Modified siO2, and preparation method and application thereof
By immobilizing condensed tannins on SiO2 and adjusting the adhesion with m-cresol-6-sulfonate ammonium, a PA6/SiO2 composite powder with good thermal stability was prepared, which solved the problem of insufficient thermal stability of modified SiO2 and realized the efficient preparation of composite powder and environmentally friendly resource utilization.
Patent Information
- Application Number
- CN202311847192.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-29
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-12-29
AI Technical Summary
In the existing technology, the thermal stability of modified SiO2 is insufficient, resulting in poor thermal stability of the composite powder. Furthermore, when physical modification is performed using condensed tannins alone, the condensed tannins are prone to detachment, affecting the stability of the composite powder.
Condensed tannins adsorbed on SiO2 were fixed with tannic acid and combined with m-cresol-6-sulfonate ammonium to prepare modified SiO2 by dissolution and precipitation method. The adhesion of tannic acid was controlled to promote the uniform precipitation of PA6 macromolecular chains with SiO2, forming PA6/SiO2 composite powder with good thermal stability.
It improves the thermal and dimensional stability of the composite powder, avoids complex chemical reactions, increases preparation efficiency, and effectively solves the environmental pollution problem caused by PA6 waste fabrics.
Smart Images

Figure CN117820727B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of waste textile recycling technology, and relates to a modified SiO2, its preparation method and application. Background Technology
[0002] PA6 (Nylon 6) is a polymer formed by the ring-opening polymerization of ε-caprolactam. It has been widely used in many fields and has become one of the most widely used synthetic fibers in the textile industry. It has good abrasion resistance and is an important raw material for manufacturing textiles such as fishing nets and stockings. However, its good physical properties make it difficult to degrade after disposal. Therefore, a suitable recycling method is extremely important. One feasible method is to make PA6 into composite powder.
[0003] Dissolution-precipitation is a common method for preparing composite powders. Reference 1, "A nanosilica / nylon-12 composite powder for selective laser sintering[J]. Journal of Reinforced Plastics and Composites, 2009, 28(23):2889-2902," describes a method that modifies SiO2 with a silane coupling agent. Using the modified SiO2 as the core and a mixed solvent of ethanol / butanone / water, PA12 (nylon 12) is completely dissolved. The PA12 is then precipitated on the SiO2 surface by cooling. The silane coupling agent-modified SiO2 contains amino groups, which can undergo amidation with the carboxyl groups of the PA12 macromolecular chain during precipitation, promoting PA12 precipitation on SiO2 and enhancing the interaction between the PA12 macromolecular chain and SiO2. The resulting composite powder exhibits good dimensional stability, but its thermal stability is poor.
[0004] Reference 2, "Microcrystalline cellulose modified by phytic acid and condensed tannins exhibits excellent flame retardant and cationic dye adsorption properties[J]. Industrial Crops and Products, 2022, 184: 115035," describes a method for modifying microcrystalline cellulose with phytic acid and condensed tannins. Through esterification, condensed tannins and microcrystalline cellulose are linked by phytic acid. The phosphorus in phytic acid imparts a flame-retardant effect. However, if only condensed tannins are used, the thermal decomposition temperature of the condensed tannin-treated microcrystalline cellulose is almost the same as that of the untreated microcrystalline cellulose. At the same decomposition temperature, the condensed tannin-treated microcrystalline cellulose has a greater residual mass, thus exhibiting better thermal stability compared to the untreated microcrystalline cellulose. Therefore, condensed tannins can enhance thermal stability.
[0005] Therefore, modifying SiO2 with condensed tannins is expected to improve the thermal stability of SiO2, and thus improve the thermal stability of the composite powder. However, experiments show that if SiO2 is modified by physical modification with condensed tannins without chemical grafting, the condensed tannins are easy to fall off. Summary of the Invention
[0006] The purpose of this invention is to solve the above-mentioned problems existing in the prior art, and to provide a modified SiO2, its preparation method and application. Modified SiO2 is obtained by immobilizing condensed tannins adsorbed on SiO2 with tannic acid. Composite powder is prepared using PA6 and modified SiO2 as the main raw materials. In this process, m-cresol-6-sulfonate ammonium is used to reduce the aggregation caused by tannic acid in modified SiO2, so that the interaction force between PA6 macromolecular chains and SiO2 is maintained at an appropriate level.
[0007] To achieve the above objectives, the technical solution adopted by the present invention is as follows:
[0008] A method for preparing modified SiO2 involves first impregnating nano-SiO2 in a condensed tannin dispersion, followed by post-treatment (centrifugation at 5000-6000 rpm for 20 min, and drying at 60°C for 24 h) to obtain nano-SiO2 adsorbed with condensed tannins. Then, the nano-SiO2 adsorbed with condensed tannins and tannic acid are mixed in a solvent and post-treated (washed 5 times with deionized water, and then dried at 60°C for 24 h) to obtain modified SiO2.
[0009] Tannic acid is a type of hydrolyzed tannin. The phenolic hydroxyl groups in tannic acid give it good adhesion, which can coat the condensed tannins adsorbed on nano-SiO2 and prevent them from falling off.
[0010] As a preferred technical solution:
[0011] In the modified SiO2 preparation method described above, the condensed tannin in the condensed tannin dispersion is condensed tannin that has been ball-milled for 24 to 36 hours.
[0012] In the modified SiO2 preparation method described above, the concentration of the condensed tannin dispersion is 15-22 wt%; the mass ratio of nano-SiO2 to the condensed tannin dispersion is 1:13.3-19; and the nano-SiO2 is impregnated in the condensed tannin dispersion at a temperature of 80-90°C for 2-3 hours.
[0013] The specific process of preparing modified SiO2 as described above, which involves mixing nano-SiO2 with adsorbed condensed tannins and tannic acid in a solvent, is as follows: After dispersing nano-SiO2 with adsorbed condensed tannins in water to obtain a dispersion, tannic acid solution is added dropwise to the dispersion.
[0014] The modified SiO2 preparation method described above involves a dispersion temperature of 60–65°C, a dispersion time of 1–1.5 min, and a dispersion speed of 1400–1300 rpm.
[0015] In the modified SiO2 preparation method described above, the mass fraction of nano-SiO2 with adsorbed condensed tannins in the dispersion is 0.2–0.5 wt%.
[0016] In the modified SiO2 preparation method described above, the mass ratio of tannic acid to nano-SiO2 with adsorbed condensed tannins is 1:17-25.
[0017] The present invention also provides a modified SiO2 prepared by the above-mentioned method, wherein the modified SiO2 contains 40-50 wt% condensed tannins and 0.06-0.07 wt% tannic acid, and the thermogravimetric residue after 5 washes is 81-83 wt%, indicating that the condensed tannins in the modified SiO2 are not easily removed.
[0018] This invention also provides a method for preparing PA6 / SiO2 composite powder with good thermal stability. The method involves mixing modified SiO2, PA6, solvent, and ammonium m-cresol-6-sulfonate as described above, and then preparing the PA6 / SiO2 composite powder with good thermal stability via a dissolution-precipitation method. In the mixture of modified SiO2, PA6, solvent, and ammonium m-cresol-6-sulfonate, the content of ammonium m-cresol-6-sulfonate is 0.2–0.4 wt%, the content of modified SiO2 is 0.2–0.4 wt%, and the mass ratio of PA6 to modified SiO2 is 12–10:1.
[0019] During the dissolution and precipitation process of PA6, under high temperature and pressure conditions, the macromolecular chains of PA6 are in a relatively free state. However, as the temperature decreases, the solubility of the solvent decreases, and the macromolecular chains of PA6 will collide and aggregate. If a solid insoluble in the solvent is used in this process, it can play a role in heterogeneous nucleation. In this invention, modified SiO2 is used as the nucleus. During the precipitation process, the macromolecular chains of PA6 will aggregate on the surface of modified SiO2. The tannic acid covering the modified SiO2 has phenolic hydroxyl groups and adhesiveness, which can attract the macromolecular chains of PA6 and promote the aggregation of PA6 macromolecular chains on the modified SiO2. However, if the adhesiveness of tannic acid is too high, it will also cause the modified SiO2 to aggregate, which is not conducive to nucleation during the dissolution and precipitation process, resulting in uneven particle size distribution. At the same time, the attracted PA6 macromolecular chains will also become violently entangled, resulting in uneven precipitation. Therefore, it is necessary to reduce the adhesiveness of tannic acid to a suitable level.
[0020] m-Cresol-6-sulfonate ammonium is an aromatic compound whose benzene ring can undergo π-π stacking with the benzene ring of tannic acid. Its sulfonic acid group can form hydrogen bonds with the hydroxyl group of tannic acid. Furthermore, after tannic acid ionizes hydrogen ions in water, m-Cresol-6-sulfonate ammonium ionizes and can combine with hydrogen ions, further increasing the ionization of tannic acid and altering its structure. The synergistic effect of these three factors can reduce the adhesiveness of tannic acid. Even after the adhesiveness is reduced, tannic acid will still retain a certain number of hydroxyl groups, which can combine with PA6 macromolecular chains to form hydrogen bonds during precipitation, thereby promoting the aggregation of PA6 macromolecular chains.
[0021] The addition of m-cresol-6-sulfonate ammonium in this invention is controlled at 0.2-0.4 wt% to maintain the adhesiveness of tannic acid within a suitable range. If the addition amount is too high, the impact on the tannic acid structure will increase, greatly weakening the strong hydrogen bonding of tannic acid. This will affect the aggregation of PA6 on modified SiO2 during precipitation, causing the PA6 macromolecular chains to self-aggregate and form particles, resulting in changes in average particle size and an increase in PDI. If the addition amount is too low, the impact on the adhesiveness of tannic acid will be relatively small. During the dissolution and precipitation process, tannic acid will attract a large number of PA6 macromolecular chains and SiO2 that also covers tannic acid, leading to uneven molding, an increase in average particle size, and an increase in PDI.
[0022] As a preferred technical solution:
[0023] The method for preparing PA6 / SiO2 composite powder with good thermal stability as described above involves a mixture of modified SiO2, PA6, solvent, and m-cresol-6-sulfonate. The mass ratio of solvent to PA6 is 7-8:1. Under this ratio, the macromolecular chains of dissolved PA6 are more freely distributed in the solvent, resulting in more uniform precipitation.
[0024] The method for preparing PA6 / SiO2 composite powder with good thermal stability as described above uses a mixture of diethylene glycol and water in a volume ratio of 2:1 as the solvent. This solvent has the characteristic of not dissolving PA6 at room temperature but dissolving PA6 at high temperature.
[0025] The preparation method of PA6 / SiO2 composite powder with good thermal stability as described above, specifically the process of preparing PA6 / SiO2 composite powder with good thermal stability by dissolution precipitation method, is as follows: a mixture of modified SiO2, PA6, solvent, and m-cresol-6-sulfonate ammonium is heated to 155-165℃ and held for 1-2 hours, then cooled to below 40℃ at a cooling rate of 0.2-1℃ / min to obtain PA6 / SiO2 composite powder with good thermal stability. The dissolution temperature and holding time are set in this way to ensure that PA6 is completely dissolved. If the dissolution temperature and dissolution time are too low, PA6 cannot be completely dissolved, and if the dissolution temperature and dissolution time are too high, it will cause some breakage of PA macromolecular chains.
[0026] The method for preparing PA6 / SiO2 composite powder with good thermal stability as described above involves washing and drying PA6 before dissolving it. The washing process is as follows: PA6 is immersed in a soaping solution with a bath ratio of 1:30 to 50 and a soaping solution concentration of 2 g / L. The PA6 is then soaked and washed at 25 to 35°C for 1 hour. The drying process involves drying at 25 to 35°C for 12 to 24 hours.
[0027] The method for preparing PA6 / SiO2 composite powder with good thermal stability as described above has a yield of 70-75% for PA6 / SiO2 composite powder with good thermal stability. The yield is calculated as: (mass of PA6 / SiO2 composite powder with good thermal stability after drying) / (mass of PA6 added + mass of modified SiO2 added) × 100%. The average particle size of the PA6 / SiO2 composite powder with good thermal stability is 30-50 μm, the PDI is 0.1-0.2, and the thermogravimetric residue is 69-73%. Therefore, it can be seen that the present invention improves the thermal stability of the composite powder by introducing condensed tannins into modified SiO2.
[0028] Beneficial effects:
[0029] (1) The present invention provides a method for preparing PA6 / SiO2 composite powder with good thermal stability. The composite powder prepared by the dissolution and precipitation method has good dimensional stability and good thermal stability, and avoids complex chemical reactions during the preparation process, resulting in high preparation efficiency.
[0030] (2) The tannic acid used in this invention has the characteristic of having multiple hydroxyl groups. SiO2 modified with tannic acid will aggregate due to mutual attraction between molecules. In order to prevent PA6 from precipitating as uniformly as possible and to maintain good dispersibility during the precipitation process, m-cresol-6-sulfonate ammonium is used to reduce the excessively strong intermolecular forces caused by tannic acid and to enhance the interaction between PA6 macromolecular chains and modified SiO2. The addition of m-cresol-6-sulfonate ammonium can shield and cover the phenolic hydroxyl groups of tannic acid, and it forms hydrogen bonds with PA6 macromolecular chains, weakening the forces between PA6 macromolecular chains and thus stabilizing them. This allows PA6 macromolecular chains to precipitate uniformly during the precipitation process to form a regular shape.
[0031] (3) The present invention can use PA6 waste yarn to prepare PA6 / SiO2 composite powder with good thermal stability, which effectively solves the problem of solid waste accumulation and pollution caused by PA6 waste fabric, and is conducive to environmental protection and resource utilization. Attached Figure Description
[0032] Figure 1 The image shows a comparison of the TG values of PA6 / SiO2 composite powder with good thermal stability prepared in Example 6 and PA6 after soaping.
[0033] Figure 2 The image shows a scanning electron microscope (SEM) image of the PA6 / SiO2 composite powder with good thermal stability prepared in Example 6. Detailed Implementation
[0034] The present invention will be further described below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Furthermore, it should be understood that after reading the teachings of this invention, those skilled in the art can make various alterations or modifications to the invention, and these equivalent forms also fall within the scope defined by the appended claims.
[0035] Unless otherwise specified, the experimental methods described in the following examples are conventional methods; unless otherwise specified, the reagents and materials are commercially available.
[0036] The testing / calculation methods for the relevant performance indicators in the following embodiments and comparative examples are as follows:
[0037] Thermogravimetric analysis: PA6 and the composite powder after soaping were thermally analyzed using a Diamond TG / DTG 5700 thermal analyzer (TA Instruments, USA). A nitrogen atmosphere was used for the composite powder testing. The composite powder weight was 5 mg, the heating rate was 20 °C / min, and the temperature range was 30-700 °C.
[0038] PDI: Accurately weigh 0.1g of PA6 / SiO2 composite powder with good thermal stability, disperse the composite powder in 50mL of deionized water, dilute until transparent, and equilibrate for 10s on a Nano-ZS90 nanoparticle size analyzer at 25℃ to obtain the PDI of the composite powder.
[0039] Average particle size: The average particle size was obtained by selecting 200 particles using Nano Measure 1.2 software based on the scanning electron microscope image with a scale bar.
[0040] Yield: Yield = mass of PA6 / SiO2 composite powder with good thermal stability after drying / (mass of PA6 added + mass of modified SiO2 added) × 100%.
[0041] Molecular weight determination: The molecular weight of different PA6 raw materials was determined by the viscosity method. The viscosity was determined using an Ubbelohde viscometer with a capillary inner diameter of 0.6 mm. An 85% formic acid aqueous solution was used as the solvent. The concentration of the formic acid solution for PA6 raw materials was 10 mg / mL. The test temperature was 25 ± 0.1℃.
[0042] Example 1
[0043] A method for preparing modified SiO2, the specific steps of which are as follows:
[0044] (1) First, condensed tannin (manufacturer: Shanghai Jizhi Biochemical Technology Co., Ltd., CAS: 4852-22-6) was ball-milled for 24 hours and then mixed with water to prepare a condensed tannin dispersion with a concentration of 15wt%. Then, nano-SiO2 was immersed in the condensed tannin dispersion at 80℃ for 2 hours, followed by centrifugation at 5000rpm for 20 minutes, and finally dried at 60℃ for 24 hours to obtain nano-SiO2 adsorbed with condensed tannin; wherein, the mass ratio of nano-SiO2 to condensed tannin dispersion was 1:13.3.
[0045] (2) After dispersing the nano-SiO2 adsorbed with condensed tannins in water at 60℃ and 1400rpm for 1min to obtain a dispersion, tannic acid was added to the dispersion; wherein, the mass ratio of tannic acid to nano-SiO2 adsorbed with condensed tannins was 1:25, and the mass fraction of nano-SiO2 adsorbed with condensed tannins in the dispersion was 0.2wt%.
[0046] (3) The product from step (2) is washed five times with deionized water and then dried at 60°C for 24 hours to obtain modified SiO2.
[0047] The final modified SiO2 contained 40 wt% condensed tannins and 0.058 wt% tannic acid. After five washes, the thermogravimetric residue was 81 wt%.
[0048] Comparative Example 1
[0049] A method for preparing modified SiO2 is basically the same as in Example 1, except that tannic acid is not added to the dispersion in step (2).
[0050] The final modified SiO2 contained 10 wt% condensed tannins, and the thermogravimetric residue after five washes was 11 wt%.
[0051] Comparing Example 1 and Comparative Example 1, it can be seen that since tannic acid is not used in Comparative Example 1, the condensed tannins cannot be firmly bonded to nano-SiO2. This is because condensed tannins are non-water-soluble and are in a solid state in water. They do not chemically react or physically bond with SiO2. Therefore, without the use of tannic acid, SiO2 cannot bond with condensed tannins, thus reducing thermal stability.
[0052] Example 2
[0053] A method for preparing modified SiO2, the specific steps of which are as follows:
[0054] (1) First, condensed tannin (manufacturer: Shanghai Jizhi Biochemical Technology Co., Ltd., CAS: 4852-22-6) was ball-milled for 28 hours and then mixed with water to prepare a condensed tannin dispersion with a concentration of 18wt%. Then, nano-SiO2 was immersed in the condensed tannin dispersion at 85℃ for 3 hours, followed by centrifugation at 5200rpm for 20 minutes, and finally dried at 60℃ for 24 hours to obtain nano-SiO2 adsorbed with condensed tannin; wherein, the mass ratio of nano-SiO2 to condensed tannin dispersion was 1:15.
[0055] (2) After dispersing the nano-SiO2 adsorbed with condensed tannins in water for 1.1 min at 61℃ and 1375 rpm to obtain a dispersion, tannic acid was added to the dispersion; wherein, the mass ratio of tannic acid to nano-SiO2 adsorbed with condensed tannins was 1:20, and the mass fraction of nano-SiO2 adsorbed with condensed tannins in the dispersion was 0.2 wt%.
[0056] (3) The product from step (2) is washed five times with deionized water and then dried at 60°C for 24 hours to obtain modified SiO2.
[0057] The final modified SiO2 contained 44 wt% condensed tannins and 0.061 wt% tannic acid. After five washes, the thermogravimetric residue was 82 wt%.
[0058] Example 3
[0059] A method for preparing modified SiO2, the specific steps of which are as follows:
[0060] (1) First, condensed tannin (manufacturer: Shanghai Jizhi Biochemical Technology Co., Ltd., CAS: 4852-22-6) was ball-milled for 30 h and then mixed with water to prepare a condensed tannin dispersion with a concentration of 20 wt%. Then, nano-SiO2 was immersed in the condensed tannin dispersion at 90 °C for 2.25 h, followed by centrifugation at 5500 rpm for 20 min, and finally dried at 60 °C for 24 h to obtain nano-SiO2 adsorbed with condensed tannin; wherein, the mass ratio of nano-SiO2 to condensed tannin dispersion was 1:17.
[0061] (2) After dispersing the nano-SiO2 adsorbed with condensed tannins in water for 1.2 min at 62℃ and 1350 rpm to obtain a dispersion, tannic acid was added to the dispersion; wherein, the mass ratio of tannic acid to nano-SiO2 adsorbed with condensed tannins was 1:21, and the mass fraction of nano-SiO2 adsorbed with condensed tannins in the dispersion was 0.3 wt%.
[0062] (3) The product from step (2) is washed five times with deionized water and then dried at 60°C for 24 hours to obtain modified SiO2.
[0063] The final modified SiO2 contained 45 wt% condensed tannins and 0.062 wt% tannic acid. After five washes, the thermogravimetric residue was 82 wt%.
[0064] Example 4
[0065] A method for preparing modified SiO2, the specific steps of which are as follows:
[0066] (1) First, condensed tannin (manufacturer: Shanghai Jizhi Biochemical Technology Co., Ltd., CAS: 4852-22-6) was ball-milled for 36 hours and then mixed with water to prepare a condensed tannin dispersion with a concentration of 22wt%. Then, nano-SiO2 was immersed in the condensed tannin dispersion at 85°C for 2.5 hours, followed by centrifugation at 5800 rpm for 20 minutes, and finally dried at 60°C for 24 hours to obtain nano-SiO2 adsorbed with condensed tannin. The mass ratio of nano-SiO2 to condensed tannin dispersion was 1:19.
[0067] (2) After dispersing the nano-SiO2 adsorbed with condensed tannins in water for 1.5 min at 63℃ and 1325 rpm to obtain a dispersion, tannic acid was added to the dispersion; wherein, the mass ratio of tannic acid to nano-SiO2 adsorbed with condensed tannins was 1:17, and the mass fraction of nano-SiO2 adsorbed with condensed tannins in the dispersion was 0.5 wt%.
[0068] (3) The product from step (2) is washed five times with deionized water and then dried at 60°C for 24 hours to obtain modified SiO2.
[0069] The final modified SiO2 contained 45.5 wt% condensed tannins and 0.063 wt% tannic acid. After five washes, the thermogravimetric residue was 82.3 wt%.
[0070] Example 5
[0071] A method for preparing modified SiO2, the specific steps of which are as follows:
[0072] (1) First, condensed tannin (manufacturer: Shanghai Jizhi Biochemical Technology Co., Ltd., CAS: 4852-22-6) was ball-milled for 36 hours and then mixed with water to prepare a condensed tannin dispersion with a concentration of 22wt%. Then, nano-SiO2 was immersed in the condensed tannin dispersion at 90℃ for 3 hours, followed by centrifugation at 6000rpm for 20 minutes, and finally dried at 60℃ for 24 hours to obtain nano-SiO2 adsorbed with condensed tannin; wherein, the mass ratio of nano-SiO2 to condensed tannin dispersion was 1:19.
[0073] (2) After dispersing the nano-SiO2 adsorbed with condensed tannins in water for 1.5 min at 65℃ and 1300 rpm to obtain a dispersion, tannic acid was added to the dispersion; wherein, the mass ratio of tannic acid to nano-SiO2 adsorbed with condensed tannins was 1:17, and the mass fraction of nano-SiO2 adsorbed with condensed tannins in the dispersion was 0.2 wt%.
[0074] (3) The product from step (2) is washed five times with deionized water and then dried at 60°C for 24 hours to obtain modified SiO2.
[0075] The final modified SiO2 contained 50 wt% condensed tannins and 0.065 wt% tannic acid. After five washes, the thermogravimetric residue was 83 wt%.
[0076] Example 6
[0077] A method for preparing PA6 / SiO2 composite powder with good thermal stability, the specific steps of which are as follows:
[0078] (1) At a temperature of 25°C, PA6 (colorless waste PA6 filaments, Wujiang Fuhua Textile Co., Ltd., Suzhou City, Jiangsu Province, with a molecular weight of 18000 g / mol) was immersed in a soaping solution with a concentration of 2 g / L at a bath ratio of 1:50. After washing for 1 h, it was dried at 25°C for 24 h to obtain the product PA6.
[0079] (2) The modified SiO2 of Example 1, the product PA6 of step (1), the solvent (a mixture of diethylene glycol and water in a volume ratio of 2:1), and m-cresol-6-sulfonate ammonium were mixed. In the mixture of modified SiO2, PA6, solvent, and m-cresol-6-sulfonate ammonium, the content of m-cresol-6-sulfonate ammonium was 0.2wt%, the content of modified SiO2 was 0.2wt%, and the mass ratio of PA6 to modified SiO2 was 10:1.
[0080] (3) The mixture of modified SiO2, PA6 (the product of step (1)), solvent and m-cresol-6-sulfonate ammonium is heated to 165°C and held for 2 hours, and then cooled to 35°C at a cooling rate of 1°C / min to obtain PA6 / SiO2 composite powder with good thermal stability.
[0081] The final obtained PA6 / SiO2 composite powder has good thermal stability (e.g. Figure 2 The yield of the PA6 / SiO2 composite powder (shown) was 70%, exhibiting good thermal stability with an average particle size of 50 μm and a PDI of 0.2. Figure 1As shown, the thermogravimetric residue of PA6 / SiO2 composite powder with good thermal stability is 69%, while the thermogravimetric residue of PA6 after soaping in step (1) is 0.3%, which fully demonstrates that the thermal stability of the composite powder is improved compared with the original sample.
[0082] Comparative Example 2
[0083] A method for preparing modified SiO2 is basically the same as in Example 6, except that in step (2), the content of m-cresol-6-sulfonate ammonium in the mixture of modified SiO2, PA6, solvent, and m-cresol-6-sulfonate ammonium is 0.1 wt%.
[0084] The yield of the final PA6 / SiO2 composite powder with good thermal stability was 70%. The average particle size of the PA6 / SiO2 composite powder with good thermal stability was 71 μm, the PDI was 0.34, and the thermogravimetric residue of the PA6 / SiO2 composite powder with good thermal stability was 68.4%.
[0085] Comparing Example 6 and Comparative Example 2, it can be seen that the low content of ammonium cresol-6-sulfonate in Comparative Example 2 leads to irregular shape of the obtained PA6 / SiO2 composite powder with good thermal stability, and an increase in average particle size and PDI. This is because the low content of ammonium cresol-6-sulfonate results in poor adhesion to tannic acid. During the dissolution and precipitation process, tannic acid attracts a large number of PA6 macromolecular chains and SiO2 that also covers tannic acid, resulting in uneven molding, increased average particle size, and increased PDI.
[0086] Comparative Example 3
[0087] A method for preparing modified SiO2 is basically the same as in Example 6, except that in step (2), the content of m-cresol-6-sulfonate ammonium in the mixture of modified SiO2, PA6, solvent, and m-cresol-6-sulfonate ammonium is 0.5 wt%.
[0088] The yield of the final PA6 / SiO2 composite powder with good thermal stability was 70%. The average particle size of the PA6 / SiO2 composite powder with good thermal stability was 46 μm, the PDI was 0.32, and the thermogravimetric residue of the PA6 / SiO2 composite powder with good thermal stability was 69.2%.
[0089] Comparing Example 6 and Comparative Example 3, it can be seen that the excessively high content of ammonium m-cresol-6-sulfonate in Comparative Example 3 leads to a decrease in the average particle size and an increase in PDI of the obtained PA6 / SiO2 composite powder with good thermal stability. This is because as the content of ammonium m-cresol-6-sulfonate increases, its influence on the tannic acid structure also increases, which greatly weakens the strong hydrogen bonding of tannic acid. During the precipitation process, it affects the aggregation of PA6 in modified SiO2, causing the PA6 macromolecular chains to self-aggregate and form particles, resulting in a change in average particle size and an increase in PDI.
[0090] Comparative Example 4
[0091] A method for preparing modified SiO2 is basically the same as in Example 6, except that in step (2), the content of modified SiO2 in the mixture of modified SiO2, PA6, solvent, and m-cresol-6-sulfonate is 0.1 wt%.
[0092] The yield of the final PA6 / SiO2 composite powder with good thermal stability was 70%. The average particle size of the PA6 / SiO2 composite powder with good thermal stability was 75 μm, the PDI was 0.29, and the thermogravimetric residue of the PA6 / SiO2 composite powder with good thermal stability was 69%.
[0093] Comparing Example 6 and Comparative Example 4, it can be seen that the low content of modified SiO2 in Comparative Example 4 leads to an increase in average particle size and PDI. This is because when the content of modified SiO2 decreases, the number of PA6 macromolecular chains aggregated on the surface of modified SiO2 increases. The outermost PA6 macromolecular chains are prone to entanglement with the PA6 macromolecular chains on the nearby modified SiO2 surface, causing particle aggregation, thereby increasing the particle size and PDI.
[0094] Comparative Example 5
[0095] A method for preparing modified SiO2 is basically the same as in Example 6, except that in step (2), the content of modified SiO2 in the mixture of modified SiO2, PA6, solvent, and m-cresol-6-sulfonate is 0.5 wt%.
[0096] The yield of the final PA6 / SiO2 composite powder with good thermal stability was 70%. The average particle size of the PA6 / SiO2 composite powder with good thermal stability was 45 μm, the PDI was 0.26, and the thermogravimetric residue of the PA6 / SiO2 composite powder with good thermal stability was 69.3%.
[0097] Comparing Example 6 and Comparative Example 5, it can be seen that the excessively high content of modified SiO2 in Comparative Example 5 leads to a decrease in average particle size and an increase in PDI. This is because during the dissolution and precipitation process, PA6 macromolecular chains need to aggregate on the surface of modified SiO2. A suitable ratio can ensure that the surface of modified SiO2 is completely covered by PA6 macromolecular chains. However, if there is too much modified SiO2, the number of nuclei for PA6 macromolecular chains to precipitate in the solvent will increase, resulting in vacancies in the PA6 macromolecular chains that were originally able to cover the surface of modified SiO2. This leads to an uneven distribution of PA6 macromolecular chains on the surface of modified SiO2. Finally, the particle size of the composite powder formed by precipitation decreases, but the morphology becomes more uneven, resulting in an increase in PDI.
[0098] Comparative Example 6
[0099] A method for preparing modified SiO2 is basically the same as in Example 6, except that in step (2), the mass ratio of PA6 to modified SiO2 in the mixture of modified SiO2, PA6, solvent, and m-cresol-6-sulfonate is 9:1.
[0100] The yield of the final PA6 / SiO2 composite powder with good thermal stability was 50%. The average particle size of the PA6 / SiO2 composite powder with good thermal stability was 28 μm, the PDI was 0.19, and the thermogravimetric residue of the PA6 / SiO2 composite powder with good thermal stability was 68%.
[0101] Comparing Example 6 and Comparative Example 6, it can be seen that the lower PA6 content in Comparative Example 6 leads to a decrease in the yield and average particle size of the obtained PA6 / SiO2 composite powder with good thermal stability. This is because when the PA6 content in the system decreases, the degradation of PA6 by the solvent becomes more pronounced, causing some PA6 to transform into small molecules, resulting in a decrease in the PA6 content. Consequently, the number of PA6 macromolecular chains on the modified SiO2 decreases, leading to uneven coating, a decrease in average particle size, and an increase in PDI, thus affecting the yield of the composite powder.
[0102] Comparative Example 7
[0103] A method for preparing modified SiO2 is basically the same as in Example 6, except that in step (2), the mass ratio of PA6 to modified SiO2 in the mixture of modified SiO2, PA6, solvent, and m-cresol-6-sulfonate is 13:1.
[0104] The yield of the final PA6 / SiO2 composite powder with good thermal stability was 70%. The average particle size of the PA6 / SiO2 composite powder with good thermal stability was 72 μm, the PDI was 0.32, and the thermogravimetric residue of the PA6 / SiO2 composite powder with good thermal stability was 69%.
[0105] Comparing Example 6 and Comparative Example 7, it can be seen that the higher content of PA6 in Comparative Example 7 leads to an increase in the average particle size and PDI of the PA6 / SiO2 composite powder with good thermal stability. This is because the increased mass of PA6 in the mixed solvent reduces the degree of freedom of PA6 in the dissolving solvent, making it easier for PA6 macromolecular chains to become violently entangled during precipitation, resulting in the formation of irregular aggregates by coating different numbers of modified SiO2.
[0106] Example 7
[0107] A method for preparing PA6 / SiO2 composite powder with good thermal stability, the specific steps of which are as follows:
[0108] (1) At a temperature of 28℃, PA6 (colorless waste PA6 filaments, Jiangsu Haiyang Chemical Fiber Co., Ltd., with a molecular weight of 18000g / mol) was immersed in a soaping solution with a concentration of 2g / L at a bath ratio of 1:30. After washing for 1h, it was dried at 28℃ for 21h to obtain the product PA6.
[0109] (2) The modified SiO2 of Example 2, the product PA6 of step (1), the solvent (a mixture of diethylene glycol and water in a volume ratio of 2:1), and m-cresol-6-sulfonate ammonium were mixed. In the mixture of modified SiO2, PA6, solvent, and m-cresol-6-sulfonate ammonium, the content of m-cresol-6-sulfonate ammonium was 0.3wt%, the content of modified SiO2 was 0.2wt%, and the mass ratio of PA6 to modified SiO2 was 10:1.
[0110] (3) The mixture of modified SiO2, PA6 (the product of step (1)), solvent and m-cresol-6-sulfonate ammonium is heated to 162°C and held for 1.75 h, and then cooled to 30°C at a cooling rate of 0.8°C / min to obtain PA6 / SiO2 composite powder with good thermal stability.
[0111] The yield of the final PA6 / SiO2 composite powder with good thermal stability was 72%. The average particle size of the PA6 / SiO2 composite powder with good thermal stability was 43 μm, the PDI was 0.16, and the thermogravimetric residue of the PA6 / SiO2 composite powder with good thermal stability was 71%.
[0112] Example 8
[0113] A method for preparing PA6 / SiO2 composite powder with good thermal stability, the specific steps of which are as follows:
[0114] (1) At a temperature of 30°C, PA6 (colorless waste PA6 filaments, Jiangsu Haiyang Chemical Fiber Co., Ltd., with a molecular weight of 18000 g / mol) was immersed in a soaping solution with a concentration of 2 g / L at a bath ratio of 1:40. After washing for 1 h, it was dried at 30°C for 18 h to obtain the product PA6.
[0115] (2) The modified SiO2 of Example 3, the product PA6 of step (1), the solvent (a mixture of diethylene glycol and water in a volume ratio of 2:1), and m-cresol-6-sulfonate ammonium were mixed. In the mixture of modified SiO2, PA6, solvent, and m-cresol-6-sulfonate ammonium, the content of m-cresol-6-sulfonate ammonium was 0.2 wt%, the content of modified SiO2 was 0.2 wt%, and the mass ratio of PA6 to modified SiO2 was 10:1.
[0116] (3) The mixture of modified SiO2, PA6 (the product of step (1)), solvent and m-cresol-6-sulfonate ammonium is heated to 165°C and held for 1.5 h, and then cooled to 35°C at a cooling rate of 0.6°C / min to obtain PA6 / SiO2 composite powder with good thermal stability.
[0117] The yield of the final PA6 / SiO2 composite powder with good thermal stability was 70%. The average particle size of the PA6 / SiO2 composite powder with good thermal stability was 44 μm, the PDI was 0.19, and the thermogravimetric residue of the PA6 / SiO2 composite powder with good thermal stability was 71%.
[0118] Example 9
[0119] A method for preparing PA6 / SiO2 composite powder with good thermal stability, the specific steps of which are as follows:
[0120] (1) At a temperature of 32℃, PA6 (colorless waste PA6 filaments, Jiangsu Haiyang Chemical Fiber Co., Ltd., with a molecular weight of 18000g / mol) was immersed in a soaping solution with a concentration of 2g / L at a bath ratio of 1:35. After washing for 1h, it was dried at 32℃ for 15h to obtain the product PA6.
[0121] (2) The modified SiO2 of Example 4, the product PA6 of step (1), the solvent (a mixture of diethylene glycol and water in a volume ratio of 2:1), and m-cresol-6-sulfonate ammonium were mixed. In the mixture of modified SiO2, PA6, solvent, and m-cresol-6-sulfonate ammonium, the content of m-cresol-6-sulfonate ammonium was 0.3wt%, the content of modified SiO2 was 0.3wt%, and the mass ratio of PA6 to modified SiO2 was 11:1.
[0122] (3) The mixture of modified SiO2, PA6 (the product of step (1)), solvent and m-cresol-6-sulfonate ammonium is heated to 158°C and held for 1 hour, and then cooled to 30°C at a cooling rate of 0.2°C / min to obtain PA6 / SiO2 composite powder with good thermal stability.
[0123] The yield of the final PA6 / SiO2 composite powder with good thermal stability was 73%. The average particle size of the PA6 / SiO2 composite powder with good thermal stability was 38 μm, the PDI was 0.13, and the thermogravimetric residue of the PA6 / SiO2 composite powder with good thermal stability was 71.6%.
[0124] Example 10
[0125] A method for preparing PA6 / SiO2 composite powder with good thermal stability, the specific steps of which are as follows:
[0126] (1) At a temperature of 35°C, PA6 (colorless waste PA6 filaments, Jiangsu Haiyang Chemical Fiber Co., Ltd., with a molecular weight of 18000 g / mol) was immersed in a soaping solution with a concentration of 2 g / L at a bath ratio of 1:30. After washing for 1 h, it was dried at 35°C for 24 h to obtain the product PA6.
[0127] (2) The modified SiO2 of Example 5, the product PA6 of step (1), the solvent (a mixture of diethylene glycol and water in a volume ratio of 2:1), and m-cresol-6-sulfonate ammonium were mixed. In the mixture of modified SiO2, PA6, solvent, and m-cresol-6-sulfonate ammonium, the content of m-cresol-6-sulfonate ammonium was 0.4 wt%, the content of modified SiO2 was 0.4 wt%, and the mass ratio of PA6 to modified SiO2 was 12:1.
[0128] (3) The mixture of modified SiO2, PA6 (the product of step (1)), solvent, and m-cresol-6-sulfonate ammonium is heated to 155°C and held for 2 hours, and then cooled to 35°C at a cooling rate of 0.5°C / min to obtain PA6 / SiO2 composite powder with good thermal stability.
[0129] The yield of the final PA6 / SiO2 composite powder with good thermal stability was 75%. The average particle size of the PA6 / SiO2 composite powder with good thermal stability was 30 μm, the PDI was 0.1, and the thermogravimetric residue of the PA6 / SiO2 composite powder with good thermal stability was 73%.
Claims
1. A method for preparing modified SiO2, characterized in that, First, nano-SiO2 is impregnated in a condensed tannin dispersion. After post-treatment, nano-SiO2 with adsorbed condensed tannin is obtained. Then, nano-SiO2 with adsorbed condensed tannin and tannic acid are mixed in a solvent and after post-treatment, modified SiO2 is obtained.
2. The method for preparing modified SiO2 according to claim 1, characterized in that, The concentration of the condensed tannin dispersion was 15-22 wt%; the mass ratio of nano-SiO2 to the condensed tannin dispersion was 1:13.3-19; the nano-SiO2 was impregnated in the condensed tannin dispersion at a temperature of 80-90℃ for 2-3 hours.
3. The method for preparing modified SiO2 according to claim 1, characterized in that, The specific process of mixing nano-SiO2 adsorbed with condensed tannins and tannic acid in a solvent is as follows: After dispersing nano-SiO2 adsorbed with condensed tannins in water to obtain a dispersion, tannic acid is added dropwise to the dispersion.
4. The method for preparing modified SiO2 according to claim 3, characterized in that, The dispersion temperature is 60~65℃, the time is 1~1.5min, and the rotation speed is 1300~1400rpm.
5. The method for preparing modified SiO2 according to claim 3, characterized in that, The mass fraction of nano-SiO2 adsorbed with condensed tannins in the dispersion is 0.2~0.5wt%; the mass ratio of tannic acid to nano-SiO2 adsorbed with condensed tannins is 1:17~25.
6. The modified SiO2 prepared by the method for preparing modified SiO2 according to any one of claims 1 to 5, characterized in that, The modified SiO2 contains 40-50 wt% condensed tannins and 0.06-0.07 wt% tannic acid. After five washings, the thermogravimetric residue is 81-83 wt%.
7. A method for preparing PA6 / SiO2 composite powder with good thermal stability, characterized in that, The modified SiO2, PA6, solvent, and ammonium m-cresol-6-sulfonate as described in claim 6 are mixed, and a PA6 / SiO2 composite powder with good thermal stability is prepared by dissolution and precipitation method; in the mixture of modified SiO2, PA6, solvent, and ammonium m-cresol-6-sulfonate, the content of ammonium m-cresol-6-sulfonate is 0.2~0.4wt%, the content of modified SiO2 is 0.2~0.4wt%, and the mass ratio of PA6 to modified SiO2 is 10~12:1; The specific process for preparing PA6 / SiO2 composite powder with good thermal stability by the dissolution-precipitation method is as follows: a mixture of modified SiO2, PA6, solvent, and m-cresol-6-sulfonate ammonium is heated to 155~165℃ and held for 1~2h, and then cooled to below 40℃ at a cooling rate of 0.2~1℃ / min to obtain PA6 / SiO2 composite powder with good thermal stability.
8. The method for preparing PA6 / SiO2 composite powder with good thermal stability according to claim 7, characterized in that, The solvent is a mixture of diethylene glycol and water in a volume ratio of 2:
1.
9. The method for preparing PA6 / SiO2 composite powder with good thermal stability according to claim 7, characterized in that, The yield of PA6 / SiO2 composite powder with good thermal stability is 70-75%. The yield is calculated as: (mass of PA6 / SiO2 composite powder with good thermal stability after drying) / (mass of PA6 added + mass of modified SiO2 added) × 100%. The average particle size of PA6 / SiO2 composite powder with good thermal stability is 30-50 μm, the PDI is 0.1-0.2, and the thermogravimetric residue is 69-73%.
Citation Information
Patent Citations
Method for manufacturing nylon6 / nanometer SiO2 composite fiber material
CN101871138A
Particle-size-controllable silica-coated zinc oxide composite nanoparticle / vegetable tannin compound tanning agent and preparation method thereof