Isolation film, method for manufacturing the same, and battery

By forming a polyurethane modified layer on a polypropylene substrate and covering it with MOF material, the thermal stability and mechanical strength issues of the polyolefin separator are solved, the adhesion between the separator and the electrode is enhanced, the internal resistance of the battery is reduced, and the overall performance of the battery is improved.

CN117832763BActive Publication Date: 2026-11-10JIANGSU ZENIO NEW ENERGY BATTERY TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311861708.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-29
Publication Date
2026-11-10
Estimated Expiration
2043-12-29

Smart Images

  • Figure HDA0004693682060000011
    Figure HDA0004693682060000011
  • Figure HDA0004693682060000012
    Figure HDA0004693682060000012
Patent Text Reader

Abstract

The present application relates to the technical field of battery, in particular to a separator and a preparation method thereof and a battery, which provides a separator, comprising a substrate and a modified layer formed on the surface of the substrate; wherein the material of the substrate comprises polyurethane modified polypropylene; the material of the modified layer comprises MOF material. The present application also provides a preparation method of the separator, comprising the following steps: reacting polypropylene containing hydroxyl with raw materials for synthesizing polyurethane to obtain polyurethane modified polypropylene; reacting the polyurethane modified polypropylene with raw materials for synthesizing MOF material to form a modified layer on the surface of the polyurethane modified polypropylene, wherein the material of the modified layer comprises MOF material, thereby obtaining the separator. The present application can increase the adhesion between the separator and the surface of the pole piece, reduce the lithium ion transmission path and lower the internal resistance of the battery while enhancing the hardness of the separator and increasing the safety.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of battery technology, and more specifically, to a separator, a method for preparing the same, and a battery. Background Technology

[0002] Lithium-ion batteries are widely used in all aspects of human society, including clothing, food, housing, and transportation, due to their advantages such as high specific energy, long cycle life, no memory effect, and low self-discharge rate. Battery safety depends on the electrode, electrolyte, separator (isolation membrane) materials, battery structure, and protection system. The separator's main function is to prevent physical contact between the anode and cathode electrodes, and it also serves as a lithium-ion transport channel within the battery.

[0003] Currently, commercially available separators are mainly polyolefin separators such as polyethylene (PE) and polypropylene (PP). However, existing polyolefin separators still have some problems, such as: (1) polyolefins have low melting points, resulting in poor thermal dimensional stability of the separators, which poses a risk to the safety of batteries at high temperatures; (2) polyolefin materials have low polarity and are intrinsically hydrophobic, resulting in poor affinity with highly polar electrolytes; (3) during the manufacturing process of lithium-ion batteries, there are certain gaps between the polyolefin separator and the electrode, which leads to an increase in the ion transport path and further increases the internal resistance of the battery. The stability and mechanical strength of porous separators are important factors affecting battery safety, and the contact between porous separators and electrodes can also affect the internal resistance of the battery.

[0004] In related technologies, to improve the aforementioned problems, methods such as coating the membrane surface with adhesives (PVDF, etc.) and ceramic particles are commonly used to improve the polyolefin membrane. The purpose of adhesive coating is to ensure sufficient contact between the membrane and the electrode, while the purpose of applying ceramic particles is to increase the membrane's puncture strength and high-temperature resistance. However, after coating the membrane surface with an adhesive layer and ceramic particles, these layers cover some of the surface voids, thus blocking lithium-ion channels, reducing the membrane's ion conductivity, increasing the battery's internal resistance, and consequently reducing the performance of the lithium-ion battery. Furthermore, the coating process requires specialized equipment, increasing energy consumption and cost. Summary of the Invention

[0005] In view of this, the present invention aims to at least partially solve one of the technical problems in the related art. To this end, the present invention provides a separator, a method for preparing the same, and a battery, which can enhance the hardness and adhesion of the separator, give the surface of the separator a rich porous structure, and reduce the internal impedance of the battery.

[0006] To solve the above-mentioned technical problems, this application is implemented as follows:

[0007] According to one aspect of this application, an embodiment of this application provides a separating membrane, the separating membrane comprising a substrate and a modified layer formed on the surface of the substrate;

[0008] The material of the substrate includes polyurethane-modified polypropylene;

[0009] The modified layer is made of MOF material.

[0010] In addition, the separator membrane according to this application may also have the following additional technical features:

[0011] In some of these embodiments, the separator membrane satisfies at least one of the following conditions (1) to (4):

[0012] (1) The MOF material includes at least one of ZIF-8, ZIF-7, ZIF-67 or ZIF-90;

[0013] (2) The mass ratio of the MOF material to the substrate is 1:80 to 1:40;

[0014] (3) The particle size of the MOF material is 50nm to 300nm;

[0015] (4) The thickness of the modified layer is 600nm to 1000nm.

[0016] According to another aspect of this application, embodiments of this application provide a method for preparing a separating membrane, the method comprising the following steps:

[0017] Polypropylene containing hydroxyl groups is reacted with raw materials used to synthesize polyurethane to obtain polyurethane-modified polypropylene.

[0018] The polyurethane-modified polypropylene is reacted with raw materials used to synthesize MOF materials to form a modified layer on the surface of the polyurethane-modified polypropylene. The material of the modified layer includes MOF materials, thereby obtaining the separator membrane.

[0019] In some embodiments, the preparation of the hydroxyl-containing polypropylene includes:

[0020] Polypropylene, a first reactant, a second reactant, and a first solvent are mixed to obtain a mixture;

[0021] The mixture is heated under reflux to obtain a dehydrogenated product on the polypropylene;

[0022] Then water, oxidant, and hydroxide are added to carry out an oxidation reaction, resulting in polypropylene containing hydroxyl groups.

[0023] In some of these embodiments, the preparation of the hydroxyl-containing polypropylene satisfies at least one of the following conditions (1) to (10):

[0024] (1) The first reactant includes at least one of sodium borohydride, potassium borohydride, calcium borohydride, magnesium borohydride or lithium borohydride;

[0025] (2) The second reactant includes at least one of ammonium sulfate, ammonium nitrate, ammonium chloride, ammonium bisulfate, ammonium fluoride, ammonium carbonate, or ammonium bicarbonate;

[0026] (3) The first solvent includes at least one of tetrahydrofuran, acetonitrile, formamide, acetone or propanol;

[0027] (4) The oxidant includes at least one of hydrogen peroxide, sodium hypochlorite, or sodium peroxide; the hydroxide includes at least one of sodium hydroxide, potassium hydroxide, lithium hydroxide, rubidium hydroxide, or cesium hydroxide.

[0028] (5) The mass ratio of the polypropylene, the first reactant, and the second reactant is 200:(2-6):(4-8);

[0029] (6) The temperature of the heating reflux is 80℃~100℃, and the reflux time is 8h~16h;

[0030] (7) The temperature of the oxidation reaction is 38℃~50℃;

[0031] (8) After adding water, oxidant and hydroxide for oxidation reaction, the process also includes filtration, washing and drying steps;

[0032] (9) The washing process includes washing with hot water first, and then washing with alcohol solvents and / or ketone solvents.

[0033] (10) The drying temperature is 40℃~80℃ and the drying time is 8h~16h.

[0034] In some embodiments, the step of reacting hydroxyl-containing polypropylene with raw materials used to synthesize polyurethane specifically includes:

[0035] A mixture is obtained by mixing polypropylene containing hydroxyl groups, isocyanate raw materials, and a second solvent.

[0036] The mixture is heated under reflux, and then polytetrahydrofuran raw materials and a second solvent are added to carry out a polymerization reaction to obtain a precipitate.

[0037] The precipitate was dried to obtain polyurethane-modified polypropylene.

[0038] In some of these embodiments, the step of reacting the hydroxyl-containing polypropylene with the raw material for synthesizing polyurethane satisfies at least one of the following conditions (1) to (7):

[0039] (1) The isocyanate raw materials include at least one of toluene diisocyanate, diphenylmethane diisocyanate or naphthalene 1,5-diisocyanate;

[0040] (2) The polytetrahydrofuran raw material includes at least one of polytetrahydrofuran, poly-2-methyltetrahydrofuran or poly-2-ethyltetrahydrofuran;

[0041] (3) The second solvent includes at least one of toluene, xylene or benzene;

[0042] (4) The mass ratio of the hydroxyl-containing polypropylene to the isocyanate raw material is 5-10:0.5-1;

[0043] (5) The mass ratio of the isocyanate raw material to the polytetrahydrofuran raw material is 0.5-1:1-5;

[0044] (6) The temperature of the heating reflux is 100℃~120℃, and the reflux time is 4h~10h;

[0045] (7) The drying temperature is 40℃~80℃ and the drying time is 10h~16h.

[0046] In some embodiments, the MOF material includes at least one of ZIF-8, ZIF-7, ZIF-67, or ZIF-90.

[0047] In some embodiments, the MOF material is ZIF-8, and the step of reacting the polyurethane-modified polypropylene with the raw materials used to synthesize the MOF material specifically includes:

[0048] Zinc nitrate hexahydrate and imidazole raw materials were dissolved in a third solvent to obtain zinc nitrate hexahydrate solution and imidazole raw material solution, respectively.

[0049] The polyurethane-modified polypropylene, zinc nitrate hexahydrate solution, and imidazole raw material solution are mixed and reacted under stirring conditions to form a modified layer on the surface of the polyurethane-modified polypropylene.

[0050] In some of these embodiments, the step of reacting the polyurethane-modified polypropylene with the raw materials used to synthesize MOF materials satisfies at least one of the following conditions (1) to (6):

[0051] (1) The MOF material is ZIF-8, the imidazole raw material includes 2-methylimidazolium, and the third solvent includes methanol;

[0052] (2) The MOF material is ZIF-7, the imidazole raw material includes benzimidazole, and the third solvent includes dimethylformamide;

[0053] (3) The MOF material is ZIF-90, the imidazole raw material includes imidazole-2-carboxaldehyde, and the third solvent includes dimethylformamide;

[0054] (4) The MOF material is ZIF-67, the zinc nitrate hexahydrate is replaced with cobalt nitrate hexahydrate, the imidazole raw material includes 2-methylimidazole, and the third solvent includes water;

[0055] (5) The mass ratio of zinc nitrate hexahydrate to imidazole raw material is 1-3:2-5;

[0056] (6) The stirring temperature is 20℃~40℃ and the stirring time is 20h~30h.

[0057] According to another aspect of this application, an embodiment of this application provides a battery including a positive electrode, a negative electrode, and a separator, wherein the separator is the aforementioned separator or a separator prepared according to the aforementioned method.

[0058] Implementing the technical solution of the present invention has at least the following beneficial effects:

[0059] In the embodiments of this application, the provided separator includes a substrate and a modified layer formed on the surface of the substrate. The substrate includes polyurethane-modified polypropylene. Since polyurethane has strong hardness and adhesive properties, using polyurethane-modified polypropylene as the substrate of the separator can enhance the hardness or puncture strength of the separator, as well as enhance the adhesion between the separator and the electrode surface. Meanwhile, the modified layer is made of MOF material. MOF is composed of metal ions and organic ligands, has abundant Lewis acid sites and highly ordered pores, and its porosity is adjustable. It can promote the shuttle of metal ions between the positive and negative electrodes, thereby helping to reduce the internal impedance of the battery and improve the first coulombic efficiency and cycle performance of the battery.

[0060] Additional aspects and advantages of this application will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of the invention. Attached Figure Description

[0061] Figure 1 The diagram shows a schematic representation of the relevant reaction equations involved in the preparation process of hydroxyl-containing polypropylene (PP-OH) according to some embodiments of the application.

[0062] Figure 2 The diagram shows a schematic representation of the relevant reaction equations involved in the preparation process of PP-PU according to some embodiments of the application. Detailed Implementation

[0063] The present application will be further described below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the present application.

[0064] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges or individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0065] The following detailed description discloses embodiments of the separator, its preparation method, and the battery described in this application. However, unnecessary details may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of essentially the same structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art.

[0066] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.

[0067] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.

[0068] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0069] Unless otherwise specified, the terms "comprising" and "including" as used in this application can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other components not listed may also be included, or that only the listed components may be included.

[0070] Unless otherwise stated, the values ​​of the parameters mentioned in this application can be determined using various testing methods commonly used in the art, such as the testing methods given in the embodiments of this application.

[0071] Typically, a secondary battery consists of electrode components and an electrolyte. The electrode components include a positive electrode, a negative electrode, and a separator. The separator, positioned between the positive and negative electrodes, primarily prevents short circuits between the two electrodes and allows active ions to pass freely, forming a closed circuit. With the increasing application and promotion of secondary batteries, the performance requirements are becoming more stringent. Optimizing components such as the separator helps to further enhance battery performance. However, existing polyolefin separators, such as those made of polyethylene and polypropylene, still have some shortcomings, such as poor thermal stability and mechanical strength, and require further improvement.

[0072] The inventors of this application made a surprising discovery during their research: While polyurethane (PU) is commonly used in the military and coating industries due to its high hardness and adhesive properties, its application in separators has been overlooked by those skilled in the art. Similarly, metal-organic frameworks (MOFs), being highly conductive porous materials, are frequently used in electrocatalysis and battery materials; their application in separators has also been neglected by those skilled in the art. Therefore, the inventors of this application, through extensive research, discovered that by compounding modified polypropylene (PP) with polyurethane (PU) to obtain PU-modified PP, the hardness or puncture strength of the separator can be enhanced (increasing safety), while simultaneously increasing the adhesion between the separator and the electrode surface (reducing lithium-ion transport pathways and lowering battery internal resistance). Furthermore, to reduce the separator's own resistance, MOF materials (such as ZIF-8) are synthesized on the surface of the PU-modified PP. The rich porous structure of MOF materials promotes the transport of metal ions such as lithium ions, and the strong conductivity of MOF materials like ZIF-8 further reduces the separator's own resistance, thereby further reducing battery internal resistance. Specific technical solutions are described below.

[0073] [Isolation membrane]

[0074] In some embodiments, this application provides a separating membrane, the separating membrane comprising a substrate and a modified layer formed on the surface of the substrate;

[0075] The substrate material includes polyurethane-modified polypropylene; the modified layer material includes MOF material.

[0076] The inventors of this application made an unexpected discovery during their research in Dali: by utilizing the strong hardness and adhesive properties of polyurethane, and using polyurethane-modified polypropylene as the substrate of the separator, the hardness or puncture strength of the separator can be enhanced, while the adhesion between the separator and the electrode surface can also be improved. Therefore, by enhancing the hardness or puncture strength of the separator, the safety of batteries using this separator can be improved; and by enhancing the adhesion between the separator and the electrode surface, the transport path of metal ions such as lithium ions can be reduced, thereby reducing the internal resistance of the battery.

[0077] Furthermore, by forming a modified MOF material layer on the surface of the substrate, the MOF, composed of metal ions and organic ligands, possesses abundant Lewis acid sites and highly ordered pores with adjustable porosity, which can promote the shuttle movement of metal ions such as lithium ions between the positive and negative electrodes, thereby helping to reduce the internal impedance of the battery. At the same time, since the MOF material has strong conductivity, it can reduce the self-resistance of the separator, thereby further reducing the internal resistance of the battery.

[0078] Furthermore, in some preferred embodiments of the present invention, hydroxylated polypropylene is reacted with polyurethane. The presence of numerous polar bonds (such as C=O) and hydrophilic groups (such as -OH, -COOH) on the interior and surface of the hydroxylated polypropylene and polyurethane can enhance the electrolyte absorption capacity of the separator, that is, improve the liquid absorption rate of the separator.

[0079] In summary, when the provided separator is applied in a secondary battery, the combination of polyurethane-modified polypropylene substrate and MOF material modified layer can reduce the battery's internal resistance, improve the battery's initial coulombic efficiency, and enhance the battery's cycle performance.

[0080] Through in-depth research, the inventors have discovered that, in addition to meeting the above-mentioned design conditions, the performance of the separator membrane can be further improved if it optionally meets one or more of the following conditions.

[0081] In some embodiments, the MOF material includes at least one of ZIF-8, ZIF-7, ZIF-67, or ZIF-90;

[0082] Optionally, the MOF material is ZIF-8, and the separator comprises a polyurethane-modified polypropylene substrate and ZIF-8 formed on the surface of the substrate.

[0083] Optionally, the MOF material is ZIF-7, and the separator comprises a polyurethane-modified polypropylene substrate and ZIF-7 formed on the surface of the substrate.

[0084] Optionally, the MOF material is ZIF-67, and the separator comprises a polyurethane-modified polypropylene substrate and ZIF-67 formed on the surface of the substrate.

[0085] Optionally, the MOF material is ZIF-90, and the separator comprises a polyurethane-modified polypropylene substrate and ZIF-90 formed on the surface of the substrate.

[0086] In addition, in other embodiments, the specific type of MOF material is not limited to the types listed above. Other types of MOF materials can also be used when the requirements of having abundant porous structure, strong conductivity, and being beneficial to improving battery performance are met. These will not be described in detail here.

[0087] The inventors of this application, through optimization of specific types of MOF materials, discovered that using the aforementioned MOF materials, such as ZIF-8, yields better application results, is more conducive to reducing battery internal resistance, and improves battery initial efficiency and cycle performance.

[0088] In some embodiments, the mass ratio of MOF material to substrate is 1:80 to 1:40. In some embodiments, the mass ratio of MOF material to substrate is 1:70 to 1:45. In some embodiments, the mass ratio of MOF material to substrate is 1:65 to 1:50. In some embodiments, the mass ratio of MOF material to substrate can be 1:80, 1:70, 1:65, 1:60, 1:55, 1:50, 1:45, 1:40, etc.

[0089] The MOF material content can be adjusted by changing the mass ratio of MOF material to substrate. If the MOF material content is too low, the resistivity of the separator will increase, and the reduced porosity will decrease the separator's liquid absorption capacity, thus increasing the battery's internal resistance and reducing its initial efficiency and cycle performance. Conversely, if the MOF material content is too high, some MOF material may agglomerate on the separator surface, clogging the pores and causing a decrease in liquid absorption, an increase in internal resistance, and a reduction in initial efficiency and cycle performance. Therefore, this application, by controlling the MOF material to substrate mass ratio within the range of 1:80 to 1:40, helps to reduce battery internal resistance and improve initial efficiency and cycle performance.

[0090] In some embodiments, the particle size of the MOF material is 50 nm to 300 nm. In some embodiments, the particle size of the MOF material is 80 nm to 200 nm. Exemplarily, the particle size of the MOF material can be 50 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, etc.

[0091] The selection of MOF material particle size is related to reactant concentration and reaction time. By keeping the MOF material particle size within the above range, it is helpful to make the MOF material's pore structure suitable, which is conducive to promoting lithium ion transport and reducing battery internal resistance.

[0092] In some embodiments, the thickness of the modified layer is 600 nm to 1000 nm. In some embodiments, the thickness of the modified layer is 650 nm to 900 nm. In some embodiments, the thickness of the modified layer is 700 nm to 800 nm. Exemplarily, the thickness of the modified layer can be 600 nm, 650 nm, 700 nm, 750 nm, 800 nm, 900 nm, 1000 nm, etc.

[0093] If the modified layer is too thick, it may increase the battery's internal resistance and reduce its initial efficiency and cycle performance; if the modified layer is too thin, its effect on reducing the battery's internal resistance is not significant. Therefore, the embodiments of this application, by controlling the thickness of the modified layer within the range of 600nm to 1000nm, help to reduce the battery's internal resistance and improve its initial efficiency and cycle performance.

[0094] [Preparation method of the separating membrane]

[0095] In some embodiments, a method for preparing a separating membrane is provided, the method comprising the following steps:

[0096] Polypropylene containing hydroxyl groups is reacted with raw materials used to synthesize polyurethane to obtain polyurethane-modified polypropylene.

[0097] Polyurethane-modified polypropylene is reacted with raw materials used to synthesize MOF materials to form a modified layer on the surface of the polyurethane-modified polypropylene. The modified layer includes MOF materials, resulting in a release membrane.

[0098] It should be understood that all the features and advantages described above regarding the "separation membrane" also apply to the "preparation method of the separation membrane," and will not be repeated here.

[0099] Therefore, by combining modified PP (polypropylene containing hydroxyl groups) with polyurethane to obtain PU-modified PP, the hardness of the separator (increasing safety) is enhanced, while the adhesion between the separator and the electrode surface is also increased. Increased adhesion reduces the lithium-ion transport path, lowering the battery's internal resistance. Simultaneously, to further reduce the separator's resistance and ion transport path, MOF materials such as ZIF-8 are grown on the surface of the PU-modified PP. The abundant porous structure of MOF materials effectively reduces the lithium-ion transport path within the battery, while also lowering the separator resistance, thereby increasing the battery's initial efficiency and cycle performance.

[0100] In some specific embodiments, the preparation method of the separator mainly includes the following steps:

[0101] S1. Preparation of hydroxyl-containing polypropylene (PP-OH), including:

[0102] Polypropylene, a first reactant, a second reactant, and a first solvent are mixed to obtain a mixture;

[0103] The mixture was heated under reflux to obtain a dehydrogenated product on polypropylene;

[0104] Then water, oxidant, and hydroxide are added to carry out an oxidation reaction, resulting in polypropylene containing hydroxyl groups.

[0105] In some embodiments, the first reactant includes, but is not limited to, at least one of sodium borohydride (NaBH4), potassium borohydride (KBH4), calcium borohydride (CaB2H8), magnesium borohydride (MgB2H8), or lithium borohydride (LiBH4). For example, the first reactant can be sodium borohydride (NaBH4), potassium borohydride (KBH4), calcium borohydride (CaB2H8), magnesium borohydride (MgB2H8), lithium borohydride (LiBH4), or any combination of two or more of the above substances, which will not be listed here.

[0106] In some embodiments, the second reactant includes, but is not limited to, at least one of ammonium sulfate ((NH4)2SO4), ammonium nitrate, ammonium chloride, ammonium bisulfate, ammonium fluoride, ammonium carbonate, or ammonium bicarbonate; for example, the second reactant can be ammonium sulfate ((NH4)2SO4), ammonium nitrate, ammonium chloride, ammonium bisulfate, ammonium fluoride, ammonium carbonate, or ammonium bicarbonate, or any combination of two or more of the above substances, which will not be listed here.

[0107] In addition, in other embodiments, the first reactant and the second reactant are not limited to the types listed above. Other types of first reactant and second reactant may be used if they meet the requirements of being able to modify polypropylene to obtain polypropylene containing hydroxyl groups. These will not be described in detail here.

[0108] In some embodiments, the first solvent includes at least one of tetrahydrofuran, acetonitrile, formamide, acetone, or propanol; for example, the first solvent may be tetrahydrofuran, acetonitrile, formamide, acetone, propanol, or any combination of two or more of the above substances.

[0109] In some embodiments, the oxidant includes at least one of hydrogen peroxide (H2O2), sodium hypochlorite, or sodium peroxide; the hydroxide includes at least one of sodium hydroxide (NaOH), potassium hydroxide, lithium hydroxide, rubidium hydroxide, or cesium hydroxide. As an example, the oxidant may be hydrogen peroxide (H2O2), and the hydroxide may be sodium hydroxide (NaOH).

[0110] However, this application is not limited to these primary solvents, oxidants, and hydroxides. Other solvents, oxidants, hydroxides, etc., that can be used in polypropylene modification may also be used. One of these substances may be used alone, or two or more may be used in combination.

[0111] In some embodiments, the mass ratio of polypropylene, the first reactant, and the second reactant is 200:(2-6):(4-8). In some embodiments, the mass ratio of polypropylene, the first reactant, and the second reactant is 200:(3-5):(5-7). As examples, the mass ratio of polypropylene, the first reactant, and the second reactant can be 200:2:4, 200:2:5, 200:3:5, 200:3:7, 200:4:6, 200:4:7, 200:5:6, 200:6:8, etc.

[0112] In some embodiments, the reflux temperature is 80°C to 100°C, and the reflux time is 8 hours to 16 hours. In some embodiments, the reflux temperature is 85°C to 95°C, and the reflux time is 10 hours to 14 hours. As examples, the reflux temperature can be 80°C, 85°C, 90°C, 95°C, 98°C, 100°C, etc.; and the reflux time can be 8 hours, 9 hours, 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, etc.

[0113] In some embodiments, the oxidation reaction temperature is 38°C to 50°C. In some embodiments, the oxidation reaction temperature is 40°C to 45°C. As examples, the oxidation reaction temperature can be 38°C, 40°C, 42°C, 45°C, 48°C, 50°C, etc.

[0114] Therefore, controlling the above process parameters within the given range is beneficial for preparing high-quality hydroxyl-containing polypropylene, which can further improve the performance of the separator membrane of this application. Those skilled in the art can selectively adjust one or more of the above process parameters according to actual production conditions.

[0115] In some embodiments, after adding water, as well as oxidizing agents and hydroxides to carry out the oxidation reaction, the process further includes steps of filtration, washing, and drying;

[0116] The washing process includes first washing with hot water, followed by washing with alcohol and / or ketone solvents; the drying temperature is 40℃~80℃, and the drying time is 8h~16h. For example, the drying temperature can be 40℃, 50℃, 60℃, 65℃, 70℃, 80℃, etc.; the drying time can be 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, 16h, etc.

[0117] As an example, step S1, the preparation of hydroxyl-containing polypropylene (PP-OH), specifically includes:

[0118] Place 200g of polypropylene into a reaction vessel, then add 2-6g of the first reactant, such as sodium borohydride, potassium borohydride, calcium borohydride, magnesium borohydride, or lithium borohydride, and 4-8g of the second reactant, such as ammonium sulfate, ammonium nitrate, ammonium chloride, ammonium bisulfate, ammonium fluoride, ammonium carbonate, or ammonium bicarbonate. Then add 500mL of the first solvent, such as tetrahydrofuran, acetonitrile, formamide, acetone, etc., and mix to obtain a mixture.

[0119] The mixture was heated and refluxed at 80℃~100℃ for 8h~16h and cooled to room temperature to obtain the dehydrogenated product on polypropylene.

[0120] Then add 500 mL of deionized water. In the first solvent, such as a mixture of tetrahydrofuran and water, use 10-50 mL of oxidizing agent such as hydrogen peroxide, sodium hypochlorite or sodium peroxide and 5-15 g of hydroxide such as sodium hydroxide, potassium hydroxide, lithium hydroxide, etc. to carry out the oxidation reaction. Oxidize the mixture at about 40°C.

[0121] The resulting substance was then filtered, washed with hot water, and then washed with ethanol and acetone. The product was dried in a vacuum oven at 40–80°C for 8–16 hours to obtain the dried substance, namely hydroxyl-containing polypropylene, which can be denoted as PP-OH. The relevant reaction equations involved in the preparation process of this hydroxyl-containing polypropylene (PP-OH) are as follows: Figure 1 As shown.

[0122] The hydroxylation mechanism is as follows: First, the first and second reactants, such as NaBH4 and (NH4)2SO4, react in tetrahydrofuran solvent to generate BH3-NH3. Then, the mixture is refluxed onto PP to obtain dehydrogenated BH-NH2. Finally, under the action of hydroxides and oxidants such as NaOH and H2O2, hydroxyl groups are generated on the PP surface to obtain PP-OH.

[0123] S2. Preparation of polyurethane-modified polypropylene, including:

[0124] The hydroxyl-containing polypropylene, isocyanate raw material, and second solvent obtained in step S1 are mixed to obtain a mixture;

[0125] The mixture was heated under reflux, and then polytetrahydrofuran raw materials and a second solvent were added to carry out a polymerization reaction to obtain a precipitate.

[0126] The precipitate was dried to obtain polyurethane-modified polypropylene.

[0127] In some embodiments, the isocyanate raw material includes at least one of toluene diisocyanate, diphenylmethane diisocyanate, or naphthalene 1,5-diisocyanate. For example, the isocyanate raw material can be toluene diisocyanate (TDI), diphenylmethane diisocyanate, naphthalene 1,5-diisocyanate, or any combination of two or more of the above substances.

[0128] In some embodiments, the polytetrahydrofuran raw material includes at least one of polytetrahydrofuran, poly-2-methyltetrahydrofuran, or poly-2-ethyltetrahydrofuran. For example, the polytetrahydrofuran raw material can be polytetrahydrofuran, poly-2-methyltetrahydrofuran, poly-2-ethyltetrahydrofuran, or a combination of any two or more of the above substances.

[0129] In some embodiments, the second solvent includes at least one of toluene, xylene, or benzene. For example, the second solvent may be toluene, xylene, benzene, or a combination of any two or more of the above substances.

[0130] In addition, in other embodiments, the isocyanate raw materials, polytetrahydrofuran raw materials, and second solvents are not limited to the types listed above. When the requirements of preparing polypropylene that can be used for polyurethane modification and improving battery performance are met, other types of isocyanate raw materials, polytetrahydrofuran raw materials, and second solvents can also be used, which will not be described in detail here.

[0131] In some embodiments, the mass ratio of hydroxyl-containing polypropylene to isocyanate raw materials is 5–10:0.5–1. In some embodiments, the mass ratio of hydroxyl-containing polypropylene to isocyanate raw materials is 6–8:0.6–0.8. As examples, the mass ratio of hydroxyl-containing polypropylene to isocyanate raw materials can be 5:0.5, 5:0.6, 6:0.5, 5:0.8, 7:0.6, 7:0.8, 8:0.6, 8:0.7, 8:0.8, 8:0.9, 10:1, etc.

[0132] By adjusting the mass ratio of hydroxyl-containing polypropylene to isocyanate raw materials, the amount of isocyanate raw materials added can be controlled. Controlling the amount of isocyanate raw materials added allows for the control of polyurethane synthesis, and consequently, the polyurethane content in the separator. The polyurethane content should not be too high or too low. Insufficient polyurethane reduces the peel strength between the electrode and the separator. Furthermore, polyurethane has a certain liquid absorption capacity; reducing polyurethane also leads to a decrease in liquid absorption rate, ultimately resulting in reduced initial efficiency and cycle performance. Conversely, a higher polyurethane content increases the peel strength between the electrode and the separator. However, excessive polyurethane can clog the separator pores, thus reducing the liquid absorption rate and ultimately increasing the battery's internal resistance, further decreasing initial efficiency and cycle performance.

[0133] In some embodiments, the mass ratio of isocyanate raw material to polytetrahydrofuran raw material is 0.5–1:1–5. In some embodiments, the mass ratio of isocyanate raw material to polytetrahydrofuran raw material is 0.6–0.8:2–4. As examples, the mass ratio of isocyanate raw material to polytetrahydrofuran raw material is 0.5:1, 0.5:2, 0.5:3, 0.6:1.5, 0.6:2.5, 0.7:1, 0.7:3, 0.7:4, 0.8:2, 0.8:5, 1:5, etc.

[0134] In some embodiments, the reflux temperature is 100°C to 120°C, and the reflux time is 4 hours to 10 hours. In some embodiments, the reflux temperature is 105°C to 115°C, and the reflux time is 5 hours to 8 hours. As examples, the reflux temperature can be 100°C, 105°C, 110°C, 115°C, 120°C, etc.; and the reflux time can be 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, etc.

[0135] In some embodiments, the drying temperature is 40℃~80℃, and the drying time is 10h~16h. In some embodiments, the drying temperature is 50℃~70℃, and the drying time is 11h~15h. As examples, the drying temperature can be 40℃, 50℃, 60℃, 65℃, 70℃, 80℃, etc.; the drying time can be 10h, 11h, 12h, 13h, 14h, 15h, 16h, etc.

[0136] Therefore, controlling the above process parameters within the given range is beneficial for preparing high-quality polyurethane-modified polypropylene, which can further improve the performance of the separator membrane of this application. Those skilled in the art can selectively adjust one or more of the above process parameters according to actual production conditions.

[0137] As an example, step S2, the preparation of polyurethane-modified polypropylene, specifically includes:

[0138] Add 0.5–1 g of hydroxyl-containing polypropylene obtained in step S1 and 5–10 g of isocyanate raw materials such as toluene diisocyanate, diphenylmethane diisocyanate or naphthalene 1,5-diisocyanate to a reaction vessel, add a second solvent such as toluene, xylene or benzene, and mix to obtain a mixture.

[0139] The reaction vessel is heated to 100℃~120℃ and refluxed in an oil bath for 4h~10h. After all the hydroxyl-containing polypropylene and isocyanate raw materials have reacted completely, 1~5g of polytetrahydrofuran raw material such as polytetrahydrofuran, poly-2-methyltetrahydrofuran or poly-2-ethyltetrahydrofuran, and 40mL of the second solvent toluene, xylene or benzene are added. The reactants are allowed to polymerize for 12 hours to completely polymerize and obtain a precipitate.

[0140] The precipitate was dried in a vacuum oven at 40℃~80℃ for 10h~16h to obtain polyurethane-modified polypropylene, which can be denoted as PP-PU. The relevant reaction equations involved in this process are as follows: Figure 2 As shown.

[0141] S3. Preparation of the separator membrane, including:

[0142] Zinc nitrate hexahydrate and imidazole raw materials were dissolved in a third solvent to obtain zinc nitrate hexahydrate solution and imidazole raw material solution, respectively.

[0143] The polyurethane-modified polypropylene obtained in step S2, zinc nitrate hexahydrate solution, and imidazole raw material solution are mixed and reacted under stirring conditions to form a modified layer on the surface of the polyurethane-modified polypropylene.

[0144] In the embodiments of this application, the MOF material can be at least one of ZIF-8, ZIF-7, ZIF-67 or ZIF-90. When different MOF materials are selected, the synthetic raw materials such as metal salts and solvents used in the preparation process are different.

[0145] In some embodiments, the MOF material is ZIF-8, the imidazole raw material includes 2-methylimidazole, and the third solvent includes methanol.

[0146] In some embodiments, the MOF material is ZIF-7, the imidazole raw material includes benzimidazole, and the third solvent includes dimethylformamide.

[0147] In some embodiments, the MOF material is ZIF-90, the imidazole raw material includes imidazole-2-formaldehyde, and the third solvent includes dimethylformamide.

[0148] In some embodiments, the MOF material is ZIF-67, zinc nitrate hexahydrate is replaced with cobalt nitrate hexahydrate, the imidazole raw material includes 2-methylimidazole, and the third solvent includes water.

[0149] In some embodiments, the mass ratio of zinc nitrate hexahydrate to imidazole raw material is 1–3:2–5. For example, the mass ratio of zinc nitrate hexahydrate to imidazole raw material is 1:2, 1:3, 1:4, 1:5, 2:2, 2:3, 2:5, 3:2, 3:5, etc.

[0150] In some embodiments, the stirring temperature is 20°C to 40°C, and the stirring time is 20h to 30h. In some embodiments, the stirring temperature is 25°C to 30°C, and the stirring time is 24h to 26h.

[0151] As an example, step S3, the preparation of the separating membrane, specifically includes:

[0152] The polyurethane-modified polypropylene obtained in step S2, 1-3g of zinc nitrate hexahydrate (Zn(NO3)2·6H2O) and 2-5g of imidazole raw materials such as 2-methylimidazolium are dissolved in 80mL of a third solvent such as methanol.

[0153] Then, polyurethane-modified polypropylene and zinc nitrate hexahydrate solution were added to the imidazole raw material solution and reacted under stirring conditions, such as continuous stirring at 25°C for 24 hours. The collected precipitate was washed several times with methanol and vacuum dried to obtain MOF nanoparticles on the PP-PU surface, such as ZIF-8 nanoparticles on the PP-PU surface, that is, a modified layer was formed on the surface of polyurethane-modified polypropylene.

[0154] [Battery]

[0155] In this application embodiment, the battery can be a secondary battery or a primary battery, preferably a secondary battery. For example, the battery can be a lithium-ion secondary battery, a lithium primary battery, a sodium-ion battery, a magnesium-ion battery, etc., but is not limited to these. The battery structure of this application includes, but is not limited to, a pouch-type lithium-ion battery, a square hard-shell battery, or a cylindrical hard-shell battery.

[0156] It should be noted that, in the specific implementation, lithium-ion batteries are used as an example of secondary batteries to explain this application, but the batteries in this application are not limited to lithium-ion batteries.

[0157] In some embodiments, the battery includes a positive electrode, a negative electrode, an electrolyte, and a separator. During battery charging and discharging, active ions repeatedly insert and extract between the positive and negative electrodes. The separator is disposed between the positive and negative electrodes to provide isolation. The electrolyte acts as a conductor for ions between the positive and negative electrodes.

[0158] In some embodiments, the positive electrode includes a positive current collector and a positive electrode film layer disposed on at least one surface of the positive current collector. The phrase "positive electrode film layer disposed on at least one surface of the positive current collector" means that the positive electrode film layer can be disposed on one surface of the positive current collector along its thickness direction, or on two surfaces of the positive current collector along its thickness direction. Here, "surface" can refer to the entire area of ​​the positive current collector or only a portion of it; this application does not impose any particular limitation, as long as the purpose of this application is achieved.

[0159] As an example, the positive current collector has two surfaces opposite each other in its own thickness direction, and the positive electrode film layer is disposed on the two opposite surfaces of the positive current collector. It can be understood that the positive electrode film layer can also be stacked on either of the two surfaces of the positive current collector.

[0160] In some embodiments, the positive current collector may be a metal foil or a composite current collector.

[0161] As an example, the metal foil may be aluminum foil or aluminum alloy foil. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. The polymer material base layer may include at least one of polypropylene, polyethylene terephthalate, polybutylene terephthalate, polystyrene, and polyethylene; the metal material layer may include at least one of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy.

[0162] In some embodiments, the positive electrode film layer includes a positive electrode active material, which may be a lithium transition metal composite oxide, a lithium-containing phosphate, or a modified compound thereof; or it may be one or more of a composite oxide obtained by adding other transition metals, non-transition metals, or non-metals to a lithium transition metal composite oxide. The transition metal may be one or more of Mn, Fe, Ni, Co, Cr, Ti, Zn, V, Al, Zr, Ce, Mg, etc. For example, the positive electrode active material in the embodiments of this application may be a high-nickel positive electrode active material, a lithium-rich manganese-based positive electrode active material, or a lithium manganese iron phosphate positive electrode active material.

[0163] As an example, the positive electrode active material can be selected from one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as NCM622), lithium nickel cobalt aluminum oxide, and lithium phosphates with olivine structure.

[0164] However, this application is not limited to these materials; other conventional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more.

[0165] In some embodiments, the positive electrode film layer further includes a binder. This application does not impose any particular limitation on the type of binder in the positive electrode film layer. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-tetrafluoroethylene-propylene terpolymer, ethylene-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, or fluorinated acrylate resin.

[0166] In some embodiments, the positive electrode film layer also includes a conductive agent. This application does not impose any particular limitation on the type of conductive agent in the positive electrode film layer. As an example, the conductive agent may include at least one of conductive carbon black, acetylene black, Ketjen black, carbon nanotubes, graphene, or carbon nanofibers.

[0167] In some embodiments, the negative electrode sheet includes a negative current collector and a negative electrode film layer disposed on at least one surface of the negative current collector. The phrase "a negative electrode film layer disposed on at least one surface of the negative current collector" means that the negative electrode film layer can be disposed on one surface of the negative current collector along its thickness direction, or on two surfaces of the negative current collector along its thickness direction. Here, "surface" can refer to the entire area of ​​the negative current collector or only a portion of it; this application does not impose any particular limitation, as long as the purpose of this application is achieved.

[0168] As an example, the negative electrode current collector has two surfaces opposite each other in its own thickness direction, and the negative electrode film layer is disposed on the two opposite surfaces of the negative electrode current collector. It can be understood that the negative electrode film layer can also be stacked on either of the two surfaces of the negative electrode current collector.

[0169] This application does not impose any particular limitation on the negative electrode current collector, as long as it can achieve the purpose of this application. In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. The metal foil includes copper foil, copper alloy foil, nickel foil, titanium foil, etc. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. The aforementioned polymer material base layer may include at least one of polypropylene, polyethylene terephthalate, polybutylene terephthalate, polystyrene, and polyethylene; the metal material layer may include at least one of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy.

[0170] In some embodiments, the negative electrode film layer includes a negative electrode active material, which may be a negative electrode active material known in the art for use in batteries. This application does not have any particular limitation on the type of negative electrode active material, as long as it can achieve the purpose of this application.

[0171] As an example, the negative electrode active material may include at least one of the following materials: natural graphite, artificial graphite, soft carbon, hard carbon, mesophase carbon microspheres, silicon-based materials, tin-based materials, lithium titanate, transition metal nitrides, etc. The aforementioned silicon-based materials may be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. Tin-based materials may be selected from at least one of elemental tin, tin oxide compounds, and tin alloys.

[0172] However, this application is not limited to these materials, and other conventional materials that can be used as negative electrode active materials in batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0173] In some embodiments, the negative electrode film layer further includes at least one of a conductive agent, a thickener, and a binder. This application does not particularly limit the types of conductive agents, thickeners, and binders in the negative electrode film layer, as long as they achieve the purpose of this application. As an example, the binder in the negative electrode film layer may be selected from at least one of styrene-butadiene rubber, polyvinylidene fluoride (PVDF), polyacrylic acid, sodium polyacrylate, polyacrylamide, etc. The conductive agent in the negative electrode film layer may be selected from at least one of acetylene black, conductive carbon black, Ketjen black, carbon nanotubes, graphene, carbon nanofibers, etc. The thickener may be sodium carboxymethyl cellulose (CMC-Na).

[0174] The electrolyte used in the embodiments of this application can be any electrolyte known in the prior art. The specific type and structure of the electrolyte can be any type of electrolyte known in the art that can be used in secondary batteries, such as ester electrolytes or ether electrolytes, etc., and there is no limitation on this, which will not be elaborated here.

[0175] Example

[0176] The following describes the implementation methods of this application. The implementation methods described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the implementation methods, they shall be performed in accordance with the techniques or conditions described in the literature in this field or according to the product instructions. Reagents, materials, or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.

[0177] Example 1

[0178] 1. Preparation of the separating membrane

[0179] S1. Place 200g of polypropylene into a reaction vessel, then add 5g of sodium borohydride and 7g of ammonium sulfate, followed by 500mL of tetrahydrofuran. Mix the mixture to obtain a final product. Heat the mixture under reflux at 90℃ for 12 hours, then cool to room temperature to obtain a dehydrogenated product on the polypropylene. Add 500mL of deionized water, and in the mixture of tetrahydrofuran and water, oxidize with 30mL of hydrogen peroxide and 10g of sodium hydroxide at 40℃. Filter the resulting product, wash with hot water, and then wash with ethanol and acetone. Dry the product in a vacuum oven at 60℃ for 12 hours to obtain the dried product, which is hydroxyl-containing polypropylene, denoted as PP-OH.

[0180] S2. Add 8g of PP-OH obtained in step S1 and 0.725g of toluene diisocyanate (TDI) to a reaction vessel, add 40mL of toluene, and mix to obtain a mixture. Heat the reaction vessel to 110℃ and reflux for 6 hours in an oil bath. After all the PP-OH and TDI have reacted completely, add 3g of polytetrahydrofuran and 40mL of toluene, and allow the reactants to react for 12 hours to completely polymerize, obtaining a precipitate. Dry the precipitate in a vacuum oven for 12 hours at a temperature of 60℃ to obtain polyurethane-modified polypropylene, which can be referred to as PP-PU.

[0181] S3. Dissolve the PP-PU obtained in step S2, 1.68 g of zinc nitrate hexahydrate (Zn(NO3)2·6H2O), and 3.7 g of 2-methylimidazole in 80 mL of methanol. Then, add the polyurethane-modified polypropylene and Zn(NO3)2·6H2O solution to the 2-methylimidazole solution and stir continuously at 25 °C for 24 h. Wash the collected precipitate several times with methanol and vacuum dry it to obtain ZIF-8 nanoparticles on the surface of PP-PU. That is, a modified layer is formed on the surface of polyurethane-modified polypropylene to obtain a release membrane.

[0182] 2. Preparation of electrolyte

[0183] Ethylene carbonate (EC), dimethyl carbonate (DMC), and diethyl carbonate (DEC) were mixed in a volume ratio of 1:2:1 to obtain a mixed organic solvent. Then, fully dried lithium salt LiPF6 was dissolved in the mixed organic solvent at a ratio of 1.5 mol / L to prepare an electrolyte.

[0184] 3. Preparation of the positive electrode sheet

[0185] The positive electrode active material is a ternary 6-series (LiNi) 0.6 Co 0.2 Mn 0.2O2 powder, conductive carbon, and PVDF (binder) are mixed in a mass ratio of 8:1:1 to obtain a mixed material. This mixed material is then thoroughly stirred in NMP to obtain the corresponding positive electrode active slurry. The positive electrode active slurry is coated onto conventional aluminum foil to obtain an electrode with a LiNi content of [missing information]. 0.6 Co 0.2 Mn 0.2 The O2 mass fraction is 80wt%, and the areal density of the positive electrode slurry is 2mg / cm³. 2 The positive electrode slurry coating is dried and pressed to obtain the positive electrode sheet.

[0186] 4. Preparation of negative electrode sheet

[0187] Graphite powder (anode active material), conductive carbon, and PVDF (binder) were mixed in a mass ratio of 8:1:1 to obtain a mixed material. This mixed material was then thoroughly stirred in deionized water to obtain the corresponding anode active slurry. The anode active slurry was coated onto conventional copper foil, resulting in an electrode with a graphite content of 80 wt% and a surface density of 1.21 mg / cm³. 2 The negative electrode slurry coating is dried and then pressed into a sheet to obtain the negative electrode sheet.

[0188] 5. Preparation of lithium-ion batteries

[0189] A button cell is obtained by sequentially placing the negative electrode, separator, and positive electrode into a battery casing. After processes such as drying, electrolyte injection, encapsulation, formation, and capacity testing, a lithium-ion battery is obtained.

[0190] Example 2

[0191] The preparation of the lithium-ion battery is basically the same as in Example 1, with the main difference being:

[0192] In the preparation of the separator membrane, 0.5 g of toluene diisocyanate (TDI) is added in step S2.

[0193] Example 3

[0194] The preparation of the lithium-ion battery is basically the same as in Example 1, with the main difference being:

[0195] In the preparation of the separator membrane, in step S2, 1.0 g of toluene diisocyanate (TDI) is added.

[0196] Example 4

[0197] The preparation of the lithium-ion battery is basically the same as in Example 1, with the main difference being:

[0198] In the preparation of the isolation membrane, in step S3, 1g of zinc nitrate hexahydrate (Zn(NO3)2·6H2O) and 2g of 2-methylimidazole are dissolved in 80mL of methanol respectively.

[0199] Example 5

[0200] The preparation of the lithium-ion battery is basically the same as in Example 1, with the main difference being:

[0201] In the preparation of the isolation membrane, in step S3, 3g of zinc nitrate hexahydrate (Zn(NO3)2·6H2O) and 5g of 2-methylimidazole are dissolved in 80mL of methanol respectively.

[0202] Example 6

[0203] The preparation of the lithium-ion battery is basically the same as in Example 1, with the main difference being:

[0204] In the process of preparing the separator membrane, in step S2, the isocyanate raw material is diphenylmethane diisocyanate, and the polytetrahydrofuran raw material is poly2-methyltetrahydrofuran.

[0205] Example 7

[0206] The preparation of the lithium-ion battery is basically the same as in Example 1, with the main difference being:

[0207] In the preparation of the separator membrane, in step S3, the imidazole raw material is benzimidazole, the third solvent is dimethylformamide, and the obtained MOF material is ZIF-7.

[0208] Example 8

[0209] The preparation of the lithium-ion battery is basically the same as in Example 1, with the main difference being:

[0210] In the preparation of the separator membrane, in step S3, the imidazole raw material is imidazole-2-formaldehyde, the third solvent is dimethylformamide, and the obtained MOF material is ZIF-90.

[0211] Comparative Example 1

[0212] The preparation of the lithium-ion battery is basically the same as in Example 1, with the main difference being:

[0213] The release liner is made of pure polypropylene (PP).

[0214] Comparative Example 2

[0215] The preparation of the lithium-ion battery is basically the same as in Example 1, with the main difference being:

[0216] The separator membrane uses polypropylene as the base material and is coated with PVDF and ceramic coatings on the polypropylene surface.

[0217] Comparative Example 3

[0218] The preparation of the lithium-ion battery is basically the same as in Example 1, with the main difference being:

[0219] In the preparation process of the separator, step S3 (ZIF-8 modification) was not performed, that is, the obtained PP-PU was used as the separator.

[0220] Comparative Example 4

[0221] The preparation of the lithium-ion battery is basically the same as in Example 1, with the main difference being:

[0222] During the preparation of the separator membrane, step S2 (no polyurethane modification) was not performed, that is, ZIF-8 was formed on the surface of polypropylene as the separator membrane.

[0223] Performance testing

[0224] 1. Testing of the separating membrane

[0225] The isolation membranes obtained in the above embodiments and comparative examples were subjected to liquid absorption rate test, heat distortion temperature test, puncture strength test, and peel strength (adhesion) test.

[0226] (1) Test method for liquid absorption rate: Take a 5×5cm sample from each group. 2 The separator membrane, weighed and recorded as 'a', is immersed in the electrolyte for 1 hour to allow it to fully absorb the electrolyte. After absorption, the separator membrane is suspended for 5 minutes to dry the electrolyte adhering to its surface, and the weight is recorded as 'b'. The electrolyte absorption rate of the separator membrane is (ba) / a × 100%.

[0227] (2) Test method for heat distortion temperature: Suspend a weight on the separator and place it in an oven at a set heating rate (2℃ / min). Record the temperature and time when the weight falls. Qualitatively evaluate the heat resistance characteristics of the separator by measuring the time from a certain temperature point to when the weight falls.

[0228] (3) Test method for puncture strength: Using a diaphragm puncture tester, cut the diaphragm into strips. The width of the strips must be greater than 100 mm. Install the 100 mm wide test piece on the membrane fixing ring, and then use a steel needle with a diameter of 1 mm and a diameter tip radius of 0.5 mm to puncture the test piece at a speed of 50 mm / min. Read the load of the steel needle penetrating the test piece.

[0229] (4) Test method for peel strength: Cut the foil into a certain width, roll the cut electrode foil and the separator film under the same pressure, and then stick them onto the iron plate with double-sided adhesive. Then use a tensile testing machine to pull it upward at a speed of 50 mm / min at a horizontal angle of 180° (i.e., perpendicular to the ground) and calculate the peel strength.

[0230] The test results are shown in Table 1 below.

[0231] Table 1. Performance test results of the separators in each embodiment and comparative example.

[0232] Group Liquid absorption rate (%) Heat distortion temperature (°C) Puncture intensity (N) Peel strength (N / m) Example 1 138 142 4.2 3.2 Example 2 126 140 4.1 2.7 Example 3 135 139 4.5 3.4 Example 4 121 141 3.9 3.2 Example 5 124 141 4.1 3.2 Example 6 136 140 4.1 3.1 Example 7 137 140 4.0 3.1 Example 8 132 138 4.2 3.1 Comparative Example 1 102 113 3.2 0.2 Comparative Example 2 117 140 3.9 3.1 Comparative Example 3 108 140 4.1 3.2 Comparative Example 4 115 138 3.3 2.6

[0233] As can be seen from the data in Table 1, compared with the pure PP release film of Comparative Example 1, the release film provided by the present invention has significant improvements in liquid absorption rate, heat distortion temperature, puncture strength, and peel strength. Furthermore, compared with the release films of Comparative Examples 2-4, the release film provided by the present invention also shows certain improvements in liquid absorption rate, heat distortion temperature, puncture strength, and peel strength.

[0234] 2. Testing of lithium-ion batteries

[0235] The lithium-ion batteries obtained from the above embodiments and comparative examples were subjected to initial coulombic efficiency, battery resistance, and cycle capacity retention tests.

[0236] (1) Initial Coulombic Efficiency (First-Effect) Test Method: First, the battery is formed according to the process of 0.1C CC to 3.75V. This step is the stage of SEI film formation in the battery, and the battery capacity C1 after formation is recorded. Second, the battery is fully charged according to the process of 1C CC to 4.4V, and 4.4V CV to I≤0.05C, and the charging capacity C2 is recorded. Finally, the battery discharge capacity C3 is obtained by charging according to 1C DC to 2.8V. The initial coulombic efficiency is calculated according to the formula C3 / (C1+C2).

[0237] (2) Battery internal resistance test method: The battery internal resistance is measured by a battery internal resistance measuring instrument.

[0238] (3) Cyclic capacity retention test method: Follow the steps a. 1C DC to 2.8V, b. rest for 30min, c. 1C DC to 4.4V, d. rest for 30min, e. 1C DC to 2.8V, f. rest for 30min to perform the test. Repeat steps c to f, record the battery capacity C4 after 300 cycles, and calculate the capacity retention rate using C4 / C3.

[0239] The test results are shown in Table 2 below.

[0240] Table 2. Battery performance test results for each embodiment and comparative example.

[0241] Group Internal resistance / Ω First-time effect % Cyclic performance % Example 1 11.21 93.2 92 Example 2 11.28 92.8 89 Example 3 11.36 92.5 91 Example 4 11.43 92.4 91 Example 5 11.28 91.6 89 Example 6 11.32 92.7 91 Example 7 11.23 92.9 91 Example 8 11.38 92.4 90 Comparative Example 1 13.28 89.2 86 Comparative Example 2 12.15 89.4 87 Comparative Example 3 13.15 89.6 89 Comparative Example 4 11.52 91.3 89

[0242] As can be seen from the data in Table 2, the battery using the separator provided in the embodiments of the present invention plays a positive role in reducing the battery's internal resistance and improving the battery's initial coulombic efficiency and cycle performance.

[0243] Meanwhile, the data in the table above also shows that the polyurethane content should not be too high or too low. When the polyurethane content is low, it will reduce the peel strength between the electrode and the separator. Polyurethane also has a certain liquid absorption capacity; reducing the polyurethane content will also lead to a decrease in the liquid absorption rate, ultimately resulting in a decrease in the battery's initial efficiency and cycle performance. When the polyurethane content is high, it will increase the peel strength between the electrode and the separator, but excessive polyurethane may clog the separator's pores, thus reducing the separator's liquid absorption rate, ultimately leading to an increase in the battery's internal resistance and a decrease in initial efficiency and cycle performance. Similarly, the MOF material content should not be too high or too low. When the content of MOF materials such as ZIF-8 is low, it increases the separator's own resistance. The reduction in the porous structure will also reduce the separator's liquid absorption capacity, thereby increasing the battery's internal resistance and reducing the battery's initial efficiency and cycle performance. Conversely, when the ZIF-8 content is high, some ZIF-8 may agglomerate on the separator surface, clogging the separator's pores, resulting in a decrease in the liquid absorption rate, an increase in the battery's internal resistance, and a decrease in initial efficiency and cycle performance.

[0244] The parts of this invention not described in detail are techniques known to those skilled in the art.

[0245] The basic principles of the present invention have been described above with reference to specific embodiments. However, it should be noted that the advantages, benefits, and effects mentioned in the present invention are merely examples and not limitations, and should not be considered as essential features of each embodiment of the present invention. Furthermore, the specific details disclosed above are for illustrative and facilitative purposes only, and are not limitations. These details do not limit the present invention to the necessity of employing the aforementioned specific details.

[0246] In the detailed description and claims, a list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms may mean any combination of the listed items. For example, if items A and B are listed, then the phrase "at least one of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, then the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may contain a single element or multiple elements. Item B may contain a single element or multiple elements. Item C may contain a single element or multiple elements.

[0247] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A separating membrane, characterized in that, The isolation membrane includes a substrate and a modified layer formed on the surface of the substrate; The material of the substrate includes polyurethane-modified polypropylene; The modified layer is made of MOF material; The method for preparing the isolation membrane includes the following steps: Polypropylene containing hydroxyl groups is reacted with raw materials used to synthesize polyurethane to obtain polyurethane-modified polypropylene. The polyurethane-modified polypropylene is reacted with raw materials used to synthesize MOF materials to form a modified layer on the surface of the polyurethane-modified polypropylene. The material of the modified layer includes MOF materials, thereby obtaining the separator membrane.

2. The separator membrane according to claim 1, characterized in that, The isolation membrane satisfies at least one of the following conditions (1) to (4): (1) The MOF material includes at least one of ZIF-8, ZIF-7, ZIF-67 or ZIF-90; (2) The mass ratio of the MOF material to the substrate is 1:80 to 1:40; (3) The particle size of the MOF material is 50 nm to 300 nm; (4) The thickness of the modified layer is 600nm to 1000nm.

3. The separator membrane according to claim 1, characterized in that, The preparation of the hydroxyl-containing polypropylene includes: Polypropylene, a first reactant, a second reactant, and a first solvent are mixed to obtain a mixture; The mixture is heated under reflux to obtain a dehydrogenated product on the polypropylene; Then water, oxidant, and hydroxide are added to carry out an oxidation reaction, resulting in polypropylene containing hydroxyl groups.

4. The separator membrane according to claim 3, characterized in that, The preparation of the hydroxyl-containing polypropylene satisfies at least one of the following conditions (1) to (10): (1) The first reactant includes at least one of sodium borohydride, potassium borohydride, calcium borohydride, magnesium borohydride or lithium borohydride; (2) The second reactant includes at least one of ammonium sulfate, ammonium nitrate, ammonium chloride, ammonium bisulfate, ammonium fluoride, ammonium carbonate, or ammonium bicarbonate; (3) The first solvent includes at least one of tetrahydrofuran, acetonitrile, formamide, acetone or propanol; (4) The oxidant includes at least one of hydrogen peroxide, sodium hypochlorite, or sodium peroxide; the hydroxide includes at least one of sodium hydroxide, potassium hydroxide, lithium hydroxide, rubidium hydroxide, or cesium hydroxide; (5) The mass ratio of the polypropylene, the first reactant, and the second reactant is 200:(2-6):(4-8); (6) The temperature of the heating reflux is 80℃~100℃, and the reflux time is 8h~16h; (7) The temperature of the oxidation reaction is 38℃~50℃; (8) After adding water, oxidant and hydroxide for oxidation reaction, the process also includes the steps of filtration, washing and drying; (9) The washing process includes washing with hot water first, and then washing with alcohol solvents and / or ketone solvents; (10) The drying temperature is 40℃~80℃ and the drying time is 8h~16h.

5. The separator membrane according to claim 1, characterized in that, The step of reacting hydroxyl-containing polypropylene with raw materials used to synthesize polyurethane specifically includes: A mixture is obtained by mixing polypropylene containing hydroxyl groups, isocyanate raw materials, and a second solvent. The mixture is heated under reflux, and then polytetrahydrofuran raw materials and a second solvent are added to carry out a polymerization reaction to obtain a precipitate. The precipitate was dried to obtain polyurethane-modified polypropylene.

6. The separator membrane according to claim 5, characterized in that, The step of reacting hydroxyl-containing polypropylene with raw materials for synthesizing polyurethane satisfies at least one of the following conditions (1) to (7): (1) The isocyanate raw materials include at least one of toluene diisocyanate, diphenylmethane diisocyanate or naphthalene 1,5-diisocyanate; (2) The polytetrahydrofuran raw material includes at least one of polytetrahydrofuran, poly-2-methyltetrahydrofuran, or poly-2-ethyltetrahydrofuran; (3) The second solvent includes at least one of toluene, xylene, or benzene; (4) The mass ratio of the hydroxyl-containing polypropylene to the isocyanate raw material is 5-10:0.5-1; (5) The mass ratio of the isocyanate raw material to the polytetrahydrofuran raw material is 0.5-1:1-5; (6) The temperature of the heating reflux is 100℃~120℃, and the reflux time is 4h~10h; (7) The drying temperature is 40℃~80℃ and the drying time is 10h~16h.

7. The separator membrane according to claim 1, characterized in that, The MOF material is ZIF-8, and the step of reacting the polyurethane-modified polypropylene with the raw materials used to synthesize the MOF material specifically includes: Zinc nitrate hexahydrate and imidazole raw materials were dissolved in a third solvent to obtain zinc nitrate hexahydrate solution and imidazole raw material solution, respectively. The polyurethane-modified polypropylene, zinc nitrate hexahydrate solution, and imidazole raw material solution are mixed and reacted under stirring conditions to form a modified layer on the surface of the polyurethane-modified polypropylene.

8. The separator membrane according to claim 7, characterized in that, The step of reacting the polyurethane-modified polypropylene with the raw materials used to synthesize MOF materials satisfies at least one of the following conditions (1) to (6): (1) The MOF material is ZIF-8, the imidazole raw material includes 2-methylimidazole, and the third solvent includes methanol; (2) The MOF material is ZIF-7, the imidazole raw material includes benzimidazole, and the third solvent includes dimethylformamide; (3) The MOF material is ZIF-90, the imidazole raw material includes imidazole-2-formaldehyde, and the third solvent includes dimethylformamide; (4) The MOF material is ZIF-67, the zinc nitrate hexahydrate is replaced with cobalt nitrate hexahydrate, the imidazole raw material includes 2-methylimidazole, and the third solvent includes water; (5) The mass ratio of zinc nitrate hexahydrate to imidazole raw material is 1-3:2-5; (6) The stirring temperature is 20℃~40℃ and the stirring time is 20h~30h.

9. A battery, comprising a positive electrode, a negative electrode, and a separator, characterized in that, The separator is the separator as described in any one of claims 1 to 8.

Citation Information

Patent Citations

  • Methods for bonding dissimilar synthetic polymeric materials and the products involved in and resulting from such methods

    CA1125588A

  • Reactive hot melt adhesive raw material and preparation method thereof

    CN112358833A