An insertion welding method based on existing railway lines

By measuring and pre-processing the height difference between the inserted rail and the existing rail, the problems of track smoothness and wheel-rail mismatch during the welding of the inserted short rail were solved, thus achieving longitudinal track smoothness and stable operation of the EMU.

CN117840562BActive Publication Date: 2026-11-17TIEKE JINHUA TESTING CENT CO LTD +4
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410213618.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-27
Publication Date
2026-11-17
Estimated Expiration
2044-02-27

AI Technical Summary

Technical Problem

When using flash welding for inserting short rails, existing technologies have issues with wear and profile inconsistencies between the inserted rails and existing track rails, leading to abrupt changes in track smoothness and unreasonable wheel-rail matching, which affects the operational quality of the EMU.

Method used

By measuring the rail head height of the inserted rail and the existing rail, calculating the height difference, and pre-processing the straightness and profile of the inserted rail to match the height of the existing rail, the smoothness of the rail and the stability of the wheel-rail relationship after welding are ensured.

Benefits of technology

This effectively avoids sudden changes in track straightness after welding, reduces abnormal vibrations in the EMU, improves the smoothness of EMU operation and passenger comfort, and extends the service life of the track.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117840562B_ABST
    Figure CN117840562B_ABST
Patent Text Reader

Abstract

This invention proposes an insertion welding method based on existing railway lines, belonging to the field of railway maintenance technology. The insertion welding method includes: measuring both ends of the inserted rail and its corresponding existing rails to obtain the rail head height of the inserted rail and the existing rail; calculating the rail head height difference between the inserted rail and the existing rail based on the rail head height of the inserted rail and the existing rail; performing straightness pretreatment on the inserted rail based on the rail head height difference; placing the pretreated inserted rail on the insertion welding section of the existing rail and performing insertion welding. This invention can effectively reduce the height difference between the inserted rail and the existing rail, reduce abrupt changes in track straightness caused by flash welding, ensure the longitudinal smoothness of the track line, reduce abnormal vibrations in the EMU after rail insertion, and ensure the operational quality of the EMU.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of railway maintenance technology, and in particular to an insertion welding method based on existing railway lines. Background Technology

[0002] With the rapid development of high-speed railways and the increasing operational mileage of high-speed railways year by year, the expansion of the high-speed railway network and the increase in the service life of rails have made the replacement of aluminothermic welded joints and some damaged rails, which are weak links in the line, an urgent problem to be solved by railway maintenance departments.

[0003] Currently, the common method for handling welded joints and severely damaged rails is to use flash welding for inserting short rails. However, it's important to note that flash welding for inserting short rails often uses new rails, which can lead to wear (primarily sagging wear) and profile inconsistencies between the inserted rail and existing track rails. For high-speed railways, abrupt changes in track smoothness and improper wheel-rail matching are major causes of abnormal vibrations in train sets. The straightness of the welded joint and the rail profile, as crucial components of the wheel-rail relationship, significantly impact the operational quality of train sets.

[0004] In view of this, based on years of experience in production and design in this and related fields, the inventor has designed an insertion welding method based on existing railway lines through repeated experiments, in order to solve the problems existing in the prior art. Summary of the Invention

[0005] The purpose of this invention is to provide an insertion welding method based on existing railway lines, which can effectively avoid abrupt changes in the profile of the inserted rail and the surrounding existing rails.

[0006] To achieve the above objectives, this invention proposes an insertion welding method based on existing railway lines, wherein the insertion welding method includes:

[0007] The height of the rail head of the inserted rail and the corresponding existing rail are measured at both ends of the inserted rail and respectively to obtain the height of the rail head of the existing rail.

[0008] The difference in rail head height between the inserted rail and the existing rail is calculated based on the rail head height of the inserted rail and the rail head height of the existing rail.

[0009] The straightness preprocessing of the inserted rail is performed based on the rail head height difference;

[0010] The pre-treated straightness of the insertion rail is placed in the insertion welding section of the existing wire rail and insertion welding is performed.

[0011] Compared with the prior art, the present invention has the following features and advantages:

[0012] The proposed insertion welding method based on existing railway lines involves measuring the rail heads of both the existing and inserted rails to obtain the height difference between their rail heads. The inserted rail is then ground according to this height difference to match the height of the rail head of the existing rail. This effectively reduces the height difference between the inserted and existing rails, minimizes abrupt changes in track straightness caused by flash welding, ensures longitudinal smoothness of the track, reduces abnormal vibrations in the train after rail insertion, and guarantees the operational quality of the train. Attached Figure Description

[0013] The accompanying drawings described herein are for illustrative purposes only and are not intended to limit the scope of the invention in any way. Furthermore, the shapes and proportions of the components in the drawings are merely illustrative to aid in understanding the invention and do not specifically limit the shapes and proportions of the components. Those skilled in the art, guided by the teachings of this invention, can select various possible shapes and proportions to implement the invention according to specific circumstances.

[0014] Figure 1 This is a schematic diagram of the pre-processing of the straightness of the insertion rail end in this invention;

[0015] Figure 2 A schematic diagram (I) illustrating the determination of the target profile of the insertion track according to the present invention;

[0016] Figure 3 Schematic diagram (II) for determining the target profile of the insertion track according to the present invention;

[0017] Figure 4 This is a schematic flowchart of the insertion welding method of the present invention;

[0018] Figure 5 This is a schematic diagram of the insertion rail pre-matching process of the present invention. Detailed Implementation

[0019] The details of the present invention can be more clearly understood by referring to the accompanying drawings and the description of specific embodiments. However, the specific embodiments of the present invention described herein are for illustrative purposes only and should not be construed as limiting the invention in any way. Under the teachings of this invention, those skilled in the art can conceive of any possible modifications based on the invention, and these should all be considered to fall within the scope of the invention.

[0020] like Figure 4 As shown, this invention proposes an insertion welding method based on existing railway lines, wherein the insertion welding method includes:

[0021] The height of the rail head of the inserted rail and the corresponding existing rail are measured at both ends of the inserted rail and respectively to obtain the height of the rail head of the existing rail.

[0022] The difference in rail head height between the inserted rail and the existing rail is calculated based on the rail head height of the inserted rail and the existing rail.

[0023] The straightness pre-processing of the inserted rail is performed based on the rail head height difference;

[0024] The pre-treated straightness of the insertion rail is placed in the insertion welding section of the existing rail and insertion welding is carried out.

[0025] The proposed insertion welding method based on existing railway lines involves measuring the rail head of both the existing and inserted rails to obtain the height difference between their rail heads. The inserted rail is then ground according to this height difference, making its rail head height closer to that of the existing rail. This avoids abrupt changes in straightness at the weld joint, thereby preventing abnormal vibrations in the train after rail insertion, improving the stability of train operation, and ensuring the quality of train operation.

[0026] The insertion welding method based on existing railway lines proposed in this invention effectively combines grinding and welding practices, which not only facilitates on-site construction operations but also effectively improves the straightness of the welded rails, thus having practical application significance.

[0027] In an optional embodiment of the present invention, such as Figure 5As shown, the insertion welding method further includes: measuring the profiles of the inserted rail and the existing line rail respectively to obtain the rail head parameters of the inserted rail and the existing line rail; calculating the target profile parameters of the inserted rail based on the rail head parameters of the existing line rail and the inserted rail; and performing profile pre-matching on the inserted rail based on the target profile parameters. In this embodiment, not only is the rail head height difference between the existing line rail and the inserted rail accurately measured, but profile pre-matching technology is also introduced. Based on this, the inserted rail is meticulously ground according to the rail head height difference. In this way, the rail head height of the inserted rail is close to that of the existing line rail, and the profile of the inserted rail is also similar to that of the existing line rail, ensuring that the rail head height of the inserted rail is more matched with that of the existing rail. This effectively avoids abrupt changes in the track profile at the welding point, ensures the longitudinal smoothness of the track line, and further guarantees the stability of the EMU operation. Through the aforementioned precise and meticulous processing, not only can the service life of the track be extended and the safety of train operation improved, but a smoother and more comfortable riding experience can also be provided for passengers. In an optional example of this implementation method, the specific method for measuring the profile of the inserted rail and the rail head profile of the existing line rail can be contact measurement or non-contact measurement, ensuring that the measurement accuracy is ≤0.10mm. The content of the measurement, i.e., the rail head parameters, includes the rail head thickness, profile, and rail base slope of the inserted rail and the existing line rail. Then, based on the rail head parameters of the existing line rail and the inserted rail, the target profile parameters of the inserted rail are calculated to determine the profile shape that the inserted rail should achieve after grinding.

[0028] In one optional example, the measured profile of the existing rail is aligned with its highest point and overlapped 16mm below the rail. The centerline is then extracted and used as the target profile for the inserted rail.

[0029] In one optional example of this implementation,

[0030] In one alternative example, profile pre-matching of the insert rail includes: calculating the profile grinding workload of the insert rail based on the target profile parameters; and grinding the insert rail according to the profile grinding workload.

[0031] Specifically, such as Figure 2 , Figure 3As shown, before the insertion welding construction, to ensure a smooth connection between the profiles of the inserted rail and the existing rail, the profiles of the existing rail on both sides of the inserted rail are measured. The measurement location is a distance D from both ends of the inserted rail, with D ranging from 2 to 3 meters. One measurement is taken on each side, and these are recorded as existing rail profile 1 and existing rail profile 3, respectively. The measured existing rail profiles 1 and 3 are aligned using the method of aligning their highest points and coinciding at 16 mm below the rail (i.e., the gauge point). The centerline of the two profile curves is then extracted, and the extracted centerline is called centerline profile 2. Centerline profile 2 is used as the target profile of the inserted rail.

[0032] Based on the measured existing rail profiles 1 and 3, a centerline profile 2 is generated within the range of -20 to +32 mm on the horizontal axis (or a grinding angle of -10° to +50°), serving as the target profile for grinding the inserted rail. The inserted rail profile is measured, and based on the difference between the measured profile and the target profile (centerline profile 2), the grinding workload for each angle within the -10° to +50° grinding angle range is determined.

[0033] In this invention, pre-matching the profile of the insertion rail can improve the profile matching degree between the ground insertion rail and the existing rail, thereby improving welding quality and reducing subsequent maintenance costs.

[0034] In one optional example, the profile must at least include the original rail base slope; that is, the measured rail profile must include its original rail base slope. The original rail base slope can be measured using contact or non-contact methods, ensuring a measurement accuracy of ≤0.10mm. Before the insertion welding is performed, the profile of the existing rails on both sides of the inserted rail should be measured again, and the measured profile must include the rail base slope.

[0035] In an optional example, profile pre-matching of the insert rail also includes: evaluating the profile quality of the insert rail after profile grinding. Before insertion welding, the rail head thickness of the insert rail and the existing rail is first measured to confirm the height difference between the rail heads of the insert rail and the existing rail. Measurement methods can include calipers or profile gauges. After determining the height difference, the reserved value h of the rail head height difference is determined according to the design speed of the line. Since the welding head is not allowed to collapse, the reserved value h of the rail head height difference should not be greater than the measured rail top height difference H1 and H2. The insert rail undergoes straightness pre-treatment. Under the design standard of 350km / h high-speed railway, the gradient can be taken as 0.20‰. At this time, the maximum grinding amount at the head end of the insert rail is 0.6mm, and the grinding length L1 is 3m. The maximum grinding amount at the tail end of the insert rail is 0.5mm, and the grinding length L2 is 2.5m. After grinding, a 1-meter straightness ruler is used for inspection to ensure that the straightness measurement of the ground area meets the requirement of not exceeding 0.2mm / 1m, thus completing the straightness pre-matching of the insert rail. During the profile pre-matching grinding operation of the insert rail, the quality of the profile pre-matching needs to be evaluated. The evaluation method is as follows: using the centerline profile 2 as the target profile of the insert rail, the profile pre-matching quality of the insert rail is evaluated using the rail profile quality evaluation method in patent ZL201910299181.5. n measuring points are randomly selected on the insert rail, with n ranging from 1 to 3 according to the design speed of the line. It is necessary to ensure that the rail profile quality index at each measuring point of the insert rail is not less than 80 as specified in patent ZL201910299181.5. At this point, the profile pre-matching grinding operation of the insert rail is considered qualified. Through the above steps, the profile pre-matching of the insert rail can be effectively performed, and its quality can be evaluated after completion. This helps ensure a smooth connection between the inserted rail and the existing rails, improving the stability and safety of the line.

[0036] In an optional embodiment of the present invention, the straightness pretreatment of the insertion rail includes: calculating the straightness grinding workload of the insertion rail based on the rail head height difference; and grinding the insertion rail according to the straightness grinding workload.

[0037] First, the height difference between the inserted rail and the adjacent existing rail needs to be measured. This measurement is usually performed near the predetermined welding position of the inserted rail, using precision measuring instruments (such as laser rangefinders or rail inspection instruments) to ensure accuracy. After the measurement is completed, the specific value of the rail head height difference is recorded.

[0038] Subsequently, based on the measured rail head height difference, the amount of straightness grinding required for the inserted rail is calculated. This calculation typically needs to be based on engineering design standards, taking into account factors such as the line's operating speed and track geometry. The calculation results will determine the grinding depth, width, and total length to be ground.

[0039] Then, based on the calculated straightness grinding workload, specialized rail grinding equipment is used to grind the inserted rails. During the grinding process, grinding parameters, including grinding depth, width, and speed, need to be strictly controlled to ensure accuracy and consistency. Simultaneously, the straightness changes of the rail head need to be continuously monitored during grinding to adjust the grinding parameters promptly.

[0040] After grinding, the straightness of the insert rail is checked again to ensure it meets design requirements. If necessary, local grinding or fine adjustments can be made to further improve the smoothness of the rail.

[0041] In this invention, by performing straightness pretreatment on the inserted rail, the height difference of the rail head can be eliminated, the longitudinal smoothness of the rail can be improved, and the rails on both sides of the welded joint can be ensured to have consistent geometric shape and dimensional accuracy. This helps to reduce welding deformation and welding defects, and improve the quality and reliability of the welded joint.

[0042] In one alternative embodiment of this implementation, the flatness grinding workload includes the maximum vertical grinding amount and the grinding section length.

[0043] The maximum vertical grinding depth refers to the maximum vertical grinding depth allowed on the rail head during the straightness pretreatment of the inserted rail. Determining this parameter requires comprehensive consideration of multiple factors, including the height difference between the rail head of the inserted rail and the existing rail, track design requirements, operating speed, and the characteristics of the rail material. First, the height difference between the rail head of the inserted rail and the existing rail needs to be measured. Then, based on design requirements and operating speed, a suitable maximum vertical grinding depth is determined. This value should ensure a smooth height transition between the ground inserted rail and the existing rail, while avoiding excessive grinding that could reduce rail strength or shorten its service life.

[0044] The grinding section length refers to the length range of the inserted rail that needs to be ground for straightness. Determining this parameter requires comprehensive consideration of multiple factors, including the connection between the inserted rail and the existing rail, the track geometry, the performance of the grinding equipment, and construction efficiency. A suitable grinding section length needs to be determined based on the actual situation. This length should ensure coverage of all areas requiring grinding, while facilitating construction operations and the effective use of the grinding equipment. The determination of the grinding section length also needs to consider factors such as construction efficiency and cost to achieve the best engineering results.

[0045] By defining the maximum vertical grinding amount, the amount of material removed during grinding can be precisely controlled, avoiding over-grinding or under-grinding, and helping to ensure that the ground track meets the smoothness requirements in the design standards. By determining the length of the grinding section, the scope and progress of the grinding operation can be rationally planned, improving grinding efficiency.

[0046] In one optional example, the formula for calculating the maximum vertical sanding amount is:

[0047] H max =H n -h,

[0048] In the formula, Hmax is the maximum vertical grinding amount; Hn is the height difference between the end of the inserted rail and the corresponding existing rail head; h is the reserved value for the height difference between the inserted rail and the existing rail head, and its reserved range is 0.3 to 1 mm.

[0049] Specifically, the height difference between the end of the inserted rail and the corresponding existing rail head is accurately measured using professional measuring equipment (such as a laser rangefinder and rail inspection instrument), denoted as Hn. Based on design requirements and practical engineering experience, the allowable height difference h between the inserted rail and the existing rail head is determined. The allowable value h is set to ensure that a certain safety margin is maintained between the inserted rail and the existing rail after grinding, avoiding new problems caused by over-grinding. The allowable value h is usually set between 0.3 and 1 mm, and the specific value can be adjusted according to the actual situation.

[0050] Hmax represents the maximum allowable amount of material to be removed in the vertical direction, which directly guides subsequent grinding operations.

[0051] Based on the Hmax value calculated using the above formula, the inserted rail is ground vertically using professional rail grinding equipment. During the grinding process, the grinding depth must be strictly controlled to ensure it does not exceed the Hmax value, while also ensuring the uniformity and smoothness of the grinding. The above calculation formula accurately determines the maximum grinding depth required (i.e., the amount of material removed vertically), thus avoiding under-grinding or over-grinding.

[0052] In an optional example, such as Figure 1 As shown, the formula for calculating the length of the grinding section of the insertion rail is:

[0053] L n =(H n -h) / a,

[0054] In the formula, Hn is the height difference between the end of the inserted rail and the corresponding rail head of the existing line; h is the reserved value for the height difference between the inserted rail and the rail head of the existing line, which is 0.3 to 1 mm; a is the gradient, which is 0.10‰ to 0.30‰.

[0055] Specifically, the height difference between the end of the inserted rail and the corresponding existing rail head is accurately measured using professional measuring equipment (such as laser rangefinders and rail inspection instruments), denoted as Hn. Based on design standards and engineering practice, a suitable reserved height difference value h is selected. The reserved height difference h ensures that the ground rail still maintains a certain safety margin, and its value is usually in the range of 0.3 to 1 mm. The gradient a refers to the ratio of the smooth transition of the rail height difference within the grinding section. A suitable gradient value is selected within the range of 0.10‰ to 0.30‰ based on engineering requirements and actual conditions. The selection of the gradient directly affects the length of the grinding section and the smoothness of the rail. Ln represents the length of the rail to be ground, which is determined based on the measured height difference Hn, the reserved height difference h, and the set gradient a. Based on the calculated grinding section length Ln, professional rail grinding equipment is used to perform the corresponding grinding operation on the inserted rail. During the grinding process, the grinding depth and range must be strictly controlled to ensure compliance with design requirements. By comprehensively considering the rail head height difference, the reserved height difference, and the gradient, the above formula can accurately calculate the length of the rail that needs to be ground, avoiding grinding sections that are too long or too short.

[0056] In an optional embodiment of the present invention, after the insertion rail is placed in the insertion welding construction section of the existing rail, the existing rail is cut, and the length of the cut is less than the length of the insertion rail.

[0057] It should be noted that preparatory work is required before cutting. This includes: confirming the model, size, and compatibility of the insert rail and the existing rail; performing necessary pretreatment on the insert rail, such as straightness adjustment, rust removal, and cleaning; and preparing welding equipment and cutting tools, such as welding machines, cutting machines, and clamps. After completing the preparatory work, the pretreated insert rail is accurately placed at the designated insertion position on the existing rail.

[0058] During the cutting process, use clamps or other fixing devices to securely fix the insert rail to the existing rail, ensuring accurate relative positioning. Cut the existing rail in the overlapping area. The cut length must be less than the length of the insert rail to ensure that both ends of the existing rail can be welded to the insert rail after cutting. During the cutting process, ensure the cut surface is flat and perpendicular to facilitate subsequent welding operations.

[0059] After cutting, the cut ends of the existing rails and the corresponding ends of the inserted rails can be welded together. During welding, welding parameters such as welding current, welding speed, and preheating temperature must be strictly controlled to ensure welding quality. By preparing and precisely placing the inserted rails in advance, and then cutting the existing rails in a planned manner, adjustment time and workload during construction can be reduced, thereby improving construction efficiency.

[0060] Please refer to Figures 1 to 3 The specific implementation process of the present invention will now be described in detail with reference to an embodiment:

[0061] (1) Before the insertion welding construction, the thickness of the rail head of the insertion rail and the existing rail should be measured first to confirm the height difference of the rail head between the insertion rail and the existing rail. The measurement method can be calipers or profile gauges. The measured height differences between the head and tail ends of the insertion rail and the existing rail are H1 and H2, respectively. It is assumed that the measured height differences H1 and H2 are 0.9mm and 0.8mm, respectively.

[0062] (2) After determining the height difference, determine the reserved value h of the rail head height difference according to the design speed of the line. Since the welding machine head is not allowed to collapse, the reserved value h of the rail head height difference should not be greater than the measured rail top height difference H1 and H2. Assume that the construction line is a high-speed railway with a design standard of 350km / h, and the value of h is taken as 0.3mm.

[0063] (3) Perform straightness pretreatment on the insert rail. Under the design standard of 350km / h high-speed railway, the gradient can be taken as 0.20‰. At this time, the maximum grinding amount at the head end of the insert rail is 0.6mm, and the grinding length L1 is 3m. The maximum grinding amount at the tail end of the insert rail is 0.5mm, and the grinding length L2 is 2.5m. After grinding, use a 1-meter straightness ruler to check and ensure that the straightness measurement of the grinding area meets the requirement of not exceeding 0.2mm / 1m, thus completing the straightness pre-matching of the insert rail.

[0064] (4) Before the insertion welding construction, the profile of the existing rail on both sides of the insertion rail shall be measured again. Contact or non-contact measurement can be used. The measured profile must include the rail bottom slope. Based on the measured existing rail profile 1 and existing rail profile 3, generate the centerline profile 2 within the range of -20 to +32 mm on the horizontal axis (or the grinding angle is -10° to +50°), and use it as the grinding target profile of the insertion rail.

[0065] (5) Measure the profile of the inserted rail. Based on the difference between the measured profile of the inserted rail and the target profile (i.e., centerline profile 2), determine the grinding amount of the inserted rail at each angle within the grinding angle range of -10° to +50°. After grinding, the grinding quality of the inserted rail is evaluated using the rail profile quality evaluation method in patent ZL201910299181.5. For a high-speed railway with a design standard of 350km / h, the evaluation adopts the method of randomly selecting 3 measuring points on the inserted rail to ensure that the profile quality index of each measuring point is not less than 80, thus completing the profile pre-matching of the inserted rail.

[0066] (6) Transport the pre-treated insertion rail to the insertion welding construction section, cut the old rail at the insertion position, and the cutting length should not be greater than the insertion rail length. The design standard for 350km / h high-speed railway requires the insertion rail length to be generally not less than 22m, so the length of the old rail to be cut for welding is 21m.

[0067] (7) After the old rail is cut, the insert rail and the adjacent existing line cutting surface are supported, rusted, and aligned to complete the welding of the insert rail head end. After the insert rail head end is welded, the welding machine moves to the insert rail tail end position, and then, according to the welding condition of the head rail, the tail rail is sawed, rusted, and aligned again to complete the welding of the insert rail tail end.

[0068] (8) After the welding of the head and tail joints of the insert rail is completed, the two joints are normalized, ground, and inspected for defects, and the rail is then reset. After the rail is reset, the geometric dimensions of the track in the welding construction section are finely adjusted to ensure that all indicators meet the requirements, and the flash welding of the insert rail of the existing high-speed railway line is finally completed.

[0069] The detailed explanations of the above embodiments are intended only to explain the present invention so as to facilitate a better understanding of the present invention. However, these descriptions should not be construed as limiting the present invention for any reason. In particular, the various features described in different embodiments can be arbitrarily combined with each other to form other embodiments. Unless there is an explicit description to the contrary, these features should be understood to be applicable to any embodiment, and not limited to the described embodiments.

Claims

1. A method of inserting welding based on an existing railway line, characterized by, The insertion welding method includes: The height of the rail head of the inserted rail and the corresponding existing rail are measured at both ends of the inserted rail and respectively to obtain the height of the rail head of the existing rail. The difference in rail head height between the inserted rail and the existing rail is calculated based on the rail head height of the inserted rail and the rail head height of the existing rail. The straightness preprocessing of the inserted rail is performed based on the rail head height difference; The pre-treated straightness rail is placed in the insertion welding section of the existing rail and insertion welding is performed. The straightness preprocessing of the inserted rail includes: The amount of grinding work required to achieve the straightness of the inserted rail is calculated based on the height difference of the rail head. The insertion rail is ground according to the required flatness grinding workload; The flatness grinding workload includes the maximum vertical grinding amount and the length of the grinding section; The formula for calculating the maximum vertical grinding amount is: H max =H n -h In the formula, H max is the maximum vertical polishing amount; H n is the height difference between the end of the inserted rail and the corresponding rail head of the existing rail; h is the height difference between the inserted rail and the existing rail head, and the reserved range is 0.3-1 mm; The formula for calculating the length of the grinding section of the insertion rail is: L n = (H n -h) / a In the formula, H n is the height difference between the end of the inserted rail and the corresponding rail head of the existing rail; h is the height difference between the inserted rail and the existing rail head, and the reserved range is 0.3-1 mm; a is the slope ratio, and the value range is 0.10‰-0.30‰.

2. The insert welding method of claim 1, wherein The insertion welding method further includes: The profiles of the inserted rail and the existing rail are measured respectively to obtain the rail head parameters of the inserted rail and the existing rail. The target profile parameters of the inserted rail are calculated based on the rail head parameters of the existing rail and the rail head parameters of the inserted rail. The insertion rail is pre-matched in profile according to the profile target parameters of the insertion rail.

3. The insert welding method of claim 2, wherein Pre-matching the profile of the insertion rail includes: The profile grinding workload of the insertion rail is calculated based on the target profile parameters; The insertion rail is ground according to the required grinding workload for the profile.

4. The insertion welding method as described in claim 3, characterized in that, The profile includes at least the original track bottom slope.

5. The insert welding method of claim 3, wherein Pre-matching the profile of the insertion rail also includes: After the profile is polished, the profile quality of the insertion rail is evaluated.

6. The insert welding method of claim 1 wherein, After the insertion rail is placed in the insertion welding section of the existing rail, the existing rail is cut, and the length of the cut is less than the length of the insertion rail.

Citation Information

Patent Citations

  • Railway steel rail profile quality evaluation method

    CN109989309A

  • Accurate checking and grinding process for flash welding of steel rail

    CN111037074A

  • Cladding strengthening and toughening treatment method for steel rail welded joint and application of method

    CN113584971A