Composite current collector, method for preparing the same, battery pole piece and battery
By modifying the composite structure of polypropylene film and metal layer, the problem of insufficient bonding force between polypropylene layer and metal layer is solved, thereby improving the energy density and cycle performance of lithium-ion battery.
Patent Information
- Application Number
- CN202311723400.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-14
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-12-14
AI Technical Summary
The low bonding force between the polypropylene layer and the metal layer in existing composite current collectors makes them prone to cracking during the rolling process, affecting the energy density and stability of lithium-ion batteries.
By modifying polypropylene with polyvinyl alcohol, polyacrylic acid and inorganic nano-oxides, a modified polypropylene membrane is formed. A metal layer is then electrodeposited on its surface to form a composite structure of modified polypropylene membrane and metal layer. A porous membrane is then prepared using electrospinning technology to improve the bonding force.
It improves the adhesion and tensile strength between the modified polypropylene film and the metal layer, reduces the delamination and detachment of the composite current collector, and enhances the energy density and cycle performance of the battery.
Smart Images

Figure CN117832504B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery technology, and more specifically, to a composite current collector and its preparation method, battery electrodes, and a battery. Background Technology
[0002] Secondary batteries, such as lithium-ion batteries, are widely used in new energy vehicles due to their advantages such as small size, light weight, high energy density, and zero pollution. Driven by the growing demand for sustainable development, the development of lithium-ion batteries (LIBs) urgently requires electrode materials with high energy density. The higher the energy density of a battery, the more electricity it can store per unit volume or weight, resulting in greater range for new energy vehicles. Therefore, improving the energy density of lithium-ion batteries is particularly important.
[0003] Current collectors are key materials in lithium-ion battery cells, serving as the positive and negative electrodes. As a structure or component that collects current, their function is to gather electrons generated by the electrochemical reaction and conduct them to the external circuit, thus realizing the conversion of chemical energy into electrical energy. Currently, most commercially available battery electrodes use copper and aluminum foil. However, copper and aluminum foil have high energy densities. Therefore, to reduce the impact of copper and aluminum foil on the energy density of lithium-ion batteries, composite current collectors using lower-density polymer materials as the substrate and metal-plated surfaces are being used to replace pure metal foils. This significantly improves the battery's energy density.
[0004] Currently, polymer-based composite current collectors primarily use polypropylene (PP) and polyethylene terephthalate (PET) as the intermediate layer. Although PP has stronger corrosion resistance than PET, its adhesion to the copper layer is relatively low due to the presence of only non-polar bonds. Therefore, excessive compaction density during rolling makes it more prone to cracking. Thus, improving the adhesion of PP in composite current collectors is a pressing technical problem that needs to be solved. Summary of the Invention
[0005] In view of this, the present invention aims to at least partially solve one of the technical problems in the related art. To this end, the present invention provides a composite current collector and its preparation method, a battery electrode, a secondary battery, and an electrical device, which can alleviate the problem of low bonding strength between the polypropylene layer and the metal layer in existing composite current collectors, and can effectively improve the bonding strength between the polypropylene layer and the metal layer.
[0006] To solve the above-mentioned technical problems, this application is implemented as follows:
[0007] According to a first aspect of this application, an embodiment of this application provides a composite current collector, which includes a modified polypropylene membrane and a metal layer disposed on at least one surface of the modified polypropylene membrane along its thickness direction.
[0008] The modified polypropylene film is formed by modifying polypropylene with polyvinyl alcohol, polyacrylic acid and inorganic nano-oxides.
[0009] In addition, the composite current collector according to this application may also have the following additional technical features:
[0010] In some embodiments, the inorganic nano-oxide has a particle size of 5 nm to 100 nm.
[0011] In some of these embodiments, the inorganic nano-oxide includes at least one of silicon dioxide, aluminum oxide, zirconium oxide, zinc oxide, titanium oxide, calcium oxide, antimony pentoxide, magnesium oxide, nickel oxide, chromium oxide, or cobalt oxide.
[0012] In some embodiments, the material of the metal layer includes at least one of copper, copper alloy, aluminum, aluminum alloy, nickel, nickel alloy, titanium, or silver.
[0013] In some embodiments, the modified polypropylene film has the metal layer on both surfaces along its thickness direction.
[0014] In some embodiments, the thickness of the metal layer is 0.5 μm to 5 μm, and the thickness of the modified polypropylene film is 1 μm to 10 μm.
[0015] In some embodiments, the modified polypropylene film comprises, by weight, the following components:
[0016] 400-600 parts of polypropylene, 100-300 parts of polyvinyl alcohol, 200-400 parts of polyacrylic acid, and 10-30 parts of inorganic nano-oxides.
[0017] According to a second aspect of this application, embodiments of this application provide a method for preparing a composite current collector, the method comprising the following steps:
[0018] A modified polypropylene membrane is provided, which is formed by modifying polypropylene with polyvinyl alcohol, polyacrylic acid and inorganic nano-oxides; a metal is electrodeposited on the surface of the modified polypropylene membrane to form a metal layer on the surface of the modified polypropylene membrane, thereby obtaining a composite current collector comprising the modified polypropylene membrane and the metal layer.
[0019] In some embodiments, the step of providing the modified polypropylene film specifically includes:
[0020] Polypropylene, polyvinyl alcohol, polyacrylic acid and solvent are mixed evenly, and then inorganic nano-oxide and non-solvent are added and mixed evenly to obtain a spinning solution; the modified polypropylene film is prepared by electrospinning of the spinning solution.
[0021] In some of these embodiments, the mass ratio of the polypropylene, the polyvinyl alcohol, the polyacrylic acid and the inorganic nano-oxide is (400-600):(100-300):(200-400):(10-30).
[0022] In some embodiments, the mass ratio of the polypropylene to the volume ratio of the solvent is (400-600) mg: (10-30) mL.
[0023] In some embodiments, the volume ratio of the solvent to the non-solvent is 4–9:1–6.
[0024] In some embodiments, the volume ratio of the solvent to the non-solvent is 5-6:4-5.
[0025] In some embodiments, the saturated vapor pressure of the solvent differs from the saturated vapor pressure of the non-solvent at the same temperature by at least 500 Pa.
[0026] In some of these embodiments, the solvent includes at least one of methanol, ethanol, isopropanol, or butanol;
[0027] In some of these embodiments, the non-solvent includes at least one of toluene, o-xylene, p-xylene, m-xylene, or nitrobenzene.
[0028] In some embodiments, after the polypropylene, polyvinyl alcohol, polyacrylic acid and solvent are mixed evenly, inorganic nano-oxide is added, the temperature is raised to 30°C to 50°C, and then a non-solvent is added. The mixture is stirred for 1 to 3 hours to obtain the spinning solution.
[0029] In some embodiments, the electrospinning operating conditions include:
[0030] The distance between the needle and the receiver is 13cm to 16cm, the voltage is set to 10 to 15kV, the ambient temperature is 20±5℃, and the air humidity is 30±3%.
[0031] In some embodiments, after preparing the modified polypropylene film by electrospinning the spinning solution, the method further includes:
[0032] The modified polypropylene film is subjected to heat treatment, which is annealing at 70℃~80℃ in a vacuum environment for 12h~18h.
[0033] According to a third aspect of this application, an embodiment of this application provides a battery electrode sheet, which includes the composite current collector described above, or includes a composite current collector prepared by the method described above, and an active material layer disposed on the composite current collector.
[0034] According to a fourth aspect of this application, an embodiment of this application provides a battery, including a positive electrode, a negative electrode, a separator, and an electrolyte. The positive electrode includes a positive current collector and a positive active material layer disposed on the positive current collector. The negative electrode includes a negative current collector and a negative active material layer disposed on the negative current collector. The positive current collector and / or the negative current collector is the aforementioned composite current collector, or a composite current collector prepared by the aforementioned method.
[0035] Implementing the technical solution of the present invention has at least the following beneficial effects:
[0036] In this embodiment, the provided composite current collector includes a modified polypropylene film and a metal layer. The modified polypropylene film is formed by modifying polypropylene with polyvinyl alcohol, polyacrylic acid, and inorganic nano-oxides. This results in hydrogen bonds on the surface of the modified polypropylene film, which further enhances the bonding force between the modified polypropylene film and the metal layer. The polyvinyl alcohol and polyacrylic acid in the modified polypropylene film have strong adhesion, which helps improve the adhesion between the metal layer and the modified polypropylene film, i.e., improves peel strength. Simultaneously, it can improve the tensile strength of the composite current collector, thus mitigating delamination and detachment. Furthermore, the inorganic nano-metal oxides and polyvinyl alcohol contain a large number of hydroxyl groups, and the polyacrylic acid contains a relatively large number of carboxyl groups, which is more conducive to the electroplating of metal ions, such as copper ions, onto the modified polypropylene film layer.
[0037] In a preferred embodiment of the present invention, a modified polypropylene membrane is prepared by electrospinning, which results in a viscous membrane surface with abundant microporous structure. The porous structure of the membrane surface allows metal ions such as copper ions to be deposited well on its surface, which is more conducive to the anchoring and deposition of metal ions and can increase the peel strength of the membrane layer.
[0038] Because the composite current collector provided by this invention has strong interlayer bonding force and stable structure, it enables batteries using this composite current collector to have good cycle performance and improve the energy density of the battery.
[0039] Additional aspects and advantages of this application will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of the invention. Attached Figure Description
[0040] The above and other objects, features, and advantages of the present invention will become more apparent from the more detailed description of the embodiments of the invention in conjunction with the accompanying drawings. The drawings are provided to further illustrate the embodiments of the invention and form part of the specification. They are used together with the embodiments of the invention to explain the invention and do not constitute a limitation thereof. In the drawings, the same reference numerals generally represent the same parts or steps.
[0041] Figure 1 The diagram shown is a structural schematic of a composite current collector provided in an embodiment of the present invention;
[0042] Figure 2 The figure shown is a phase diagram of the PAA+PVA system, solvent methanol, and non-solvent toluene provided in an embodiment of the present invention.
[0043] Figure 3 The image shown is a SEM image of the modified polypropylene membrane provided in an embodiment of the present invention.
[0044] Figure 4 The diagram shows the electrodeposition method in the preparation process of the composite current collector provided in an embodiment of the present invention.
[0045] Explanation of reference numerals in the attached figures:
[0046] 10-Composite current collector;
[0047] 110-Modified polypropylene film;
[0048] 120 - Metal layer. Detailed Implementation
[0049] The composite current collector and its preparation method, battery electrode, and battery of the present invention will be further described in detail below with reference to specific embodiments. The present invention can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a thorough and complete understanding of the disclosure of the present invention. Of course, they are merely examples and are not intended to limit the invention.
[0050] When a numerical range is disclosed herein, the range is considered continuous and includes the minimum and maximum values of the range, as well as every value between the minimum and maximum values. Furthermore, when the range refers to integers, it includes every integer between the minimum and maximum values of the range. Additionally, when multiple ranges are provided to describe a feature or characteristic, the ranges may be combined. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges to which they are incorporated.
[0051] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention.
[0052] The composite current collector, its preparation method, battery electrode, and battery of this application are described in detail below.
[0053] [Composite current collector]
[0054] like Figure 1 As shown, in some embodiments, the composite current collector 10 of this application includes a modified polypropylene membrane 110 and a metal layer 120 disposed on at least one surface of the modified polypropylene membrane 110 along its thickness direction; wherein, the modified polypropylene membrane 110 is formed by modifying polypropylene with polyvinyl alcohol, polyacrylic acid and inorganic nano-oxides.
[0055] The provided composite current collector 10 includes a modified polypropylene membrane 110 (layer) and a metal layer 120 stacked together. The modified polypropylene membrane 110 has a first surface and a second surface opposite each other in the thickness direction, and the metal layer 120 can be disposed on the first surface and / or the second surface. For example, the metal layer 120 can be disposed on the first surface of the modified polypropylene membrane 110, or it can be disposed on the second surface of the modified polypropylene membrane 110. Of course, the metal layer 120 can also be disposed on both the first and second surfaces of the modified polypropylene membrane 110.
[0056] In some preferred embodiments, the modified polypropylene film 110 has a metal layer 120 on both surfaces along its thickness direction, that is, the first and second surfaces of the modified polypropylene film 110 are both provided with a metal layer 120.
[0057] The metal layer 120, also known as the conductive metal layer, is laminated on the surface of the modified polypropylene film 110 and serves to conduct electricity. Simultaneously, the modified polypropylene film 110 provides good support for the metal layer 120.
[0058] To alleviate the low adhesion of existing polypropylene-based composite current collectors, i.e., the low bonding strength between the existing polypropylene layer and the metal layer, this application modifies the polypropylene. In this embodiment, the modified polypropylene film is formed by modifying polypropylene with polyvinyl alcohol, polyacrylic acid, and inorganic nano-oxides. That is, polypropylene is modified with polyvinyl alcohol, polyacrylic acid, and inorganic nano-oxides to obtain modified polypropylene, which is then made into a film. By blending polypropylene with polyvinyl alcohol, polyacrylic acid, and inorganic nano-oxides, polyvinyl alcohol and polyacrylic acid modified polypropylene are obtained. Polyacrylic acid and polyvinyl alcohol contain strong adhesiveness, and the polar bonds they contain are more conducive to improving the bonding strength between the metal layer and the modified polypropylene film. In some preferred embodiments, modified polypropylene membranes are prepared by electrospinning. Compared with existing electrospinning methods that use only one solvent and cannot form a porous structure on the fiber surface, the embodiments of this application simultaneously dissolve polypropylene (PP), polyvinyl alcohol (PVA), and polyacrylic acid (PAA) in a solvent and a non-solvent (relative to PVA and PAA). The resulting spinning solution is then electrospinned, which can produce a membrane with adhesive surface and rich microporous structure. This is more conducive to the anchoring and deposition of metal ions (such as copper ions).
[0059] Therefore, the provided composite current collector utilizes the hydrogen bonds formed by polyvinyl alcohol and polyacrylic acid on the surface of the modified polypropylene film, which is more conducive to improving the bonding force between the modified polypropylene film and the metal layer. The polyvinyl alcohol and polyacrylic acid in the modified polypropylene film have strong adhesion, which is beneficial to improving the adhesion between the metal layer and the modified polypropylene film, while also increasing the tensile strength of the composite current collector and improving the phenomena of delamination and peeling. Furthermore, the inorganic nano-metal oxides and polyvinyl alcohol surfaces contain a large number of hydroxyl groups, and polyacrylic acid contains a large number of carboxyl groups, which is more conducive to the electroplating of metal ions such as copper ions on the modified polypropylene film layer. The modified polypropylene film is prepared by a preferred electrospinning method, which allows the adhesive film surface to also have a rich microporous structure. This porous structure allows metal ions such as copper ions to be deposited well on its surface, which is more conducive to the anchoring and deposition of metal ions, and can increase the peel strength of the film layer.
[0060] Furthermore, since the density of the modified polypropylene film is lower than that of metal, it helps to reduce the weight of the battery, thereby further improving the energy density of the battery. In addition, it can also improve the cycle performance of batteries using this composite current collector.
[0061] In some embodiments, the inorganic nano-oxide includes at least one selected from silicon dioxide, aluminum oxide, zirconium oxide, zinc oxide, titanium oxide, calcium oxide, antimony pentoxide, magnesium oxide, nickel oxide, chromium oxide, or cobalt oxide. The inorganic nano-oxide can be nanoscale ceramic particles, and the nanoscale inorganic oxide can be, for example, silicon dioxide, aluminum oxide, zirconium oxide, zinc oxide, titanium oxide, calcium oxide, antimony pentoxide, magnesium oxide, nickel oxide, chromium oxide, cobalt oxide, or a composition of any two or more of the above substances. Preferably, the inorganic nano-oxide includes one or more selected from silicon dioxide, aluminum oxide, or zirconium oxide. More preferably, the inorganic nano-oxide is silicon dioxide. By selecting the above-mentioned inorganic nano-oxides, they are widely available, easily obtained, and have low cost. Furthermore, their application in the modified polypropylene membrane of this application yields better results and can be used to improve the relevant properties of the modified polypropylene membrane.
[0062] Because the aforementioned inorganic nano-oxides, such as silica, possess strong heat resistance and hardness, this embodiment modifies the polypropylene fiber membrane by embedding these inorganic nano-oxides, such as nano-silica, into the modified polypropylene membrane and connecting them through ester groups and hydrogen bonds. This modification effectively improves the high-temperature resistance and puncture strength of the modified polypropylene fiber membrane. Furthermore, the oxygen atoms on the surface of inorganic nano-oxides, such as silica, readily react with water molecules to generate hydroxyl groups, which facilitates the electroplating of metal ions onto the modified polypropylene membrane.
[0063] In some embodiments, the particle size of the inorganic nano-oxide is 5 nm to 100 nm. Further, the particle size of the inorganic nano-oxide is 10 nm to 50 nm. Exemplarily, the particle size of the inorganic nano-oxide is 5 nm, 10 nm, 15 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, etc. By employing inorganic nano-oxides within the above particle size range, for example, the relevant properties of modified polypropylene fibers can be improved, such as high-temperature resistance and puncture strength.
[0064] In some embodiments, the material of the metal layer includes at least one selected from copper, copper alloy, aluminum, aluminum alloy, nickel, nickel alloy, titanium, or silver. Exemplarily, the metal layer can be a copper layer, a copper alloy layer, an aluminum layer, an aluminum alloy layer, a nickel layer, a nickel alloy layer, a titanium layer, a silver layer, or a composite metal layer formed by combining several of the above metal layers.
[0065] For example, in some embodiments, the metal layer comprises aluminum or an aluminum alloy, wherein the aluminum alloy preferably has an aluminum content of 80 wt% or more, more preferably 90 wt% or more.
[0066] For example, in some embodiments, the metal layer comprises copper or a copper alloy, wherein the weight percentage of copper in the copper alloy is preferably 80 wt% or more, more preferably 90 wt% or more.
[0067] In some embodiments, the thickness of the metal layer is 0.5 μm to 5 μm. The thickness of the metal layer refers to the thickness of the metal layer on one side of the modified polypropylene film.
[0068] In some embodiments, a metal layer is provided on both surfaces of the modified polypropylene film along its thickness direction. For example, the thickness of the metal layer on both opposite surfaces of the modified polypropylene film can be 0.5 μm to 5 μm. Further, the thickness of the metal layer is 1 μm to 4 μm. Exemplarily, the thickness of the metal layer is 0.5 μm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, etc. A metal layer thickness within the above range allows the metal layer to have high conductivity, which is beneficial for the composite current collector to have high conductivity and current collection performance, thereby improving battery performance; and it also makes the metal layer less prone to breakage during processing and use, giving the composite current collector high fracture toughness, ensuring good mechanical and operational stability. Furthermore, with a metal layer thickness within the above range, in the event of abnormalities such as pin penetration in the electrochemical device, the burrs generated by the metal layer are smaller, thereby reducing the risk of the generated metal burrs contacting the counter electrode.
[0069] In some embodiments, the thickness of the modified polypropylene film is 1 μm to 10 μm. Further, the thickness of the modified polypropylene film is 2 μm to 8 μm. Exemplarily, the thickness of the modified polypropylene film is 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, etc. The selection and thickness of the modified polypropylene film layer meet the application requirements of the composite current collector while simplifying the preparation process and reducing costs. Simultaneously, a thickness within the above range is more conducive to giving it higher mechanical strength, making it less prone to breakage during reprocessing and use, and providing good support and protection for the metal layer, thus improving the mechanical and operational stability of the composite current collector. It also helps to achieve a smaller battery volume and lower weight, thereby improving the battery's energy density.
[0070] In some embodiments, the modified polypropylene film comprises, by weight, the following components: 400-600 parts of polypropylene, 100-300 parts of polyvinyl alcohol, 200-400 parts of polyacrylic acid, and 10-30 parts of inorganic nano-oxide.
[0071] In some embodiments, the modified polypropylene film comprises, by weight, the following components: 450-550 parts polypropylene, 150-250 parts polyvinyl alcohol, 250-350 parts polyacrylic acid, and 15-20 parts inorganic nano-oxide.
[0072] By controlling the proportions of polypropylene, polyvinyl alcohol, polyacrylic acid, and inorganic nano-oxide within the aforementioned range, that is, by adjusting the amount of polyvinyl alcohol, polyacrylic acid, and inorganic nano-oxide added, it is helpful to give full play to their respective roles, achieve better modification of polypropylene, and reduce costs.
[0073] In the composite current collector of this invention, the tensile strength of the modified polypropylene film layer is preferably 210MPa≤T≤320MPa, and more preferably 230MPa≤T≤290MPa.
[0074] The tensile strength of the modified polypropylene film layer is within the aforementioned range, which is beneficial for the composite current collector to have high mechanical properties, making it less prone to breakage or cracking. Furthermore, it prevents excessive elongation or deformation of the modified polypropylene film layer, thus preventing band breakage or cracking of the metal layer. Simultaneously, it ensures a high bonding strength between the modified polypropylene film layer and the metal layer, making the metal layer less prone to peeling. Therefore, using this composite current collector is beneficial for improving battery life and cycle performance. The tensile strength of the modified polypropylene film layer within the aforementioned range also allows it to provide good support for the metal layer.
[0075] The hydrogen bond structure of the composite current collector in this application embodiment can improve the adhesion between the metal layer and the polymer layer, and the interlayer bonding force is better. This can improve the phenomenon of delamination and detachment of the composite current collector. At the same time, when applied to a battery, it can improve the energy density of the battery and improve the cycle performance of the battery.
[0076] [Preparation method of composite current collector]
[0077] In some embodiments, a method for preparing a composite current collector is also provided, the method comprising the following steps:
[0078] A modified polypropylene film is provided, wherein the modified polypropylene film is formed by modifying polypropylene with polyvinyl alcohol, polyacrylic acid and inorganic nano-oxides;
[0079] Metal is electrodeposited on the surface of a modified polypropylene membrane to form a metal layer on the surface of the modified polypropylene membrane, resulting in a composite current collector comprising a modified polypropylene membrane and a metal layer.
[0080] The method for preparing the composite current collector in this application is based on the same inventive concept as the aforementioned composite current collector, and therefore has at least all the features and advantages described in the aforementioned composite current collector, which will not be repeated here.
[0081] In this embodiment, a metal layer can be formed on at least one surface of the modified polypropylene film by electroplating. For example, a metal layer can be formed on the first surface of the modified polypropylene film by electroplating; or, a metal layer can be formed on the second surface of the modified polypropylene film by electroplating; or, a metal layer can be formed on both the first and second surfaces of the modified polypropylene film by electroplating. Preferably, the metal layer is disposed on both the first and second surfaces of the modified polypropylene film.
[0082] In this embodiment, a modified polypropylene membrane is obtained by dissolving polypropylene, polyvinyl alcohol, and polyacrylic acid in a solvent and then electrospinning. The polyvinyl alcohol and polyacrylic acid possess strong viscosity, and the hydrogen bonding formed by their combination further enhances the adhesion between the metal layer and the modified polypropylene membrane. Furthermore, the porous fiber membrane obtained through electrospinning phase separation allows for efficient deposition of metal ions on its surface.
[0083] In some embodiments, the step of providing the modified polypropylene film specifically includes:
[0084] Polypropylene, polyvinyl alcohol and polyacrylic acid are added to a solvent in a certain proportion and mixed evenly. Then, inorganic nano-oxides are added until completely dissolved. Finally, non-solvents are added and mixed evenly to obtain a spinning solution.
[0085] Modified polypropylene membranes were prepared by electrospinning the spinning solution.
[0086] It should be noted that the solvents and non-solvents mentioned above are relative to polyvinyl alcohol and polyacrylic acid. That is, solvents can be used to dissolve polyvinyl alcohol and polyacrylic acid, while non-solvents cannot be used to dissolve polyvinyl alcohol and polyacrylic acid.
[0087] In some embodiments, the mass ratio of polypropylene, polyvinyl alcohol, polyacrylic acid, and inorganic nano-oxide is (400–600):(100–300):(200–400):(10–30). Further, the mass ratio of polypropylene, polyvinyl alcohol, polyacrylic acid, and inorganic nano-oxide is (450–550):(150–250):(250–350):(15–25). For example, the mass ratio of polypropylene, polyvinyl alcohol, polyacrylic acid, and inorganic nano-oxide is 400:100:200:10, 450:150:250:12, 500:200:300:20, 550:220:350:25, 600:300:400:30, etc.
[0088] In some embodiments, the mass-to-volume ratio of polypropylene to solvent is (400–600) mg : (10–30) mL. Further, the mass-to-volume ratio of polypropylene to solvent is (400–600) mg : (12–20) mL. For example, the mass-to-volume ratio of polypropylene to solvent is 400 mg : 12 mL, 450 mg : 12 mL, 500 mg : 12 mL, 500 mg : 15 mL, 500 mg : 18 mL, 600 mg : 20 mL, etc.
[0089] In the process of preparing modified polypropylene membranes, by controlling the amount of polypropylene, polyvinyl alcohol, polyacrylic acid, inorganic nano-oxides, etc. added, it is helpful to give full play to their respective roles, achieve better modification of polypropylene, and reduce costs.
[0090] In some embodiments, the volume ratio of solvent to non-solvent is 4–9:1–6. Preferably, in some embodiments, the volume ratio of solvent to non-solvent is 5–6:4–5. More preferably, in some embodiments, the volume ratio of solvent to non-solvent is 6:4. For example, the volume ratios of solvent to non-solvent are 9:1, 8:2, 7:3, 6:4, 5:5, 4:6, etc.
[0091] This application conducted several gradient experiments on the volume ratio of solvent and non-solvent in its embodiments. The results show that during electrospinning, the porosity of the fiber membrane can be adjusted by regulating the volume ratio of solvent and non-solvent. In other words, the ratio of solvent to non-solvent has a certain influence on the porosity of the obtained modified polypropylene membrane. Experiments have shown that controlling the volume ratio of solvent to non-solvent within the above-mentioned range helps to ensure that the porosity of the obtained modified polypropylene membrane is within a suitable range, enabling the formation of a rich porous structure on the surface of the fiber membrane, which can improve the physical properties of the fiber membrane, such as tensile strength, peel strength, and puncture strength. In particular, a solvent-to-non-solvent volume ratio of 6:4 yields even better results.
[0092] In some embodiments, the difference between the saturated vapor pressure of the solvent and the saturated vapor pressure of the non-solvent at the same temperature is not less than 500 Pa. In some embodiments, the difference between the saturated vapor pressure of the solvent and the non-solvent at the same temperature is not less than 800 Pa. In some embodiments, the difference between the saturated vapor pressure of the solvent and the non-solvent at the same temperature is not less than 1000 Pa. No upper limit is imposed on the difference between the saturated vapor pressures of the solvent and the non-solvent. Furthermore, this embodiment does not limit the specific values of the saturated vapor pressures of the solvent and the non-solvent, as long as the difference between their saturated vapor pressures meets a certain range, it is not intended to limit the purpose of this application.
[0093] The selected solvent and non-solvent need to have different saturated vapor pressures so that they evaporate at different rates during electrospinning, allowing phase separation to occur and forming a porous cross-linked network, which can then be used to control the porosity of the resulting fiber membrane.
[0094] In some embodiments, the solvent includes at least one of methanol, ethanol, isopropanol, or butanol. For example, the solvent can be methanol, ethanol, isopropanol, butanol, or any combination of two or more of the above substances. Preferably, methanol is chosen as the solvent because it has a simple structure and is more effective when applied to the electrospinning solution of this application, making it easier to adjust the porosity of the resulting fiber membrane.
[0095] In some embodiments, the non-solvent includes at least one of toluene, o-xylene, p-xylene, m-xylene, or nitrobenzene. For example, the non-solvent can be toluene, o-xylene, p-xylene, m-xylene, nitrobenzene, or any combination of two or more of the above substances. Preferably, toluene is chosen as the non-solvent because it has a simple structure and is more effective when applied to the electrospinning solution of this application, making it easier to adjust the porosity of the resulting fiber membrane.
[0096] Furthermore, in other embodiments, the solvents and non-solvents are not limited to the types listed above. When a certain range of saturated vapor pressure difference is met, and when used in combination with polyacrylic acid and polyvinyl alcohol, other types of solvents and non-solvents may be used, which will not be described in detail here.
[0097] In some embodiments, polypropylene, polyvinyl alcohol, polyacrylic acid and solvent are mixed evenly, then inorganic nano-oxide is added, and then the temperature is raised to 30℃~50℃ (e.g. 30℃, 35℃, 40℃, 50℃, etc.), then non-solvent is added, and the mixture is stirred for 1h~3h (e.g. 1h, 2h, 3h, etc.) until it is evenly mixed to obtain a spinning solution.
[0098] In some embodiments, the operating conditions for electrospinning include: a distance of 13cm to 16cm between the needle and the receiver (e.g., 13cm, 14cm, 15cm, 16cm, etc., preferably 15cm); a voltage of 10 to 15kV (e.g., 10kV, 11kV, 12kV, 13kV, 14kV, 15kV, etc.); an ambient temperature of 20±5℃; and an air humidity of 30±3%. Further, the ambient temperature can be 20±1℃, and the air humidity can be 30±2%.
[0099] In some embodiments, after preparing the modified polypropylene membrane by electrospinning the spinning solution, the process further includes: heat-treating the modified polypropylene membrane by annealing it under vacuum at 70°C to 80°C for 12 to 18 hours. Heat treatment of the modified polypropylene membrane can enhance the toughness of the fiber membrane.
[0100] In some specific embodiments, the preparation of the modified polypropylene film includes the following steps:
[0101] S100, Preparation of spinning solution:
[0102] Polypropylene, polyvinyl alcohol, and polyacrylic acid are added to a solvent in a certain proportion and mixed evenly. While magnetically stirring at room temperature, inorganic nano-oxides can be added until completely dissolved. The temperature is then raised to 30℃~50℃, and stirring continues before adding a non-solvent. The mixture is stirred for 1h~3h to obtain a spinning solution. The mass ratio of polypropylene, polyvinyl alcohol, polyacrylic acid, and inorganic nano-oxides is (400~600):(100~300):(200~400):(10~30); the mass ratio of polypropylene to solvent is (400~600) mg:(10~30) mL; and the volume ratio of solvent to non-solvent is 4~9:1~6. The particle size of the inorganic nano-oxides is 5nm~100nm.
[0103] The above process is illustrated using silica particles as an example of the added inorganic nano-oxide. Silica has a three-dimensional network structure based on silicon-oxygen tetrahedra. In its crystal structure, the four valence electrons of silicon atoms form four covalent bonds with four oxygen atoms. The Si atom is located at the center of the tetrahedron, and the O atom is located at the vertices of the tetrahedron. This inorganic nano-oxide, such as silica particles, possesses strong heat resistance and hardness. When doped into fiber membranes, it connects with the fiber membrane through ester groups and hydrogen bonds, thus modifying the fiber membrane and effectively improving its high-temperature resistance and puncture strength. This is beneficial for improving the mechanical properties of the modified polypropylene membrane. Furthermore, the oxygen atoms on the silica surface readily react with water molecules to generate hydroxyl groups, i.e., O... 2- +H₂O=2OH - This is more conducive to the electroplating of metal ions such as copper ions on modified polypropylene films.
[0104] Figure 2 The three-dimensional phase diagram of the PAA+PVA system, with methanol as the solvent and toluene as the non-solvent, is shown, as follows. Figure 2As shown, the ratio of solvent to non-solvent can adjust the porosity of the fiber membrane, based on the three-dimensional phase diagram and mechanistic explanation. In this step, excess polyacrylic acid (PAA) and silica can be directly anchored through ester groups and hydrogen bonds, further enhancing the effective distribution of silica (SiO2) in the mixture of polypropylene (PP), polyvinyl alcohol (PVA), and polyacrylic acid (PAA). The relevant reactions are shown below:
[0105]
[0106] S200, Preparation of modified polypropylene membrane (porous fiber membrane):
[0107] The spinning solution obtained in step S100 is transferred to a syringe. After assembling the electrospinning apparatus, the needle is aligned with the center of the receiving drum, and aluminum foil is used for receiving. The distance from the needle tip to the current collector (i.e., the distance between the needle tip and the receiver) and the voltage are set to 13-16 cm (e.g., 15 cm) and 10-15 kV, respectively. The electrospinning experiment is conducted at room temperature (20±1℃) and relative humidity of 30±3%. After preparation, the obtained porous fiber membrane, i.e., the modified polypropylene membrane, is peeled off from the aluminum foil and then annealed in a vacuum environment at 70-80℃ for 12-18 hours to enhance the toughness of the fiber membrane. The modified polypropylene membrane obtained in this way can be used in secondary batteries such as lithium-ion batteries.
[0108] SEM images of the prepared modified polypropylene membrane are shown below. Figure 3 As shown, from Figure 3 As can be seen, the modified polypropylene membrane is a porous membrane with a porous structure.
[0109] The formation mechanism of pores in modified polypropylene membranes is explained as follows:
[0110] During electrospinning, the electrostatic repulsion of the fiber surface charges causes significant elongation of the spinning jet, resulting in a rapid increase in the jet surface area within milliseconds. This greatly accelerates the simultaneous evaporation of both solvent and non-solvent. Since the vapor pressure of methanol is much higher than that of toluene, the increased non-solvent fraction destabilizes the jet composition. Therefore, phase separation occurs during electrospinning. Figure 2As shown, the entire system can be divided into three states: steady (I), metastable (II), and unstable (III). The unstable and metastable states are separated by a double-nodal line (IV). Liquid-liquid separation plays a crucial role in non-solvent-induced phase separation; once the system components cross the double-nodal line, separation begins. Based on the principle that multiple substances can maintain phase equilibrium under the same environment, adjusting the solvent-to-solvent ratio allows polymerization to proceed in the unstable phase region. Under non-solvent induction (for example, toluene evaporates before methanol), a porous cross-linked network forms on the PAA and PVA surfaces in the unstable phase region. According to this principle, a strong phase separation process occurs when the solvent-to-solvent volume ratio is 6:4, resulting in a rich porous structure on the PAA-PVA surface.
[0111] Furthermore, after preparing the modified polypropylene membrane, a metal layer is prepared to obtain the composite current collector. For example, when the metal layer is a copper layer, the preparation process can be as follows:
[0112] Using the principle of an electrolytic cell, the modified polypropylene film obtained above was used as the working electrode, and a platinum sheet and an Ag / AgCl electrode were used as the counter electrode and reference electrode, respectively. The film was immersed in a 0.5 mol / L copper sulfate solution containing sulfuric acid. Electrodeposition was performed for 300–1000 s at a constant potential of -1.1 V (relative to the Ag / AgCl electrode) to obtain a metal layer, i.e., a copper layer, on the surface of the modified polypropylene film. After slight rinsing with anhydrous ethanol, the surface was vacuum dried at 35°C for 12 h to obtain a composite current collector. In this composite current collector, the metal layer is a Cu layer, and the volume ratio of solvent to non-solvent is 6:4; therefore, this composite current collector can be denoted as Cu / PP-PVA-PAA-6:4. The electrodeposition method in the preparation process of this composite current collector is as follows: Figure 4 As shown.
[0113] It should be understood that the preparation of other types of metal layers follows the same principle as the preparation of the copper layer described above, and will not be described in detail here.
[0114] Therefore, based on the above, the composite current collector and its preparation method provided in this embodiment of the invention have hydrogen bonds formed by polyvinyl alcohol and polyacrylic acid on the modified polypropylene surface, which is more conducive to improving the bonding force with the copper layer; the synthesized polyvinyl alcohol and polyacrylic acid have strong adhesion, which is conducive to improving the adhesion force between the metal layer such as the copper layer and the modified polypropylene film, while improving the tensile strength of the composite current collector; the inorganic nano-oxides such as silica and polyvinyl alcohol contain a large number of hydroxyl groups on their surfaces, and polyacrylic acid contains more carboxyl groups, which is more conducive to the electroplating of metal ions on the modified polypropylene film layer; the dense porous structure formed on the porous film surface allows metal ions to be well anchored on its surface, further enhancing the peel strength of the metal film.
[0115] [Battery electrode plates]
[0116] In some embodiments, a battery electrode is provided, the battery electrode comprising a composite current collector and an active material layer stacked together, wherein the composite current collector is the composite current collector of the first aspect of the present invention or the composite current collector prepared according to the second aspect of the present invention.
[0117] Due to the use of the composite current collector in this embodiment of the invention, the battery electrode of this embodiment of the invention has high mechanical properties, while also having low weight and high electrochemical performance.
[0118] As an example, the provided battery electrode includes a composite current collector and an active material layer stacked together. The composite current collector has two opposing surfaces in its thickness direction. The active material layer is stacked on at least one surface of the composite current collector. For example, the active material layer may be stacked on one surface of the composite current collector, or the active material layer may be stacked on both surfaces of the composite current collector.
[0119] The battery electrode sheets in this embodiment of the invention can be used as any one or both of the positive and negative electrode sheets. That is, the composite current collector in this application embodiment can be applied to the negative electrode sheet, or it can also be applied to the positive electrode sheet.
[0120] When the battery electrode sheet in this embodiment of the invention is used as the positive electrode sheet, the active material layer is the positive active material layer, and the composite current collector is the positive current collector.
[0121] When the composite current collector is used as the positive electrode current collector, the metal layer may include one or more of aluminum, aluminum alloy, nickel, nickel alloy, titanium and silver, such as aluminum or aluminum alloy, wherein the weight percentage of aluminum in the aforementioned aluminum alloy is preferably 80 wt% or more, more preferably 90 wt% or more.
[0122] The aforementioned positive electrode active material layer can be made of positive electrode active materials known in the art that are capable of reversible ion insertion / deintercalation, and the present invention does not impose any restrictions.
[0123] For example, the positive electrode active material for lithium-ion secondary batteries can be one or more of lithium transition metal composite oxides, or composite oxides obtained by adding other transition metals, non-transition metals, or non-metals to lithium transition metal composite oxides. For instance, the positive electrode active material can be selected from at least one of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (ternary material), lithium nickel cobalt aluminum oxide, and lithium phosphates with an olivine structure.
[0124] Optionally, the positive electrode active material layer may further include a positive electrode binder. The embodiments of the present invention do not limit the type of positive electrode binder. As an example, the positive electrode binder may be one or more of the following: polyvinylidene fluoride (PVDF), styrene-butadiene rubber (SBR), waterborne acrylic resin, carboxymethyl cellulose (CMC), polytetrafluoroethylene (PTFE), ethylene-vinyl acetate copolymer (EVA), polyvinyl alcohol (PVA), and polyvinyl butyral (PVB).
[0125] Optionally, the positive electrode active material layer may also include a conductive agent, and the embodiments of the present invention do not limit the type of conductive agent. As an example, the conductive agent may be one or more of conductive graphite, acetylene black, carbon black, Ketjen black, carbon nanotubes, graphene, or carbon nanofibers.
[0126] When the battery electrode sheet in this embodiment of the invention is used as the negative electrode sheet, the active material layer is the negative active material layer, and the composite current collector is the negative current collector.
[0127] When the composite current collector is used as the negative electrode current collector, the metal layer may include one or more of copper, copper alloy, nickel, nickel alloy, titanium and silver, such as copper or copper alloy, wherein the weight percentage of copper in the aforementioned copper alloy is preferably 80 wt% or more, more preferably 90 wt% or more.
[0128] The aforementioned negative electrode active material layer can be made of negative electrode active materials known in the art that are capable of reversible ion insertion / extraction, and the present invention does not impose any restrictions.
[0129] For example, the negative electrode active material for lithium-ion secondary batteries can be one or more of the following: graphite (including natural graphite, artificial graphite, etc.), mesophase micro carbon spheres, hard carbon, soft carbon, silicon-based materials, metallic lithium, spinel-structured lithium titanate, and Li-Al alloys.
[0130] Optionally, the negative electrode active material layer may also include a conductive agent, and the present invention does not limit the type of conductive agent. As an example, the conductive agent may be one or more of graphite, superconducting carbon, acetylene black, carbon black, Ketjen black, carbon nanotubes, graphene, and carbon nanofibers.
[0131] Optionally, the negative electrode active material layer may also include a binder, and the present invention does not limit the type of binder. As an example, the binder is one or more of carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR), waterborne acrylic resin, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-vinyl acetate copolymer (EVA), polyvinyl alcohol (PVA), etc.
[0132] The aforementioned battery electrode can be prepared using conventional methods in the art, such as coating. As an example, the active material, along with optional conductive agents and binders, is dispersed in a solvent, such as NMP or deionized water, to form a uniform electrode slurry. This electrode slurry is then coated onto a composite current collector, and after drying and other processes, the battery electrode is obtained.
[0133] [Battery]
[0134] In some embodiments, a battery is provided, including a positive electrode, a negative electrode, a separator, and an electrolyte. The positive electrode includes a positive current collector and a positive active material layer disposed on the positive current collector. The negative electrode includes a negative current collector and a negative active material layer disposed on the negative current collector. The positive current collector and / or the negative current collector is the aforementioned composite current collector, or a composite current collector prepared by the method described above. That is, the above-mentioned positive electrode and / or negative electrode is the battery electrode of the third aspect of the present invention. The description of the positive and negative electrode can be referred to the foregoing description of battery electrodes, and will not be repeated here.
[0135] The batteries mentioned above can be lithium-ion secondary batteries, lithium primary batteries, sodium-ion batteries, magnesium-ion batteries, etc., but are not limited to these.
[0136] In the aforementioned battery, the electrolyte may include an organic solvent, an electrolyte salt, and additives. The organic solvent serves as a medium for transporting ions in the electrochemical reaction and can be any organic solvent in the art. The electrolyte salt serves as a source of ions and can be any electrolyte salt in the art. The additives can also be any additives known in the art, and this application does not limit their use.
[0137] As an example, the organic solvent can be an ester solvent, such as at least one of ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), propylene carbonate (PC), methyl ethyl carbonate (EMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butenyl carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), ethyl acetate (EA), methyl acetate (MA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), methyl propionate (MB), propyl propionate (PP), ethyl butyrate (EB), etc., preferably a combination of two or more of the above substances.
[0138] As an example, electrolyte salts used in lithium-ion secondary batteries can be LiPF6 (lithium hexafluorophosphate), LiBF4 (lithium tetrafluoroborate), LiClO4 (lithium perchlorate), etc.
[0139] In the aforementioned battery, a separator is disposed between the positive and negative electrodes, serving as a barrier. This invention does not impose any particular limitation on the type of separator; any known porous separator with good chemical and mechanical stability can be used, such as glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film. When the separator is a multi-layer composite film, the materials of each layer can be the same or different.
[0140] The battery can be manufactured using methods known in the art. As an example,
[0141] The positive electrode, separator, and negative electrode are stacked in sequence, with the separator acting as a separator between the positive and negative electrodes to obtain the battery cell. Alternatively, the battery cell can be obtained by winding. The battery cell is then placed in a packaging shell and subjected to processes such as drying, electrolyte injection, encapsulation, formation, and capacity testing to prepare the battery.
[0142] Example
[0143] The following examples describe the disclosure of this invention in more detail. These examples are merely illustrative, as various modifications and variations will be apparent to those skilled in the art within the scope of this disclosure. Unless otherwise stated, all reagents used in the examples are commercially available or synthesized using conventional methods and can be used directly without further processing, as are the instruments used in the examples.
[0144] Example 1
[0145] Preparation of composite current collectors:
[0146] S100: Add 500 mg of polypropylene, 200 mg of polyvinyl alcohol, and 300 mg of polyacrylic acid to 12 mL of methanol solvent and mix thoroughly. While magnetically stirring at room temperature, add 20 mg of nano-silica with a particle size of 10-20 nm until completely dissolved. Then, raise the temperature to 40 °C, continue stirring, and add non-solvent toluene. Stir for 2 hours to mix thoroughly to obtain the spinning solution. The volume ratio of solvent to non-solvent is 6:4.
[0147] S200: Transfer the spinning solution obtained in step S100 into a syringe. After assembling the electrospinning apparatus, align the needle with the center of the receiving drum, and use aluminum foil for receiving. The distance from the needle tip to the collector (i.e., the distance between the needle tip and the receiver) and the voltage are set to 5 cm and 12 kV, respectively. The electrospinning experiment is conducted at room temperature (20±1℃) and relative humidity 30±3%. After preparation, peel the obtained porous fiber membrane, i.e., the modified polypropylene membrane, from the aluminum foil, and then anneal it in a vacuum environment at 75℃ for 15 h to obtain the modified polypropylene membrane.
[0148] S300: Using the principle of an electrolytic cell, the modified polypropylene membrane obtained in step S200 is used as the working electrode, and the platinum sheet and Ag / AgCl electrode are used as the counter electrode and reference electrode, respectively. The membrane is immersed in a 0.5 mol / L copper sulfate solution containing sulfuric acid and electrodeposited for 600 s at a constant potential of -1.1 V (relative to the Ag / AgCl electrode) to obtain a metal layer, namely a copper layer, on the surface of the modified polypropylene membrane. After slightly rinsing the surface with anhydrous ethanol, the membrane is vacuum dried at 35°C for 12 h to obtain a composite current collector.
[0149] Example 2
[0150] The preparation of the composite current collector is basically the same as in Example 1, except that the volume ratio of solvent to non-solvent is 9:1.
[0151] Example 3
[0152] The preparation of the composite current collector is basically the same as in Example 1, except that the volume ratio of solvent to non-solvent is 8:2.
[0153] Example 4
[0154] The preparation of the composite current collector is basically the same as in Example 1, except that the volume ratio of solvent to non-solvent is 7:3.
[0155] Example 5
[0156] The preparation of the composite current collector is basically the same as in Example 1, except that the volume ratio of solvent to non-solvent is 5:5.
[0157] Example 6
[0158] The preparation of the composite current collector is basically the same as in Example 1, except that the volume ratio of solvent to non-solvent is 4:6.
[0159] Example 7
[0160] The preparation of the composite current collector is basically the same as in Example 1, except that the mass ratio of polypropylene, polyvinyl alcohol, polyacrylic acid and inorganic nano-oxide is 400:100:200:10.
[0161] Example 8
[0162] The preparation of the composite current collector is basically the same as in Example 1, except that the mass ratio of polypropylene, polyvinyl alcohol, polyacrylic acid and inorganic nano-oxide is 600:300:400:30.
[0163] Example 9
[0164] The preparation of the composite current collector is basically the same as in Example 1, except that the inorganic nano-oxide is zirconium oxide.
[0165] Example 10
[0166] The preparation of the composite current collector is basically the same as in Example 1, except that the solvent is isopropanol and the non-solvent is p-xylene.
[0167] Comparative Example 1
[0168] In this comparative example, an existing copper foil current collector is used.
[0169] Comparative Example 2
[0170] In this comparative example, a composite current collector formed by combining existing polypropylene and copper foil is used.
[0171] Comparative Example 3
[0172] The difference between the composite current collector in this comparative example and the composite current collector in Example 1 is that polyvinyl alcohol was not added in this comparative example.
[0173] Comparative Example 4
[0174] The difference between the composite current collector in this comparative example and the composite current collector in Example 1 is that polyacrylic acid was not added in this comparative example.
[0175] Preparation of negative electrode sheet
[0176] The negative electrode active material, binder and conductive agent are mixed in the following mass ratio: 95.4 wt% graphite, 1.9 wt% binder, 1.1 wt% CMC (sodium carboxymethyl cellulose) and 1.6 wt% SP (conductive carbon black) to obtain a mixed material. The mixed material is then thoroughly stirred in deionized water to obtain the corresponding negative electrode active slurry.
[0177] The negative electrode active slurry was homogenized and coated onto the composite current collectors of Examples 1-10 and Comparative Examples 1-4, respectively, to obtain a thickness of 149 μm and a one-sided density of 0.012 g / cm³. 2 The negative electrode slurry coating is dried and pressed to obtain the negative electrode sheet.
[0178] Preparation of positive electrode sheet
[0179] The positive electrode active material, binder, and conductive agent are mixed according to 96.2 wt% LiNi 0.6 Co 0.2 Mn 0.2 O2 (ternary material), 1 wt% PVDF, 2 wt% SP, and 0.8 wt% CNT (carbon nanotubes) were mixed to obtain a mixed material. This mixed material was then thoroughly stirred in NMP to obtain the corresponding positive electrode active slurry. The positive electrode slurry was coated onto a positive electrode current collector aluminum foil to obtain a thickness of 125 μm and a one-sided density of 0.02 g / cm³. 2 The positive electrode slurry coating is dried and pressed to obtain the positive electrode sheet.
[0180] Preparation of electrolyte
[0181] Ethylene carbonate (EC), dimethyl carbonate (DMC), and diethyl carbonate (DEC) were mixed in a volume ratio of 1:1:1 to obtain a mixed organic solvent. Then, fully dried lithium salt LiPF6 was dissolved in the mixed organic solvent at a ratio of 1 mol / L to prepare an electrolyte.
[0182] Preparation of lithium-ion batteries
[0183] The negative electrode, separator (8μm polypropylene separator), and positive electrode are stacked in sequence and then wound to obtain the cell. The cell is then installed in the battery case and undergoes processes such as drying, electrolyte injection, encapsulation, formation, and capacity testing to obtain a lithium-ion battery.
[0184] Performance testing
[0185] 1. Testing of current collectors
[0186] The composite current collectors obtained in the above embodiments and comparative examples were subjected to tensile strength, puncture strength, and peel strength (adhesion) tests; the modified polypropylene membranes in the above embodiments and comparative examples were subjected to porosity tests.
[0187] (1) Tensile strength test: The specimen was placed in the clamps of a universal tensile testing machine, and the tensile strength of the diaphragm was tested directly using the universal tensile testing machine. Specific method: The composite current collector test samples of each embodiment and comparative example were cut into strips 15mm wide and 200mm long. The top and bottom ends of the test sample were clamped on the tensile testing machine, the tensile direction was 180°, the tensile speed was 250mm / min, and the gauge length of the specimen was 100mm. The tensile test was completed until the test sample broke. The tensile strength value of this experiment was obtained on the tensile testing machine. The test results are shown in Table 1.
[0188] (2) Puncture strength test: Using a diaphragm puncture testing machine, the composite current collector test samples of each embodiment and comparative example were cut into strips. The width of the strip composite current collector test sample must be greater than 100 mm. The 100 mm wide test piece was installed on the membrane fixing clamp, and then a steel needle with a diameter of 1 mm and a top radius of 0.5 mm was used to puncture the test piece at a speed of 50 mm / min. The load of the steel needle penetrating the test piece was read. The test results are shown in Table 1.
[0189] (3) Peel strength test: The adhesion between the modified polypropylene film and the metal layer in the composite current collector was tested. The composite current collector test samples of each embodiment and comparative example were cut to a certain width. The cut composite current collector test samples were pasted onto an iron plate with double-sided adhesive. A tensile testing machine was used to pull the sample upwards at a speed of 50 mm / min, perpendicular to the ground at a horizontal angle of 180°. The peel strength, i.e., the adhesion force between the modified polypropylene film and the metal layer in the composite current collector, was calculated. The test results are shown in Table 1.
[0190] (4) Porosity: Cut the modified polypropylene film into rectangular samples. Measure the length (L), width (D), and thickness (H) using a micrometer. Weigh the samples using an analytical balance (m0). Place the cut samples into a container filled with the relevant liquid, ensuring complete immersion for at least 1 hour to allow for full absorption. After absorption, wipe the liquid off the sample surface with clean paper and press the sample approximately 3-5 times. Then, use clean paper to absorb the remaining liquid. Weigh the final sample using an analytical balance (m1). Calculate the porosity of the sample using the formula P = (m1 - m0) / (ρ * L * D * H). Note: ρ is the density of the liquid.
[0191] 2. Battery performance testing
[0192] (1) Cyclic performance test: At room temperature (25℃), with starting and stopping voltages of 2.8V and 4.35V respectively, the battery was charged at 0.5C to 4.35V, then charged at a constant voltage of 4.35V until the current decreased to 0.05C, then discharged at 0.5C to 2.8V, then charged at 0.5C to 4.35V again, then charged at a constant voltage of 4.35V until the current decreased to 0.05C, and finally discharged at 0.5C to 2.8V. The battery was cycled in this manner, and the capacity retention rate after 200 cycles was calculated. The test results are shown in Table 2.
[0193] (2) Energy density test: Lithium-ion batteries including the current collectors provided in the above embodiments and comparative examples were selected, charged at 0.33C to 4.35V, charged at 4.35V at constant voltage until the current decreased to 0.05C, and discharged at 0.33C at constant current to 2.8V. The resulting discharge capacity was recorded as Q, and the plateau voltage of the discharge curve was recorded as U. Based on the battery weight m, the energy density released by the lithium-ion battery cell was calculated using Q*U / m. The test results are shown in Table 2.
[0194] Test Results
[0195] Table 1. Performance test results of the current collectors in each embodiment and comparative example.
[0196] Group Porosity (%) Tensile strength (MPa) Puncture intensity (N) Peel strength (N / m) Example 1 85.62 288.25 4.45 64.6 Example 2 76.82 232.78 3.87 45.9 Example 3 77.63 269.86 4.03 51.3 Example 4 79.15 270.56 4.19 52.3 Example 5 80.28 273.26 4.26 55.6 Example 6 83.27 274.32 4.32 57.8 Example 7 83.58 280.38 4.36 41.5 Example 8 82.13 287.65 4.34 54.2 Example 9 85.56 288.13 4.43 64.4 Example 10 85.54 288.11 4.42 64.3 Comparative Example 1 / 282.92 / / Comparative Example 2 53.62 204.44 3.65 10.3 Comparative Example 3 82.65 278.62 4.25 42.3 Comparative Example 4 82.48 279.13 4.28 43.6
[0197] In Table 1, the porosity is characterized by tests performed on the modified polypropylene film before Cu electrodeposition.
[0198] As can be seen from the data in Table 1, compared with the current collectors provided in Comparative Examples 1 and 2, the composite current collectors provided in Examples 1-10 of this application have greater porosity, and their tensile strength, puncture strength, and peel strength are all improved to a certain extent. A comparative analysis of the examples with Comparative Examples 3 and 4 also shows that modifying polypropylene by using polyvinyl alcohol and polyacrylic acid in combination can achieve higher peel strength, which is more conducive to improving the adhesion between the metal layer and the modified polypropylene film layer.
[0199] Table 2 contains the electrochemical performance test results of the current collectors for each embodiment and comparative example of the lithium-ion batteries.
[0200]
[0201]
[0202] As can be seen from the data in Table 2, compared with the batteries using the current collectors provided in Comparative Examples 1 to 4, the batteries using the composite current collectors provided in Examples 1 to 10 of this application have higher energy density and stronger cycle performance.
[0203] The parts of this invention not described in detail are techniques known to those skilled in the art.
[0204] The basic principles of the present invention have been described above with reference to specific embodiments. However, it should be noted that the advantages, benefits, and effects mentioned in the present invention are merely examples and not limitations, and should not be considered as essential features of each embodiment of the present invention. Furthermore, the specific details disclosed above are for illustrative and facilitative purposes only, and are not limitations. These details do not limit the present invention to the necessity of employing the aforementioned specific details.
[0205] In the detailed description and claims, a list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms may mean any combination of the listed items. For example, if items A and B are listed, then the phrase "at least one of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, then the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may contain a single element or multiple elements. Item B may contain a single element or multiple elements. Item C may contain a single element or multiple elements.
[0206] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A composite current collector, characterized in that, It includes a modified polypropylene film and a metal layer disposed on at least one surface of the modified polypropylene film along its thickness direction. The modified polypropylene film is formed by modifying polypropylene with polyvinyl alcohol, polyacrylic acid and inorganic nano-oxides. The preparation steps of the modified polypropylene film specifically include: Polypropylene, polyvinyl alcohol, polyacrylic acid and solvent are mixed evenly, and then inorganic nano-oxides and non-solvent are added and mixed evenly to obtain a spinning solution; The modified polypropylene film was prepared by electrospinning the spinning solution. After preparing the modified polypropylene film by electrospinning the spinning solution, the method further includes: subjecting the modified polypropylene film to heat treatment, wherein the heat treatment is annealing at 70°C to 80°C in a vacuum environment for 12 to 18 hours. The solvent includes at least one of methanol, ethanol, isopropanol or butanol, and the non-solvent includes at least one of toluene, o-xylene, p-xylene, m-xylene or nitrobenzene, with a volume ratio of solvent to non-solvent of 4-9:1-6.
2. The composite current collector according to claim 1, characterized in that, The composite current collector satisfies at least one of the following characteristics (1) to (5): (1) The inorganic nano-oxides include at least one of silicon dioxide, aluminum oxide, zirconium oxide, zinc oxide, titanium oxide, calcium oxide, antimony pentoxide, magnesium oxide, nickel oxide, chromium oxide or cobalt oxide; (2) The particle size of the inorganic nano-oxide is 5 nm to 100 nm; (3) The material of the metal layer includes at least one of copper, copper alloy, aluminum, aluminum alloy, nickel, nickel alloy, titanium or silver; (4) The modified polypropylene film has the metal layer on both surfaces along its thickness direction; (5) The thickness of the metal layer is 0.5μm to 5μm, and the thickness of the modified polypropylene film is 1μm to 10μm.
3. A method for preparing a composite current collector, characterized in that, Includes the following steps: A modified polypropylene film is provided, wherein the modified polypropylene film is formed by modifying polypropylene with polyvinyl alcohol, polyacrylic acid and inorganic nano-oxides; Metal is electrodeposited on the surface of the modified polypropylene film to form a metal layer on the surface of the modified polypropylene film, thereby obtaining a composite current collector comprising a modified polypropylene film and a metal layer. The step of providing the modified polypropylene film specifically includes: Polypropylene, polyvinyl alcohol, polyacrylic acid and solvent are mixed evenly, and then inorganic nano-oxides and non-solvent are added and mixed evenly to obtain a spinning solution; The modified polypropylene film was prepared by electrospinning the spinning solution. The volume ratio of the solvent to the non-solvent is 4-9:1-6; The solvent includes at least one of methanol, ethanol, isopropanol, or butanol; The non-solvent includes at least one of toluene, o-xylene, p-xylene, m-xylene, or nitrobenzene; After preparing the modified polypropylene film by electrospinning the spinning solution, the method further includes: subjecting the modified polypropylene film to heat treatment, wherein the heat treatment is annealing at 70℃~80℃ in a vacuum environment for 12h~18h.
4. The method for preparing the composite current collector according to claim 3, characterized in that, The step of providing the modified polypropylene film satisfies at least one of the following features (1) to (3): (1) The mass ratio of the polypropylene, the polyvinyl alcohol, the polyacrylic acid and the inorganic nano-oxide is (400-600):(100-300):(200-400):(10-30); (2) The mass ratio of the polypropylene to the volume ratio of the solvent is (400-600) mg: (10-30) mL; (3) The difference between the saturated vapor pressure of the solvent and the saturated vapor pressure of the non-solvent at the same temperature is not less than 500 Pa.
5. The method for preparing the composite current collector according to claim 3, characterized in that, The volume ratio of the solvent to the non-solvent is 5-6:4-5.
6. The method for preparing the composite current collector according to claim 3, characterized in that, After the polypropylene, polyvinyl alcohol, polyacrylic acid and solvent are mixed evenly, inorganic nano-oxide is added, and then the temperature is raised to 30℃~50℃. Then, a non-solvent is added and stirred for 1h~3h to mix evenly to obtain the spinning solution.
7. The method for preparing the composite current collector according to any one of claims 3 to 6, characterized in that, The electrospinning operating conditions include: the distance between the needle and the receiver is 13cm to 16cm, the voltage is set to 10 to 15KV, the ambient temperature is 20±5℃, and the air humidity is 30±3%.
8. A battery electrode, characterized in that, It includes the composite current collector as described in any one of claims 1 to 2, or the composite current collector prepared by the method as described in any one of claims 3 to 7, and an active material layer disposed in the composite current collector.
9. A battery, comprising a positive electrode, a negative electrode, a separator, and an electrolyte, wherein the positive electrode comprises a positive current collector and a positive active material layer disposed on the positive current collector, and the negative electrode comprises a negative current collector and a negative active material layer disposed on the negative current collector; characterized in that, The positive current collector and / or the negative current collector are composite current collectors as described in any one of claims 1 to 2, or composite current collectors prepared by the method described in any one of claims 3 to 7.
Citation Information
Patent Citations
Electrode pole sheet and electrochemical device
CN110660957A
Composite current collector, preparation method thereof and lithium ion battery
CN115663200A