath the thin film. The upper wafer has a cavity with a silicon support frame along its upper edge. A two-dimensional sensitive thin film, supported by the silicon support frame, is positioned above the cavity, and a Si / SiO2 mass is suspended below it. The lower wafer has a via cavity connected to the cavity on the upper wafer. Under acceleration, the Si / SiO2 mass causes deformation of the two-dimensional sensitive thin film. This deformation converts the acceleration signal into resonant frequency shifts or resistance changes. The cavity and via cavity allow the Si / SiO2 mass to move along a direction perpendicular to the plane of the silicon support frame when subjected to acceleration. The fabrication method includes the following steps: (1) Thermal oxidation to fabricate the first Si substrate A silicon wafer is subjected to thermal oxidation; the thickness of the silicon wafer is 1. ~500 This allows a layer of SiO2 to grow on the upper and lower surfaces of the wafer; (2) SiO2 etching Based on step (1), photoresist is coated onto the wafer and exposed and developed, and the SiO2 layer is etched using reactive ion beam technology; (3) Electrode preparation Based on step (2), electrodes are fabricated using evaporation and sputtering metal deposition processes. After electrode deposition, residual photoresist is removed using a metal stripping process. (4) Back etching Based on step (3), a layer of photoresist is coated on the back of the wafer, and exposure and development are performed to determine the position of the cavity. The back SiO2 layer is etched using the RIE process, and the Si layer is etched using the DRIE process. When the surface SiO2 is reached, the etching is stopped. At this time, the cavity has been initially formed, and the position of the SiO2 / Si mass block is defined. The characteristics of the RIE and DRIE processes ensure the perpendicularity of the etched cavity, which is beneficial to reducing the size of the chip. The shape of the mass block includes cube, cuboid, cylinder, and hexagon. The side length of the mass block includes the range from nanometer to millimeter. The height of the mass block includes the range from nanometer to millimeter. The number of mass blocks is at least one. The levitation method of the mass block includes the levitation of a single mass block and the levitation of an array of mass blocks. (5) Thermal oxidation to fabricate a second Si substrate Another silicon wafer was subjected to thermal oxidation; the thickness of the silicon wafer was 1. ~500 This allows a layer of SiO2 to grow on the upper and lower surfaces of the wafer. (6) Etching the Si / SiO2 substrate to form through-hole cavities Based on step (5), the second silicon wafer is coated with photoresist and exposed and developed. According to the position of the cavity formed in step (4), the position of the through-hole cavity of the wafer is determined, and the SiO2 layer and Si layer are etched by RIE process and DRIE process respectively. (7) Bonding of two processed silicon substrates The structures formed in steps (4) and (6) are wafer bonded; the bonding methods include direct wafer bonding, anodic wafer bonding, adhesive wafer bonding, glass frit wafer bonding, eutectic wafer bonding, transient liquid phase wafer bonding, and metal hot pressing wafer bonding; (8) Transfer of two-dimensional sensitive thin film Based on step (7), the two-dimensional sensitive film is transferred to the surface of the structure formed in step (7) using a two-dimensional sensitive film transfer method; Two-dimensional sensitive films can be transferred using methods such as transfer with polymethyl methacrylate (PMMA) as a support layer and transfer without a support layer; electrostatic transfer; chemical reaction transfer; non-electrochemical bubbling-assisted transfer; heat-release tape; polydimethylsiloxane imprinting; dry transfer; and metal-assisted peeling. The materials used in the two-dimensional sensitive films include graphene, molybdenum disulfide (MoS2), tungsten disulfide (WS2), molybdenum diselenide (MoSe2), tungsten diselenide (WSe2), platinum diselenide (PtSe2), molybdenum distelluride (MoTe2), tungsten distelluride (WTe2), vanadium diselenide (VSe2), chromium disulfide (CrS2), chromium diselenide (CrSe2), other transition metal sulfides (TMDC), black phosphorus (P), MXene, hexagonal boron nitride (h-BN), and suspended two-dimensional material heterolayers. The suspended two-dimensional material heterolayer includes hexagonal boron nitride / graphene, hexagonal boron nitride / molybdenum disulfide, hexagonal boron nitride / tungsten diselenide, hexagonal boron nitride / molybdenum diselenide, hexagonal boron nitride / tungsten disulfide, boron hexadecimal nitride / platinum diselenide, hexagonal boron nitride / molybdenum ditelluride, hexagonal boron nitride / tungsten ditelluride, hexagonal boron nitride / vanadium diselenide, hexagonal boron nitride / chromium disulfide, hexagonal boron nitride / chromium diselenide, hexagonal boron nitride / TMDC, graphene / molybdenum disulfide, graphene / tungsten diselenide, graphene / molybdenum diselenide, graphene / tungsten disulfide, graphene / platinum diselenide, graphene / molybdenum ditelluride, graphene / tungsten ditelluride, graphene / ... Vanadium selenide, graphene / chromium disulfide, graphene / chromium diselenide, graphene / TMDC, hexagonal boron nitride / graphene / molybdenum disulfide, hexagonal boron nitride / graphene / tungsten diselenide, hexagonal boron nitride / graphene / molybdenum diselenide, hexagonal boron nitride / graphene / tungsten disulfide, hexagonal boron nitride / graphene / platinum diselenide, hexagonal boron nitride / graphene / molybdenum distelluride, hexagonal boron nitride / graphene / tungsten distelluride, hexagonal boron nitride / graphene / vanadium diselenide, hexagonal boron nitride / graphene / chromium disulfide, hexagonal boron nitride / graphene / chromium diselenide, hexagonal boron nitride / graphene / TMDC, MXene / graphene, MXene / Hexagonal boron nitride, MXene / molybdenum disulfide, MXene / tungsten disulfide, MXene / molybdenum diselenide, MXene / tungsten diselenide, MXene / platinum diselenide, MXene / molybdenum ditelluride, MXene / tungsten ditelluride, MXene / vanadium diselenide, MXene / chromium disulfide, MXene / chromium diselenide, MXene / TMDC; The two-dimensional sensitive film includes any two or more stacks of two-dimensional films among graphene, molybdenum disulfide, tungsten disulfide, molybdenum diselenide, tungsten diselenide, platinum diselenide, molybdenum distelluride, tungsten distelluride, vanadium diselenide, chromium disulfide, chromium diselenide, other transition metal sulfides (TMDC), black phosphorus, MXene, and hexagonal boron nitride. The two-dimensional sensitive film also includes its composite with other types of nanofilms, including composites of metals, metal oxides, organic polymers, polymethyl methacrylate, polycarbonate and silicon nitride with two-dimensional materials and heterolayers; The thickness of the two-dimensional sensitive film is one of the following: a single atomic layer, two atomic layers, three atomic layers, four atomic layers, five atomic layers, six atomic layers, seven atomic layers, eight atomic layers, nine atomic layers, and ten atomic layers. (9) Patterned etching of two-dimensional thin films Based on step (8), the transferred two-dimensional thin film is patterned using traditional photolithography, laser etching, or focused ion beam etching processes. The shape of the two-dimensional sensitive thin film includes a film that fully covers the cavity and the Si / SiO2 mass block, a strip that partially covers the cavity and the Si / SiO2 mass block, and a cantilever beam that partially covers the cavity and the Si / SiO2 mass block. The width of the two-dimensional thin film is greater than the total width of the mass block and the trench, or less than or equal to the width of the mass block. (10) Etch the sacrificial layer to release the mass block. The SiO2 on the top layer of the cavity surrounding the Si / SiO2 mass block was etched using a gas-phase hydrofluoric acid process, thereby achieving self-levitation of the two-dimensional thin film and finally obtaining a two-dimensional thin film suspended Si / SiO2 mass block sensitive structure.
Citation Information
Patent Citations
Acceleration sensor based on suspension two-dimensional material and heterogeneous layer suspension mass block
CN111983257A