A method for recovering selenium and mercury from smelting acid mud by two-stage oxidation acid leaching
Through the two-stage oxidation acid leaching grading method, selenium oxide is oxidized by sulfuric acid and hydrogen peroxide and reduced by SO2, combined with the characteristics of mercury sulfate, the high energy consumption and recovery rate in selenium mercury recovery technology in acid sludge is solved. The problem of low and large waste production has achieved efficient and low energy consumption selenium mercury recycling and product purity improvement.
Patent Information
- Application Number
- CN202410030748.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-09
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-01-09
AI Technical Summary
The existing selenium mercury recovery technology in acid sludge has problems such as high energy consumption, low recovery rate, low product purity and large waste production, especially the lack of energy consumption and pollution control of ignition and wet processes.
The two-stage oxidized acid leaching grading method is used to oxidize and leaching the low-priced selenium in the acid sludge through sulfuric acid and hydrogen peroxide. Then, SO2 is used to reduce it to the elemental selenium, and the mercury in the leaching slag is dissolved and precipitated by the characteristics of mercury sulfate. Efficient recycling of selenium and mercury is carried out separately, reducing the use of auxiliary reagents and waste production.
It realizes efficient recycling of selenium and mercury, improves product purity, reduces energy consumption and waste production, and all stages of processes can be recycled, and almost no new waste is generated, solving the high energy consumption and low recovery rate in the existing technology. , the problem of low product purity and large waste production.
Smart Images

Figure CN117843027B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solid waste, hazardous waste disposal and valuable component recovery, and specifically relates to a method for recovering selenium and mercury in smelting acid mud by two-stage oxidation acid leaching and classification. Background Art
[0002] Smelting acid mud is an inevitable product in the non-ferrous metal smelting process, and the amount of production is large. The water content of acid mud is about 20%, and it contains 5-30% selenium, 5-40% mercury, 20-28% lead, 0.1-1.5% silver, and a small amount of copper and zinc. The selenium and mercury contained in acid mud have extremely high economic value.
[0003] The existing technology for recovering selenium and mercury from acid mud has high energy consumption, low efficiency, difficult classification, and large waste production. In the currently used methods for recovering selenium and mercury from acid mud, mercury is mainly treated by pyrolysis, and selenium is mainly treated by wet processing. The most widely used process flow is calcium addition to fix selenium to collect mercury-oxidation leaching-reduction precipitation of selenium. It mainly uses acid mud and calcium oxide to mix and roast to generate calcium selenite, and mercury escapes in the form of steam. After condensation by the condensation system, mercury and selenium are separated; the generated steamed mercury slag is further leached with sulfuric acid, and a reducing agent is introduced into the filtrate to obtain crude selenium. However, the pyrolysis method consumes 1000-1300GJ of coal gas per ton of acid mud, which has high energy consumption and does not meet the requirements of energy conservation, carbon reduction and environmental protection, and the escape of mercury vapor is extremely difficult to control; in addition, in the roasting process, selenium not only generates CaSeO3, but also forms PbSeO3, resulting in a low subsequent selenium leaching rate, and the selenium recovery rate is only 80%; the solid selenium process requires the addition of lime 10 times the mass of acid mud, and the slag production is large. In order to overcome the shortcomings of the above methods, researchers have developed a fully wet method for recovering selenium and mercury in recent years, that is, using mixed acid and oxidant to leach selenium and mercury in acid mud in a one-step method, and recover mercury and selenium in steps by step-by-step precipitation and / or reduction. The energy consumption of the wet treatment process is lower than that of the pyrolysis process, but due to the complex composition of the acid mud, in order to obtain a satisfactory leaching rate, it is necessary to add 10 times excess potassium chlorate, sodium chlorate and other auxiliary reagents, which are expensive and consume a lot, resulting in increased process costs; because the liquid-to-solid ratio of the leaching process is higher than 10:1, and even reaches 20:1, after recovering selenium and mercury, 10-20m 3 The high-salinity mixed acid tail liquid cannot be recycled and still needs lime neutralization treatment. For every ton of acid mud treated, 1-3 tons of gypsum slag will be produced, which greatly increases the amount and difficulty of solid waste disposal. Due to the existence of the above problems, the full wet process technology is currently only in laboratory research and has not yet been put into production.
[0004] In view of the current situation that there is a lack of high recovery rate, high product purity, low energy consumption and low waste generation technology for the recovery of selenium and mercury in acid sludge, a method of secondary oxidation acid leaching for graded recovery of selenium and mercury in acid sludge is proposed. Summary of the invention
[0005] In order to solve the technical problems of high energy consumption, low recovery rate, low product purity and large waste generation in the existing acid mud disposal methods and realize the efficient and high-quality graded recovery of selenium and mercury in acid mud, the present invention provides a method for graded recovery of selenium and mercury in smelting acid mud by two-stage oxidation acid leaching.
[0006] The technical solution provided by the present invention is as follows:
[0007] The method for recovering selenium and mercury from smelting acid mud by two-stage oxidation acid leaching comprises two processing steps.
[0008] The first stage is the leaching and recovery of selenium.
[0009] Use sulfuric acid and hydrogen peroxide to oxidize the low-valent selenium in the acid mud into a high-valent state and leach it in the form of selenious acid (H2SeO3) (reaction formula 1-3), collect the selenium leaching solution, and then use SO2 to reduce the selenious acid to elemental selenium (reaction formula 4). The released hydrogen ions react with the oxidized SO2 to form sulfuric acid, and after solid-liquid separation, a crude selenium product and sulfuric acid tail liquid are obtained. The sulfuric acid tail liquid can be reused in this leaching stage.
[0010] After the first stage of leaching, the mercury in the acid mud is converted into mercuric sulfate (HgSO4) and continues to remain in the leaching residue and enters the second stage of leaching process.
[0011] Se+2H2O2→H2SeO3+H2O (1)
[0012] HgSe+3H2O2+H2SO4→H2SeO3+HgSO4(↓)+3H2O (2)
[0013] PbSe+3H2O2+H2SO4→H2SeO3+PbSO4(↓)+3H2O (3)
[0014] H2SeO3+2SO2+H2O→Se(↓)+2H2SO4 (4)
[0015] The second stage is to leach and recover mercury. The mercury sulfate in the leaching residue is dissolved in hydrochloric acid using the property that mercury sulfate is soluble in hydrochloric acid (reaction formula 5), and the mercury leachate is collected. Then, H2S is used to convert mercuric chloride into HgS precipitation (reaction formula 6). At the same time, the released hydrogen ions react with the chloride ions in the leachate to form hydrochloric acid. After solid-liquid separation, HgS products and hydrochloric acid tail liquid are obtained. The hydrochloric acid can be reused in this stage of mercury leaching. After two stages of leaching, lead sulfate continues to remain in the leaching residue and can be returned to the zinc smelting system for recovery.
[0016] HgSO4+2HCl→HgCl2+H2SO4 (5)
[0017] HgCl2+H2S →HgS(↓)+2HCl (6)
[0018] The whole flow chart is shown in Figure 1.
[0019] The above scheme provided by the present invention is processed in two steps. The first step is to leach and recover selenium separately, and the second step is to leach and recover mercury separately. The two steps are highly independent, and the recovery of selenium and mercury does not affect each other.
[0020] The acidic tail liquid of the above scheme provided by the present invention can be recycled to the leaching process respectively, and the lead-rich slag produced can be returned to the lead smelting process to realize the recovery of valuable metals such as lead, and the whole process hardly generates new waste.
[0021] The method for recovering selenium and mercury from smelting acid mud by two-stage oxidation acid leaching comprises the following steps:
[0022] S1. Take a certain mass of acid mud, add sulfuric acid and hydrogen peroxide, the mass ratio of sulfuric acid to hydrogen peroxide = 1:2-2:1, the mass ratio of sulfuric acid to selenium = 1:1-8:1, the liquid-solid ratio = 4:1-10:1, react at 60°C-100°C, and mix evenly; the above-mentioned proportion of dosage and the above-mentioned reaction conditions can ensure that the selenium leaching rate reaches more than 95%;
[0023] S2, after reacting for 4-8 hours, perform solid-liquid separation to obtain selenium leaching solution and selenium leaching residue respectively;
[0024] S3, passing SO2 gas into the selenium leaching solution, wherein the molar ratio of SO2 to Se in the selenium leaching solution is 1:1-2:1, reacting at room temperature for 1-2 hours, obtaining elemental selenium precipitate and sulfuric acid solution; solid-liquid separation, collecting elemental selenium product and sulfuric acid tail liquid; sulfuric acid can be added in the form of dilute sulfuric acid, or in the form of recycling the sulfuric acid tail liquid to S1; the above-mentioned proportion of dosage and the above-mentioned reaction conditions can ensure that the recovery rate of selenium in the selenium leaching solution is more than 96%;
[0025] S4, adding 2-6 mol / L hydrochloric acid to the selenium leaching residue, the mass ratio of hydrochloric acid to mercury in the selenium leaching residue is 4:1-8:1, the liquid-solid ratio is 4:1-10:1, reacting at 60°C-90°C, and uniformly mixing; the above-mentioned proportion of dosage and the above-mentioned reaction conditions can ensure that the leaching rate of mercury is more than 95%;
[0026] S5, after reacting for 4-8 hours, perform solid-liquid separation to obtain mercury leaching solution and mercury leaching residue respectively;
[0027] S6, passing H2S gas into the mercury leachate, with the molar ratio of S to Hg in the mercury leachate being 1:1-2:1, reacting at room temperature for 1-4 hours to obtain mercuric sulfide precipitate and hydrochloric acid; then performing solid-liquid separation, collecting the mercuric sulfide product and hydrochloric acid tail liquid; the hydrochloric acid can be added in the form of a dilute hydrochloric acid solution, or in the form of recycling the hydrochloric acid tail liquid to S4; the above-mentioned proportion of dosage and the above-mentioned reaction conditions can ensure a recovery rate of mercury in the mercury leachate of more than 96%;
[0028] S7, returning the mercury leaching slag to the lead-zinc smelting process to further recover valuable elements such as lead and silver.
[0029] The method for recovering selenium and mercury from smelting acid mud by two-stage oxidation acid leaching provided by the present invention has a wide application range, and is applicable to but not limited to: smelting acid mud with a water content of about 20%, 5-30% selenium, 5-40% mercury, 20-28% lead, and 0.1-1.5% silver.
[0030] The beneficial effects of the present invention are:
[0031] 1. Selenium has a very high reaction and solubility in a sulfuric acid + oxidant system, and mercury and its compounds have a very high reaction and solubility in a hydrochloric acid system. First, a segmented leaching method is used to separate selenium and mercury in the leaching stage, and then they are recovered separately. This is not only conducive to improving the leaching efficiency of selenium and mercury, but also improves the purity of the recovered products. The leaching efficiency of selenium and mercury can reach more than 95%, which is better than the leaching rate of more than 85% of conventional wet leaching; and the product purity of selenium and mercuric sulfide can reach 97%, which is also better than the 80% purity of conventional wet recovery products.
[0032] 2. Use SO2 to reduce selenic acid in the selenium leaching solution. SO2 itself is oxidized and reacts with H in selenic acid. + They combine to form sulfuric acid, which is the main component of the selenium leaching solution and can be recycled to the selenium leaching step.
[0033] 3. Use H2S to recover the mercury in the mercury immersion solution by sulfide precipitation to avoid the introduction of other impurity ions. The S in H2S reacts with Hg to form HgS precipitation, in which H + With Cl - The formed HCl is the main component of the mercury leaching solution and can be recycled to the mercury leaching step.
[0034] 4. The lead and silver in the acid mud form insoluble lead sulfate and silver sulfate precipitates in the first leaching process. They are insoluble in hydrochloric acid in the second leaching process and are always retained in the leaching residue. They are enriched and concentrated and can be returned to the lead-zinc smelting process for complete recovery.
[0035] 5. The present invention combines two-stage processes for recovering selenium and mercury separately, so that the entire process achieves efficient recovery of selenium and mercury, and each stage of the process can be optimized according to the situation of smelting acid mud, thereby obtaining process conditions without secondary pollution, that is, achieving the effect of efficient recovery of selenium and mercury, and having the advantage of no secondary pollution in the entire process.
[0036] The segmented leaching and graded recovery method of selenium and mercury in acid mud of the present invention not only efficiently recovers selenium and mercury, but also enriches and recovers lead and silver, and almost no new waste is generated in the whole process, thus solving the technical problems of high energy consumption, low recovery rate, low product purity and large waste generation in the existing acid mud disposal method, and generating excellent economic and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 The present invention provides a two-stage oxidation acid leaching method for recovering selenium and mercury from smelting acid mud. DETAILED DESCRIPTION
[0038] The principles and features of the present invention are described below. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.
[0039] The method for recovering selenium and mercury from smelting acid mud by two-stage oxidation acid leaching comprises the following steps:
[0040] S1. Take a certain mass of acid mud, add sulfuric acid and hydrogen peroxide, the mass ratio of sulfuric acid to hydrogen peroxide = 1:2-2:1, the mass ratio of sulfuric acid to selenium = 1:1-8:1, the liquid-solid ratio = 4:1-10:1, react at 60°C-100°C, and mix evenly;
[0041] S2, after reacting for 4-8 hours, perform solid-liquid separation to obtain selenium leaching solution and selenium leaching residue respectively;
[0042] S3, passing SO2 gas into the selenium leaching solution, with a molar ratio of SO2 to Se of 1:1-2:1, reacting at room temperature for 1-2 hours to obtain elemental selenium precipitate and sulfuric acid solution; solid-liquid separation, collecting elemental selenium product and sulfuric acid tail liquid; the sulfuric acid tail liquid is recycled to S1;
[0043] S4, adding 2-6 mol / L hydrochloric acid to the selenium leaching residue, with a mass ratio of hydrochloric acid to mercury of 4:1-8:1 and a liquid-solid ratio of 4:1-10:1, reacting at 60° C.-90° C. and mixing evenly;
[0044] S5, after reacting for 4-8 hours, perform solid-liquid separation to obtain mercury leaching solution and mercury leaching residue respectively;
[0045] S6, passing H2S gas into the mercury leachate, with a molar ratio of S to Hg of 1:1-2:1, reacting at room temperature for 1-4 hours to obtain mercuric sulfide precipitate and hydrochloric acid; then separating the solid and liquid, collecting the mercuric sulfide product and hydrochloric acid tail liquid; the hydrochloric acid tail liquid is recycled to S4;
[0046] S7, returning the mercury leaching slag to the lead-zinc smelting process to further recover valuable elements such as lead and silver.
[0047] Example 1
[0048] One-stage treatment: leaching and recovery of selenium.
[0049] Take 100g of acid mud, use X-ray fluorescence spectrometer to detect 10% selenium and 20% mercury, add a certain volume of sulfuric acid and hydrogen peroxide mixture, use a constant temperature water bath magnetic stirrer, react for a certain time under heating conditions of 60-90℃, filter, and obtain selenium leaching solution and selenium leaching residue.
[0050] Take 1L of selenium leaching solution, introduce SO2 gas, continuously monitor the SO2 gas flow and volume, ensure that the SO2 / Se molar ratio is within a certain range, react for 2 hours, filter, and obtain elemental selenium and sulfuric acid solution. The sulfuric acid solution is reused in the leaching acid mud selenium leaching process.
[0051] Table 1 Effect of sulfuric acid and hydrogen peroxide ratio on leaching rate during selenium leaching (liquid-solid ratio = 10:1, temperature = 80 °C, reaction time = 4h)
[0052] Dosage of concentrated sulfuric acid 30% hydrogen peroxide dosage Selenium concentration Selenium leaching rate 600mL 400mL 9.72g / L 97.2% 700mL 300mL 9.82g / L 98.2% 800mL 200mL 9.59g / L 95.9% 900mL 100mL 9.56g / L 95.6% 950mL 50mL 9.53g / L 95.3%
[0053] Table 2 Effect of reaction temperature and reaction time on selenium leaching rate during selenium leaching (concentrated sulfuric acid dosage 800 mL, 30% hydrogen peroxide dosage 200 mL)
[0054] Reaction temperature Reaction time Selenium concentration Selenium leaching rate 60℃ 4h 9.52g / L 95.2% 70℃ 4h 9.54g / L 95.4% 80℃ 4h 9.59g / L 95.9% 90℃ 4h 9.86g / L 98.6% 80℃ 5h 9.73g / L 97.3% 80℃ 6h 9.83g / L 98.3% 80℃ 8h 9.86g / L 98.6%
[0055] Table 3 Effect of liquid-solid ratio on selenium leaching rate during selenium leaching (concentrated sulfuric acid addition volume: 30% hydrogen peroxide addition volume = 4:1, reaction temperature 80°C, reaction time 4h)
[0056] Liquid-to-solid ratio Selenium concentration Selenium leaching rate 4:1 9.82g / L 98.2% 6:1 9.79g / L 97.9% 8:1 9.76g / L 97.6% 10:1 9.59g / L 95.9%
[0057] Table 4 Selenium recovery process, effect of SO2 / Se molar ratio on selenium recovery rate (initial selenium concentration 9.59 g / L)
[0058] <![CDATA[SO2 / Se molar ratio]]> Selenium Residual Concentration Selenium recovery 1:1 0.17 98.2% 1.25:1 0.12 98.7% 1.5:1 0.30 96.9% 1.75:1 0.33 96.6% 2:1 0.26 97.3%
[0059] Tables 1 to 3 show the optimization process of selenium leaching conditions, and Table 4 shows the optimization process of selenium reduction and recovery conditions.
[0060] As can be seen from Table 1, under the conditions of liquid-to-solid ratio of 10:1, reaction temperature of 80°C and reaction time of 4h, the selenium leaching rate can reach more than 95.9% by changing the ratio of sulfuric acid and hydrogen peroxide.
[0061] It can be seen from Table 2 that under the conditions of a liquid-to-solid ratio of 10:1, a reaction temperature of 60-90°C, and a reaction time of 4-8h, the selenium leaching rate can reach more than 95.2%.
[0062] As can be seen from Table 3, under the conditions of 93% concentrated sulfuric acid added volume: 30% hydrogen peroxide added volume = 4:1, reaction temperature 80°C, reaction time 4h, liquid-solid ratio 4:1-10:1, the selenium leaching rate can reach more than 95.9%.
[0063] It can be seen from Table 4 that when the SO2 / Se molar ratio is 1:1-2:1, the recovery rate of selenium in the selenium leaching solution can reach more than 96.6%.
[0064] Secondary treatment: mercury leaching and mercury recovery.
[0065] Collect 100g of selenium leaching residue in multiple batches, add a certain volume of hydrochloric acid solution, use a constant temperature water bath magnetic stirrer, react for a certain time under heating conditions of 60-90°C, filter, and obtain mercury leaching solution and mercury leaching residue.
[0066] Take 1L of mercury leaching solution, introduce H2S gas, continuously monitor the flow rate and volume of H2S gas, ensure that the S / Se molar ratio is within a certain range, react for 2 hours, filter, and obtain mercury sulfide and hydrochloric acid solution. The hydrochloric acid solution is reused in the mercury leaching process of selenium leaching residue.
[0067] Table 5 Effect of hydrochloric acid concentration on leaching rate during mercury leaching (liquid-solid ratio = 10:1, reaction temperature 80°C, reaction time 4h)
[0068] Hydrochloric acid concentration (g / L) Mercury concentration Mercury leaching rate 73 19.26 96.3% 109 19.48 97.4% 146 19.36 96.8% 182 19.3 96.5% 219 19.28 96.4%
[0069] Table 6 Effect of reaction temperature and reaction time on mercury leaching rate during mercury leaching (liquid-solid ratio = 10:1, hydrochloric acid concentration 219 g / L)
[0070] Reaction temperature Reaction time Mercury concentration (g / L) Mercury leaching rate 60℃ 4h 19.26 96.3% 70℃ 4h 19.32 96.6% 80℃ 4h 19.28 96.4% 90℃ 4h 19.5 97.5% 80℃ 5h 19.28 96.4% 80℃ 6h 19.52 97.6% 80℃ 8h 19.54 97.7%
[0071] Table 7 Effect of liquid-solid ratio on mercury leaching rate during mercury leaching (hydrochloric acid concentration 219 g / L, reaction temperature 80°C, reaction time 4 h)
[0072] Liquid-to-solid ratio Mercury concentration (g / L) Mercury leaching rate 4:1 19.26 96.3% 6:1 19.68 98.4% 8:1 19.76 98.8% 10:1 19.28 96.4%
[0073] Table 8 Effect of S / Hg molar ratio on mercury recovery rate during mercury recovery process (initial mercury concentration 19.28 g / L)
[0074] S / Hg molar ratio Mercury residual concentration (g / L) Mercury recovery rate 1:1 0.35 98.2% 1.25:1 0.25 98.7% 1.5:1 0.60 96.9% 1.75:1 0.66 96.6% 2:1 0.52 97.3%
[0075] Tables 5 to 7 show the optimization process of the two-stage mercury leaching conditions, and Table 8 shows the optimization process of the mercury sulfide precipitation recovery conditions.
[0076] It can be seen from Table 5 that under the conditions of liquid-to-solid ratio = 10:1, reaction temperature 80°C, reaction time 4h, hydrochloric acid concentration 73-219g / L, the mercury leaching rate can reach more than 96.3%.
[0077] It can be seen from Table 6 that under the conditions of a liquid-to-solid ratio of 10:1, a hydrochloric acid concentration of 219 g / L, a reaction temperature of 60-90°C, and a reaction time of 4-8 h, the mercury leaching rate can reach more than 96.3%.
[0078] As can be seen from Table 7, under the conditions of hydrochloric acid concentration of 219 g / L, reaction temperature of 80°C, reaction time of 4 h, liquid-solid ratio of 4:1-10:1, the mercury leaching rate can reach more than 96.3%.
[0079] It can be seen from Table 8 that when the S / Hg molar ratio is 1:1-2:1, the recovery rate of mercury in the mercury leaching solution can reach more than 96.6%.
[0080] After the second stage of recovery of selenium and mercury, the remaining residue is returned to the lead and zinc smelting process for recovery of other valuable elements.
[0081] Example 2
[0082] Example of treatment of smelting acid mud with low selenium and mercury content
[0083] One-stage treatment: leaching and recovery of selenium.
[0084] Take 500g of acid mud, use X-ray fluorescence spectrometer to detect 5.5% selenium and 14.1% mercury, add 2L 93% sulfuric acid and 500mL 30% hydrogen peroxide mixture, use constant temperature water bath magnetic stirrer, react at 90℃ for 6h, filter, and obtain selenium leaching solution and selenium leaching residue. The concentration of selenium in the selenium leaching solution is 53.3g / L by inductively coupled plasma emission spectrometry, and the selenium leaching rate is calculated to be 96.9%.
[0085] Take 2L of selenium leaching solution, introduce SO2 gas, continuously monitor the SO2 gas flow and volume, ensure that the SO2 / Se molar ratio is 1.5 / 1, react for 2h, filter, obtain elemental selenium and sulfuric acid solution, and separate the solid and liquid to obtain elemental selenium product and sulfuric acid tail liquid. The residual concentration of selenium in the sulfuric acid solution was determined by inductively coupled plasma emission spectroscopy to be 2.2g / L, and the recovery rate of selenium was calculated to be 95.8%. The sulfuric acid tail liquid was reused in the acid mud selenium leaching process.
[0086] Secondary treatment: mercury leaching and mercury recovery.
[0087] Take 400g of the selenium leaching residue after the first stage of leaching, add 2L of 200g / L hydrochloric acid, use a constant temperature water bath magnetic stirrer, react at 80℃ for 5h, filter, and obtain mercury leaching solution and mercury leaching residue. The mercury concentration in the mercury leaching solution is 135.6g / L using inductively coupled plasma emission spectrometry, and the mercury leaching rate is calculated to be 96.2%.
[0088] Take 2L of mercury leaching liquid, pass H2S gas, continuously monitor the flow rate and volume of H2S gas, ensure that the S / Se molar ratio is 2 / 1, react for 2h, filter, obtain mercury sulfide and hydrochloric acid solution, and separate the solid and liquid to obtain mercury sulfide product and hydrochloric acid tail liquid. The residual concentration of mercury in the hydrochloric acid solution is 2.4g / L determined by inductively coupled plasma emission spectrometry, and the recovery rate of mercury is calculated to be 98.2%. The hydrochloric acid solution is reused in the mercury leaching process of selenium leaching residue.
[0089] Example 3
[0090] Example of treatment of smelting acid mud with high selenium and mercury content
[0091] One-stage treatment: leaching and recovery of selenium.
[0092] Take 1000g of acid mud, use X-ray fluorescence spectrometer to detect 25.5% selenium and 34.1% mercury, add 4L 93% sulfuric acid and 1L 30% hydrogen peroxide mixture, use constant temperature water bath magnetic stirrer, react at 90℃ for 6h, filter, and obtain selenium leaching solution and selenium leaching residue. The concentration of selenium in the selenium leaching solution is 244g / L by inductively coupled plasma emission spectrometry, and the selenium leaching rate is calculated to be 95.7%.
[0093] Take 5L of selenium leaching solution, introduce SO2 gas, continuously monitor the SO2 gas flow and volume, ensure that the SO2 / Se molar ratio is 1.5 / 1, react for 2h, filter, obtain elemental selenium and sulfuric acid solution, and separate the solid and liquid to obtain elemental selenium product and sulfuric acid tail liquid. The residual concentration of selenium in the sulfuric acid solution was determined by inductively coupled plasma emission spectroscopy to be 10.2g / L, and the recovery rate of selenium was calculated to be 95.8%. The sulfuric acid tail liquid was reused in the acid mud selenium leaching process.
[0094] Secondary treatment: mercury leaching and mercury recovery.
[0095] Take 400g of the selenium leaching residue after the first stage of leaching, add 2L of 200g / L hydrochloric acid, use a constant temperature water bath magnetic stirrer, react at 80℃ for 5h, filter, and obtain mercury leaching solution and mercury leaching residue. The mercury concentration in the mercury leaching solution is 328g / L determined by inductively coupled plasma emission spectrometry, and the mercury leaching rate is calculated to be 96.2%.
[0096] Take 2L of mercury leaching liquid, pass H2S gas, continuously monitor the flow rate and volume of H2S gas, ensure that the S / Se molar ratio is 2 / 1, react for 2h, filter, obtain mercuric sulfide and hydrochloric acid solution, and separate the solid and liquid to obtain mercuric sulfide product and hydrochloric acid tail liquid. The residual concentration of mercury in the hydrochloric acid solution is 9.1g / L determined by inductively coupled plasma emission spectrometry, and the recovery rate of mercury is calculated to be 97.2%. The hydrochloric acid solution is reused in the mercury leaching process of selenium leaching residue.
[0097] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for recovering selenium and mercury from smelting acid mud by two-stage oxidation acid leaching, characterized in that: The following steps are involved: 1) First, sulfuric acid and hydrogen peroxide are used to oxidize the low-valent selenium in the smelting acid mud into a high-valent state and leach it in the form of selenious acid, solid-liquid separation is performed, and selenium leaching solution and selenium leaching residue are collected. Subsequently, sulfur dioxide is used to reduce the selenious acid in the selenium leaching solution to elemental selenium, and sulfuric acid is formed in the leaching solution. Then, solid-liquid separation is performed to obtain a crude selenium product and sulfuric acid tail liquid. The mass ratio of sulfuric acid to selenium in the acid mud is 1:1-8:1, and the liquid-solid ratio is 4:1-10:1; 2) using hydrochloric acid to dissolve the mercuric sulfate in the selenium leaching slag obtained in step 1), and performing solid-liquid separation to obtain a mercury leaching solution and mercury leaching slag, and then using hydrogen sulfide to convert the mercuric chloride in the mercury leaching solution into mercuric sulfide precipitate, and forming hydrochloric acid in the tail liquid, and then performing solid-liquid separation to obtain a mercury sulfide product and a hydrochloric acid tail liquid.
2. The method for recovering selenium and mercury from smelting acid mud by two-stage oxidation acid leaching according to claim 1, characterized in that: In step 1), the sulfuric acid used includes sulfuric acid tail liquid.
3. The method for recovering selenium and mercury from smelting acid mud by two-stage oxidation acid leaching according to claim 1, characterized in that: In step 2), the hydrochloric acid used includes hydrochloric acid tail liquid.
4. The method for recovering selenium and mercury from smelting acid mud by secondary oxidation acid leaching according to claim 1, characterized in that: Step 1) includes the following steps: 1a) Take a certain mass of smelting acid mud, add sulfuric acid and hydrogen peroxide, the mass ratio of sulfuric acid to hydrogen peroxide is 1:2-2:1, and mix and react evenly at 60℃-100℃; 1b) After reacting for 4-8 hours, solid-liquid separation is performed to obtain selenium leaching solution and selenium leaching residue respectively; 1c) introducing sulfur dioxide gas into the selenium leaching solution, wherein the molar ratio of sulfur dioxide to selenium in the selenium leaching solution is 1:1-2:1, reacting at room temperature for 1-2 hours to obtain elemental selenium precipitate and sulfuric acid solution; then separating the solid and the liquid, and collecting the crude selenium product of elemental selenium and sulfuric acid tail liquid.
5. The method for recovering selenium and mercury from smelting acid mud by two-stage oxidation acid leaching according to claim 4, characterized in that: The sulfuric acid tail liquid obtained in step 1c) is recycled to step 1a) as a source of sulfuric acid.
6. The method for recovering selenium and mercury from smelting acid mud by secondary oxidation acid leaching according to claim 1, characterized in that: Step 2) includes the following steps: 2a) adding 2-6 mol / L hydrochloric acid to the selenium leaching residue obtained in step 1), with a mass ratio of hydrochloric acid to mercury in the selenium leaching residue of 4:1-8:1 and a liquid-solid ratio of 4:1-10:1, and uniformly mixing and reacting at 60° C.-90° C.; 2b) After reacting for 4-8 hours, solid-liquid separation is performed to obtain mercury leaching solution and mercury leaching residue respectively; 2c) introducing hydrogen sulfide gas into the mercury leachate, wherein the molar ratio of S in the hydrogen sulfide gas to mercury in the mercury leachate is 1:1-2:1, reacting at room temperature for 1-4 hours to obtain mercuric sulfide precipitate and hydrochloric acid; then separating the solid and liquid, and collecting the mercuric sulfide product and hydrochloric acid tail liquid.
7. The method for recovering selenium and mercury from smelting acid mud by two-stage oxidation acid leaching according to claim 6, characterized in that: The hydrochloric acid tail liquid obtained in step 2c) is recycled to step 2a) as a source of hydrochloric acid.
8. The method for recovering selenium and mercury from smelting acid mud by two-stage oxidation acid leaching according to claim 4 or 5, characterized in that: The mass ratio of selenium in the crude selenium product obtained in step 1c) to selenium in the smelting acid mud reaches more than 95%; the purity of selenium in the crude selenium product reaches more than 97%.
9. The method for recovering selenium and mercury from smelting acid mud by two-stage oxidation acid leaching according to claim 6 or 7, characterized in that: The mass ratio of mercury in the mercuric sulfide product obtained in step 2c) to mercury in the smelting acid mud reaches more than 95%; the purity of mercury sulfide in the mercury sulfide product reaches more than 97%.
10. The method for recovering selenium and mercury from smelting acid mud by two-stage oxidation acid leaching according to claim 6 or 7, characterized in that: The mercury leaching slag includes lead sulfate and silver sulfate.