A method and system for predicting rheological behavior of cement-based materials

By calculating the physical properties and particle surface adsorption amount of composite gel materials, the yield stress and plastic viscosity of cement-based materials are predicted, which solves the problem of predicting and adjusting the rheological properties of cement-based materials, and improves rheological performance stability and engineering adaptability. sex.

CN117825212BActive Publication Date: 2024-10-08QINGDAO UNIV OF TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410185462.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-19
Publication Date
2024-10-08
Estimated Expiration
2044-02-19

AI Technical Summary

Technical Problem

It is difficult to accurately predict and quickly adjust the rheological properties of cement-based materials with existing technology, especially when the physical property parameters of raw materials change, resulting in poor rheological stability of the mix.

Method used

By obtaining the physical properties of the raw materials in the cement slurry mix ratio, we can calculate the physical properties and packing density of the composite gel material, obtain the adsorption amount and saturation content on the particle surface, calculate the yield stress and plastic viscosity, and adjust and optimize the cement slurry based on these parameters. It provides the rheological properties prediction method of cement-mineral powder and cement-fly ash microbead systems.

Benefits of technology

It achieves accurate prediction and rapid adjustment of the rheological properties of cement-based materials, improves the stability of the rheological properties of the mix, saves cost and time, and adapts to different construction conditions and changes in raw materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117825212B_ABST
    Figure CN117825212B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of cement-based materials, and provides a method and system for predicting the rheological behavior of cement-based materials, comprising: obtaining physical properties of raw materials in a cement paste mix ratio; calculating physical properties and bulk density of a composite gel material system according to the obtained physical properties; obtaining the adsorption amount and saturated dosage on the surface of composite gel material particles, and calculating the separation distance on the surface of composite gel material particles; calculating the yield stress and plastic viscosity of a cement-mineral admixture composite cementitious material cement paste based on the obtained physical properties and bulk density of the composite gel material system and the separation distance on the surface of the composite gel material particles; adjusting and optimizing the rheological properties of the cement paste according to the obtained yield stress and plastic viscosity, and completing the prediction of the rheological behavior of the cement-based material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of cement-based materials, and in particular relates to a method and system for predicting the rheological behavior of cement-based materials. Background Art

[0002] The statements in this section merely provide background information related to the present invention and do not necessarily constitute prior art.

[0003] With the increasing number of large-scale infrastructure construction, the requirements for energy conservation and environmental protection of cement-based raw materials are becoming higher and higher. In order to reduce the adverse effects of excessive use of cement clinker on the environment, mineral admixtures, as a low-carbon, energy-saving auxiliary cementitious material, are increasingly used in cement-based materials. In the process of preparing cement-based materials, adding an appropriate amount of mineral admixtures to replace cement clinker can not only reduce carbon emissions and achieve sustainable development, but also improve the mechanical properties and durability of cement-based materials and extend the service life of the structure; among them, mineral powder and fly ash microspheres are currently widely used due to their excellent physical and chemical properties.

[0004] According to the inventors’ understanding, the rheological properties of cement-based materials can be controlled by adjusting a large number of macroscopic tests on the proportion of each component in the mix ratio. However, the rheological properties of the prepared mixture are relatively poorly stable, and it is impossible to accurately predict and quickly adjust the mix ratio according to changes in the physical property parameters of the raw materials. It is of broader theoretical and engineering significance to study the influence rules and mechanisms of the yield stress and plastic viscosity of cement pastes made of mineral powder and fly ash microbeads, and to predict and optimize their rheological properties through physical and chemical properties such as raw material particle size distribution, density and specific surface area. Therefore, how to provide a theoretical method for accurately predicting and quickly adjusting the mix ratio of cement-based materials according to the specific construction conditions for the requirements of the rheological properties of cement-based materials and the changes in the physical property parameters of raw materials is a technical problem that technical personnel in this field urgently need to solve. Summary of the invention

[0005] To solve the above problems, the present invention proposes a method and system for predicting the rheological behavior of cement-based materials. Based on the volume proportion of cementitious materials in cement paste and the accurate prediction of physical properties such as particle size distribution, density and specific surface area of ​​each component, and optimization of the yield stress and plastic viscosity of cement paste, a theoretical method is provided for predicting and optimizing the rheological properties of cement pastes in cement-mineral powder and cement-fly ash microbead systems.

[0006] According to some embodiments, a first solution of the present invention provides a method for predicting the rheological behavior of cement-based materials, using the following technical solution:

[0007] A method for predicting the rheological behavior of cement-based materials, comprising:

[0008] Obtain the physical properties of raw materials in cement paste mix;

[0009] Calculating the physical properties and bulk density of the composite gel material system based on the obtained physical properties;

[0010] Obtaining the adsorption amount and saturation dosage on the surface of the composite gel material particles, and calculating the separation distance on the surface of the composite gel material particles;

[0011] Based on the obtained physical properties and bulk density of the composite gel material system and the separation distance of the composite gel material particle surfaces, the yield stress and plastic viscosity of the cement-mineral admixture composite cementitious material cement paste are calculated;

[0012] The rheological properties of cement paste are adjusted and optimized according to the obtained yield stress and plastic viscosity to complete the prediction of rheological behavior of cement-based materials.

[0013] As a further technical limitation, a total organic carbon adsorption test was used to test the adsorption amount and saturated dosage of different water reducer dosages on the surface of composite gelling material particles, and the adsorption amount and saturated dosage on the surface of composite gelling material particles were obtained; then, according to the Langmuir monolayer adsorption model, the adsorption-desorption equilibrium rate constant of the water reducer used was calculated, and the separation distance between the surfaces of composite gelling material particles was calculated by the statistical distribution formula.

[0014] As a further technical definition, the yield stress of the cement paste of the cement-mineral admixture composite cementitious material is in, is an explicit function that takes into account the influence of particle size distribution of cementitious material system; A0 is the non-delayed Hamaker constant; a * is the curvature radius of the contact point; d is the average radius of the composite system; is the solid volume fraction of gel particles in the suspension; is the percolation volume fraction of the cementitious material in the suspension; h is the separation distance between the surfaces of the cementitious material particles mixed with the water reducing agent; is the bulk density of different composite cementitious material systems.

[0015] Furthermore, the plastic viscosity μ of the cement paste of the cement-mineral admixture composite cementitious material is p for Where, μ0 is the plastic viscosity of the interstitial liquid; q p is the exponential power.

[0016] As a further technical definition, the calculated physical properties of the composite gel material system include at least the particle size distribution of the composite system, an explicit function considering the effect of the particle size distribution of the gel material system, and an average radius.

[0017] As a further technical limitation, a modified model based on a compressible stacking model (hereinafter referred to as a 3-parameter stacking model) is used to calculate the stacking density of the composite gel material system; the 3-parameter stacking model includes a loosening effect, a wall effect, and a wedge effect.

[0018] As a further technical definition, the physical properties of the cement paste obtained include at least cementitious material density, specific surface area and particle size distribution.

[0019] According to some embodiments, a second solution of the present invention provides a rheological behavior prediction system for cement-based materials, which adopts the following technical solution:

[0020] A rheological behavior prediction system for cement-based materials, comprising:

[0021] An acquisition module configured to acquire physical properties of raw materials in a cement paste mix;

[0022] A calculation module, which is configured to calculate the physical properties and bulk density of the composite gel material system according to the obtained physical properties; obtain the adsorption amount and saturation dosage on the surface of the composite gel material particles, and calculate the separation distance of the surface of the composite gel material particles; based on the obtained physical properties and bulk density of the composite gel material system, and the separation distance of the surface of the composite gel material particles, calculate the yield stress and plastic viscosity of the cement-mineral admixture composite cementitious material cement paste;

[0023] The prediction module is configured to adjust and optimize the rheological properties of the cement paste according to the obtained yield stress and plastic viscosity, so as to complete the prediction of the rheological behavior of the cement-based material.

[0024] According to some embodiments, a third solution of the present invention provides a computer-readable storage medium, which adopts the following technical solution:

[0025] A computer-readable storage medium stores a program, which, when executed by a processor, implements the steps in the method for predicting the rheological behavior of cement-based materials as described in the first embodiment of the present invention.

[0026] According to some embodiments, a fourth solution of the present invention provides an electronic device, which adopts the following technical solution:

[0027] An electronic device comprises a memory, a processor and a program stored in the memory and running on the processor, wherein when the processor executes the program, the steps in the method for predicting the rheological behavior of cement-based materials as described in the first embodiment of the present invention are implemented.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] The present invention solves the problem of regulating the rheological properties of cement-based materials by adjusting the proportion of each component in the mix ratio through a large number of macro tests in the project, thereby saving cost and time, reducing workload, and the prepared mixture has more excellent rheological stability. The mix ratio can be predicted based on the physical properties of the raw materials to meet the requirements of the rheological properties of the mix in different projects, and the mix ratio can be quickly adjusted when the requirements of the rheological properties of the mix or the physical property parameters of the raw materials change according to different construction scenarios. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The drawings in the specification that constitute a part of this embodiment are used to provide a further understanding of this embodiment. The schematic embodiments of this embodiment and their descriptions are used to explain this embodiment and do not constitute improper limitations on this embodiment.

[0031] Figure 1 This is a flow chart of the method for predicting the rheological behavior of cement-based materials in Example 1 of the present invention;

[0032] Figure 2 Detailed step schematic diagram of the method for predicting the rheological behavior of cement-based materials in Example 1 of the present invention;

[0033] FIG3( a ) is a schematic diagram showing the relationship between the yield stress test value and the calculated value in Example 1 of the present invention;

[0034] FIG3( b ) is a schematic diagram showing the relationship between the plastic viscosity test value and the calculated value in Example 1 of the present invention;

[0035] Figure 4 This is a structural block diagram of the rheological behavior prediction system for cement-based materials in Example 2 of the present invention. DETAILED DESCRIPTION

[0036] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.

[0037] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.

[0038] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0039] In the present invention, terms such as "upper", "lower", "left", "right", "front", "back", "vertical", "horizontal", "side", "bottom", etc. indicate directions or positional relationships based on the directions or positional relationships shown in the accompanying drawings. They are relational words determined only for the convenience of describing the structural relationships of the various parts or elements of the present invention, and do not specifically refer to any part or element in the present invention and should not be understood as limitations on the present invention.

[0040] In the present invention, terms such as "fixed connection", "connected", "connection", etc. should be understood in a broad sense, indicating that it can be fixedly connected, integrally connected or detachably connected; it can be directly connected or indirectly connected through an intermediate medium. For relevant scientific research or technical personnel in this field, the specific meanings of the above terms in the present invention can be determined according to specific circumstances, and they cannot be understood as limitations on the present invention.

[0041] In the absence of conflict, the embodiments of the present invention and the features of the embodiments may be combined with each other.

[0042] Embodiment 1

[0043] Embodiment 1 of the present invention introduces a method for predicting the rheological behavior of cement-based materials.

[0044] like Figure 1 and Figure 2 A method for predicting the rheological behavior of a cement-based material is shown, comprising:

[0045] Obtain the physical properties of raw materials in cement paste mix;

[0046] Calculating the physical properties and bulk density of the composite gel material system based on the obtained physical properties;

[0047] Obtaining the adsorption amount and saturation dosage on the surface of the composite gel material particles, and calculating the separation distance on the surface of the composite gel material particles;

[0048] Based on the obtained physical properties and bulk density of the composite gel material system and the separation distance of the composite gel material particle surfaces, the yield stress and plastic viscosity of the cement-mineral admixture composite cementitious material cement paste are calculated;

[0049] The rheological properties of cement paste are adjusted and optimized according to the obtained yield stress and plastic viscosity to complete the prediction of rheological behavior of cement-based materials.

[0050] As one or more implementation modes, the physical properties of the cement paste obtained include at least the density of the cementitious material, the specific surface area and the particle size distribution; the physical properties of the composite cementitious material system are calculated based on the obtained physical properties such as the particle size distribution of the cementitious material; wherein the particle size distribution and the average radius need to be calculated based on the proportion of the cementitious material in the mix ratio and the particle size distribution of the cementitious material.

[0051] As one or more embodiments, according to the physical properties of the composite cementitious material system, the packing density of the composite cementitious material system is calculated by a 3-parameter packing model; that is, Among them, y i is the volume fraction of particles of size i, φ i is the packing density of particles of size i; a ij 、b ij and c ij They are the “loosening effect”, “wall effect” and “wedge effect” in the 3-PM model. ij =1-(1-s) 3.3 -2.6·s·(1-s) 3.6 , b ij =1-(1-s) 1.9 -2·s·(1-s) 6 , c ij =0.322·tanh(11.9·s).

[0052] As one or more implementation methods, a total organic carbon adsorption test is used to first test the adsorption amount and saturation amount of different water reducer dosages on the surface of composite cementitious material particles, and then calculate the adsorption-desorption equilibrium rate constant of the water reducer used according to the Langmuir monolayer adsorption model, and finally calculate the separation distance between the surfaces of composite cementitious material particles using a statistical distribution formula. Wherein, Γ is the unit adsorption amount of medium water reducing agent (SP) on cement particles, mg / g; V is the volume of SP solution, ml; C0 and C1 are the concentrations of organic carbon in SP solution before and after adsorption, respectively, and C2 is the concentration of organic carbon in cement paste without water reducing agent, g / ml; m is the mass of cement, g; the coverage rate of polymer on the surface of cementitious material particles is D rsp is the relative dosage of water reducing agent (D rsp =D sp / D sat , where D sp is the mass dosage of water reducer relative to cementitious material, D sat is the saturated dosage of water reducer; h is the separation distance between the surfaces of the cementitious material particles mixed with water reducer, nm; H p It is the separation distance between the surfaces after the water reducer is saturatedly adsorbed on the particle surface, which is approximately equal to four times the dynamic radius of the polymer in the water reducer, and its value is usually 4nm~12nm; H0 is the separation distance between the surfaces of the cementitious material particles without water reducer, and its value is usually 1nm~2nm.

[0053] As one or more embodiments, based on the YODEL model, the yield stress of cement paste of cement-mineral admixture composite cementitious material is calculated. Among them, τ p is the yield stress of the suspension, Pa; A0 is the non-delayed Hamaker constant, usually 1.6×10-20J; a * is the curvature radius of the contact point, ranging from 300 to 500 nm; d is the average radius of the composite system; is the solid volume fraction of gel particles in the suspension; is the percolation volume fraction of the gelling material in the suspension, usually ranging from 20 to 40%; is the maximum volume fraction of different composite cementitious material systems, which can be calculated through step b; is an explicit function that takes into account the influence of particle size distribution of cementitious material system, namely

[0054] Plastic viscosity of cement paste of cement-mineral admixture composite cementitious material Among them, μ p is the plastic viscosity of the suspension, Pa·s; μ0 is the plastic viscosity of the interstitial liquid, Pa·s; q p is an index, usually

[0055] This embodiment takes cement-mineral powder and cement-microsphere system cement paste as examples for detailed description; the cement paste formulation ratios used are shown in Table 1.

[0056] Table 1 Cement paste mix ratio

[0057]

[0058]

[0059] Based on the shear stress and shear rate curves of each group of cement pastes in Table 1 tested by the rheometer, the HB model was used to calculate the yield stress and plastic viscosity of each group of pastes; that is, Where τ is the shear stress, Pa; τ p is the yield stress of the mixture, Pa; is the shear rate, s -1 , a and b are fitting; Among them, μ p is the plastic viscosity of the mixture, Pa·s; is the maximum shear rate, s -1 .

[0060] The relationship between the experimental value and the calculated value of the yield stress and plastic viscosity of each group is shown in Figure 3 (a) and Figure 3 (b) respectively. In order to reduce the amount of calculation, this embodiment uses the yield stress and plastic viscosity of the pure cement system as the benchmark, and uses the relative yield stress and plastic viscosity of the cement-mineral powder and cement-fly ash microsphere system to represent the influence of the physical and chemical properties of each component in the composite cementitious material system on the rheological parameters; it can be obtained that the calculated value of the relative yield stress and plastic viscosity has a high degree of agreement with the experimental value, which verifies that the basic characteristics of the maximum bulk density and size distribution of the pure cement system are also applicable to the cement paste system with mineral admixtures. Combined with the yield stress and plastic viscosity model, the yield stress and plastic viscosity of the cement paste are predicted and optimized according to the proportion of cementitious materials and their respective physical properties such as particle size distribution and density.

[0061] This embodiment solves the problem of regulating the rheological properties of cement-based materials by adjusting the proportion of each component in the mix ratio through a large number of macro tests in the project, saving cost and time, reducing workload, and the prepared mixture has better rheological stability; the mix ratio can be predicted based on the physical properties of the raw materials to meet the requirements of the rheological properties of the mixture in different projects, and the mix ratio can also be quickly adjusted when the requirements of the rheological properties of the mixture or the physical property parameters of the raw materials change according to different construction scenarios.

[0062] Embodiment 2

[0063] The second embodiment of the present invention introduces a rheological behavior prediction system for cement-based materials.

[0064] like Figure 4 A rheological behavior prediction system for cement-based materials is shown, comprising:

[0065] An acquisition module configured to acquire physical properties of raw materials in a cement paste mix;

[0066] A calculation module, which is configured to calculate the physical properties and bulk density of the composite gel material system according to the obtained physical properties; obtain the adsorption amount and saturation dosage on the surface of the composite gel material particles, and calculate the separation distance of the surface of the composite gel material particles; based on the obtained physical properties and bulk density of the composite gel material system, and the separation distance of the surface of the composite gel material particles, calculate the yield stress and plastic viscosity of the cement-mineral admixture composite cementitious material cement paste;

[0067] The prediction module is configured to adjust and optimize the rheological properties of the cement paste according to the obtained yield stress and plastic viscosity, so as to complete the prediction of the rheological behavior of the cement-based material.

[0068] The detailed steps are the same as those of the method for predicting the rheological behavior of cement-based materials provided in Example 1, and will not be repeated here.

[0069] Embodiment 3

[0070] Embodiment 3 of the present invention provides a computer-readable storage medium.

[0071] A computer-readable storage medium stores a program, which, when executed by a processor, implements the steps in the method for predicting the rheological behavior of cement-based materials as described in the first embodiment of the present invention.

[0072] The detailed steps are the same as those of the method for predicting the rheological behavior of cement-based materials provided in Example 1, and will not be repeated here.

[0073] Embodiment 4

[0074] A fourth embodiment of the present invention provides an electronic device.

[0075] An electronic device comprises a memory, a processor and a program stored in the memory and running on the processor, wherein when the processor executes the program, the steps in the method for predicting the rheological behavior of cement-based materials as described in the first embodiment of the present invention are implemented.

[0076] The detailed steps are the same as those of the method for predicting the rheological behavior of cement-based materials provided in Example 1, and will not be repeated here.

[0077] The above description is only a preferred embodiment of the present embodiment and is not intended to limit the present embodiment. For those skilled in the art, the present embodiment may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present embodiment shall be included in the protection scope of the present embodiment.

Claims

1. A method for predicting the rheological behavior of cement-based materials, characterized in that: include: Obtain the physical properties of raw materials in cement paste mix; Calculating the physical properties and bulk density of the composite gel material system based on the obtained physical properties; Obtaining the adsorption amount and saturation dosage on the surface of the composite gel material particles, and calculating the separation distance on the surface of the composite gel material particles; Based on the obtained physical properties and bulk density of the composite gel material system and the separation distance of the composite gel material particle surfaces, the yield stress and plastic viscosity of the cement-mineral admixture composite cementitious material cement paste are calculated; The rheological properties of cement paste are adjusted and optimized according to the obtained yield stress and plastic viscosity to complete the rheological behavior prediction of cement-based materials; The physical properties of the cement paste obtained include at least density, specific surface area and particle size distribution of the cementitious material; The total organic carbon adsorption test was used to test the adsorption amount and saturation amount of different water reducer dosages on the surface of composite gelling material particles, and the adsorption amount and saturation amount on the surface of composite gelling material particles were obtained; then, the adsorption-desorption equilibrium rate constant of the water reducer used was calculated according to the Langmuir monolayer adsorption model, and the separation distance between the surfaces of composite gelling material particles was calculated by the statistical distribution formula; The yield stress τ of the cement paste of the cement-mineral admixture composite cementitious material p for in, is an explicit function that takes into account the influence of particle size distribution of cementitious material system; A0 is the non-delayed Hamaker constant; a * is the curvature radius of the contact point; d is the average radius of the composite system; is the solid volume fraction of gel particles in the suspension; is the percolation volume fraction of the cementitious material in the suspension; h is the separation distance between the surfaces of the cementitious material particles mixed with the water reducing agent; is the bulk density of different composite cementitious material systems; The plastic viscosity μ of the cement paste of the cement-mineral admixture composite cementitious material p for Where, μ0 is the plastic viscosity of the interstitial liquid; q p is the exponential power.

2. The method for predicting the rheological behavior of cement-based materials as claimed in claim 1, characterized in that: The packing density of the composite gel material system is calculated by using a modified model based on a compressible packing model; the modified model based on the compressible packing model includes a loosening effect, a wall effect and a wedge effect.

3. A rheological behavior prediction system for cement-based materials, characterized in that: include: An acquisition module, which is configured to acquire physical properties of raw materials in a cement paste mix ratio; A calculation module, which is configured to calculate the physical properties and bulk density of the composite gel material system according to the obtained physical properties; obtain the adsorption amount and saturation dosage on the surface of the composite gel material particles, and calculate the separation distance of the surface of the composite gel material particles; based on the obtained physical properties and bulk density of the composite gel material system, and the separation distance of the surface of the composite gel material particles, calculate the yield stress and plastic viscosity of the cement-mineral admixture composite cementitious material cement paste; A prediction module, which is configured to adjust and optimize the rheological properties of the cement paste according to the obtained yield stress and plastic viscosity, and complete the rheological behavior prediction of the cement-based material; The physical properties of the cement paste obtained include at least density, specific surface area and particle size distribution of the cementitious material; The total organic carbon adsorption test was used to test the adsorption amount and saturation amount of different water reducer dosages on the surface of composite gelling material particles, and the adsorption amount and saturation amount on the surface of composite gelling material particles were obtained; then, the adsorption-desorption equilibrium rate constant of the water reducer used was calculated according to the Langmuir monolayer adsorption model, and the separation distance between the surfaces of composite gelling material particles was calculated by the statistical distribution formula; The yield stress τ of the cement paste of the cement-mineral admixture composite cementitious material p for in, is an explicit function that takes into account the influence of particle size distribution of cementitious material system; A0 is the non-delayed Hamaker constant; a * is the curvature radius of the contact point; d is the average radius of the composite system; is the solid volume fraction of gel particles in the suspension; is the percolation volume fraction of the cementitious material in the suspension; h is the separation distance between the surfaces of the cementitious material particles mixed with the water reducing agent; is the bulk density of different composite cementitious material systems; The plastic viscosity μ of the cement paste of the cement-mineral admixture composite cementitious material p for Where, μ0 is the plastic viscosity of the interstitial liquid; q p is the exponential power.

4. A computer-readable storage medium having a computer program stored thereon, characterized in that: When the program is executed by a processor, the steps of the method for predicting the rheological behavior of cement-based materials as described in any one of claims 1-2 are implemented.

5. An electronic device comprising a memory, a processor, and a computer program stored in the memory and running on the processor, characterized in that: When the processor executes the program, the steps of the method for predicting the rheological behavior of cement-based materials as described in any one of claims 1-2 are implemented.