Modified cellulose nanofiber composite material, epoxy resin film and epoxy high build paint

By treating phosphorylated cellulose nanofibers PEG/P-CNF with polyethylene glycol PEG-coated liquid ammonia, the problem of decreased anti-corrosion performance of epoxy resin coatings under long-term exposure has been solved, and high-quality epoxy resin composite materials have been achieved. The mechanical properties, UV resistance and anti-sag properties ensure the stable dispersion and cross-linked network of nanofibers.

CN117866237BActive Publication Date: 2024-10-11BAOHONG COATINGS (GUANGDONG) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410017782.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-04
Publication Date
2024-10-11
Estimated Expiration
2044-01-04

AI Technical Summary

Technical Problem

Existing epoxy resin coatings are easily damaged under long-term exposure and are affected by factors such as ultraviolet rays, humidity and heat, salt spray, etc., resulting in a decrease in anti-corrosion performance, and it is difficult to achieve stable dispersion of nanopowders in composite materials.

Method used

Polyethylene glycol PEG-coated liquid ammonia is used to treat phosphorylated cellulose nanofibers PEG/P-CNF. Nanofibers with surface ammonium phosphate groups are formed through phosphoric acid hydrolysis and liquid ammonia treatment, combined with the hydrogen bonding of PEG to improve The dispersion and cross-linked network of nanofibers enhance the mechanical and thermal properties of composite materials.

Benefits of technology

It improves the UV stability and anti-corrosion properties of epoxy resin, ensures the uniform dispersion of nanofibers in composite materials, and significantly improves the mechanical properties and anti-UV and anti-sag capabilities of composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117866237B_ABST
    Figure CN117866237B_ABST
Patent Text Reader

Abstract

The invention discloses a polyethylene glycol (PEG)-coated liquid ammonia-treated phosphorylated cellulose nanofiber PEG / P-CNF and a preparation method thereof, an epoxy resin composite film and a preparation method thereof, and an anti-ultraviolet, anti-sagging and wear-resistant epoxy mastic paint and a preparation method thereof.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of coatings, and in particular to a polyethylene glycol (PEG)-coated liquid ammonia-treated phosphorylated cellulose nanofiber PEG / P-CNF and a preparation method thereof, an epoxy resin composite film and a preparation method thereof, and an anti-ultraviolet, anti-sagging, and wear-resistant epoxy thick paste paint and a preparation method thereof. Background Art

[0002] The epoxy resin molecular structure contains multiple epoxy groups, which can undergo cross-linking reactions with a variety of curing agents to form an insoluble, infusible three-dimensional network polymer structure. Epoxy resin cured products have excellent physical properties, bonding properties, mechanical properties and chemical stability, and are widely used in adhesives, anti-corrosion coatings, repair materials and other fields. Because of its good adhesion on surfaces such as concrete, metal, and plastic, it has become a commonly used protective and repair material in the coating field. However, simple epoxy resin coatings only show good anti-corrosion ability in the early stage. As time goes by, due to the influence of the cross-linking density of epoxy resin, the micropores and defects in the epoxy coating structure cause the epoxy coating to be exposed to ultraviolet radiation, heat and humidity, salt spray, moisture, and some pollutants for a long time, causing a series of physical and chemical changes, and the coating structure is damaged. Therefore, the research and preparation of epoxy resin anti-corrosion materials with better performance has become a hot topic at present. A large number of research reports show that in recent years, more and more scholars have begun to pay attention to the research of new epoxy resin materials, functional anti-corrosion coatings and epoxy resin composites. From the perspective of epoxy resin, there are three basic ideas to improve its anti-corrosion performance: (1) increase the tortuosity of the diffusion path of the corrosive medium and reduce the porosity of the epoxy resin coating; (2) reduce the affinity between the corrosive medium and the epoxy resin coating; (3) inhibit the reaction between the corrosive medium and the metal substrate. In recent years, a large number of literatures have reported that water-based coatings with nanocomposite materials as fillers have good anti-corrosion effects, which has attracted more and more attention from the academic community.

[0003] Cellulose nanofibers (CNF) have a large aspect ratio and a large specific surface area due to their nanostructure characteristics (diameter 1-100nm, length up to several microns). They can easily form a variety of structures through mutual entanglement, hydrogen bonding, etc., and can be constructed through structural design. This is unmatched by ordinary cellulose. At the same time, a large number of hydroxyl groups are retained on the surface of nanocellulose, which can be easily modified with low surface energy substances. Therefore, it can be used in the fields of medicine, coatings, papermaking, etc.

[0004] Therefore, the inventor attempts to embed nano fillers in epoxy resin film, which can make the coating obtain expected corrosion resistance, oxidation resistance and good mechanical properties. However, nano powders can spontaneously form aggregates under the influence of surface energy due to large specific surface area. The key problem of applying nano powders to composite materials as protection is to make them have stable dispersion characteristics. These problems can be solved by physically or chemically modifying the nano material surface, making its surface functionalized or covering active substances. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a polyethylene glycol (PEG)-coated liquid ammonia-treated phosphorylated cellulose nanofiber PEG / P-CNF, and a preparation method thereof comprises the following steps:

[0006] S1: hydrolyzing wood pulp fiber SP with phosphoric acid, cooling, filtering, obtaining phosphorylated cellulose nanofiber P-CNF precipitate, then treating the P-CNF precipitate with liquid ammonia, centrifuging, washing the precipitate, high pressure homogenizing, freeze drying, obtaining liquid ammonia treated P-CNF powder;

[0007] S2: Disperse the liquid ammonia treated P-CNF powder in NaOH and urea aqueous solutions, filter to obtain a saturated liquid ammonia treated P-CNF solution, add polyethylene glycol PEG aqueous solution to the saturated liquid ammonia treated P-CNF solution, stir, then add poor solvent ethanol, co-precipitate the liquid ammonia treated P-CNF and polyethylene glycol PEG to obtain a co-precipitate, wash the precipitate, disperse it with water, then add molten PEG to coat the precipitate, centrifuge, high pressure homogenize, and freeze-dry to obtain liquid ammonia treated phosphorylated cellulose nanofiber PEG / P-CNF coated with polyethylene glycol PEG.

[0008] Furthermore, in step S1: phosphoric acid is a 10M phosphoric acid solution, the mass ratio of phosphoric acid solution to cellulose SP is (10-15):1, and the hydrolysis temperature is 110°-140°. These hydrolysis conditions are selected because the conditions for the hydrolysis of CNF with phosphoric acid reported previously are not harsh enough to completely cleave the amorphous regions of CNF, thereby generating personalized CNF with an optimal surface phosphate group density.

[0009] The wood pulp fiber SP is prepared by beating 2% concentrated slurry of coniferous wood pulp with water to a beating degree of 85°SR, and drying to obtain the wood pulp fiber SP.

[0010] The liquid ammonia treatment of P-CNF precipitation was terminated when the pH value reached 7.0.

[0011] The cleaning precipitate is prepared by treating the P-CNF precipitate with liquid ammonia, dispersing it in ethanol after centrifugation, and then ultrasonically cleaning it.

[0012] The P-CNF in the present invention is obtained by hydrolyzing wood pulp fiber SP with phosphoric acid. The optimal hydrolysis condition is to graft more phosphoric acid groups on the surface hydroxyl sites. During the liquid ammonia treatment process, the surface phosphoric acid groups are attacked by nucleophilic ammonia, resulting in P-CNF with surface ammonium phosphate groups. These groups absorb ultraviolet photons and convert them into low heat energy or short-wave electromagnetic waves, thereby improving the ultraviolet stability of epoxy resin.

[0013] Furthermore, in step S2: the NaOH aqueous solution is a 14wt.% NaOH aqueous solution, the urea solution is a 24wt.% pre-cooled urea solution, the liquid ammonia treated P-CNF powder is dispersed in the NaOH aqueous solution and then pre-cooled, and then the urea solution is added and filtered to obtain a saturated liquid ammonia treated P-CNF solution; the reason why 14wt.% NaOH aqueous solution and 24wt.% pre-cooled urea solution are used to dissolve the liquid ammonia treated P-CNF powder. The inventors found in previous studies that due to the strong hydrogen bonding effect, cellulose is difficult to be dissolved by conventional solvents, and the NaOH / urea aqueous solution promotes the production of alkali hydrates and urea hydrates, which can destroy the original hydrogen bond network of cellulose to obtain a uniform cellulose solution.

[0014] The PEG solution is a 10wt.% PEG aqueous solution; the saturated liquid ammonia treated P-CNF solution and the PEG solution are mixed in a mass ratio of 1:4; the mass ratio of molten PEG to liquid ammonia treated P-CNF powder is (2-14):(18-20).

[0015] Both PEG and cellulose surfaces are rich in hydroxyl groups, which theoretically have good affinity. These hydroxyl groups have strong affinity within each component itself and form strong hydrogen bonding, which makes it difficult to prepare uniformly dispersed PEG composites. Therefore, it is best to prepare them into a homogeneous solution system before blending to achieve uniform mixing between them. The poor solvent ethanol is selected as a precipitant, and a large amount of ethanol is added to flocculate the two components at the same time, thereby obtaining strong interactions between molecular chain entanglement and hydrogen bonds. In addition, P-CNF can also act as a heterogeneous nucleating agent to improve the crystallinity of the composite system. These physical cross-linked networks and increased crystallinity improve the dynamic mechanical properties and thermal properties of the material, and the large number of hydroxyl groups on the surface of P-CNF can act as ester exchange sites in the epoxy-anhydride system and interact with the hydroxyl groups therein, which is expected to make the composite material have excellent comprehensive properties.

[0016] The present invention also provides a modified cellulose nanofiber, which is prepared by the preparation method of the above-mentioned polyethylene glycol (PEG)-coated liquid ammonia-treated phosphorylated cellulose nanofiber PEG / P-CNF.

[0017] The present invention also provides a modified epoxy resin composite film, which is obtained by an ester exchange reaction of epoxy resin, the modified cellulose nanofiber composite material, polyethylene glycol PEG, a curing agent and a catalyst.

[0018] Furthermore, the epoxy resin is bisphenol A epoxy resin; the curing agent is succinic anhydride, and the amount of succinic anhydride is anhydride group: epoxy group = 1:2;

[0019] The modified cellulose nanofiber composite material is 10%-40% of the total feed amount by weight, preferably 20%;

[0020] The polyethylene glycol PEG, by weight, is 2%-12% of the total feed amount, preferably 4%. In general, the composite material is prepared by dispersing the PEG-coated liquid ammonia-treated phosphorylated cellulose nanofibers in an epoxy matrix. Adding PEG alone not only fails to significantly improve the toughness of the composite material, but also significantly deteriorates the tensile strength, flexural strength, etc.; however, with the addition of PEG / P-CNF, various parameters of the mechanical properties are significantly increased, and the addition amount is more appropriate between 2% and 6%. The unnotched impact strength of the composite material sample containing 4% PEG / P-CNF reached 23.6k J / m 2 , which is 95% higher than that of the EP-20PEG sample without the addition of PEG / P-CNF.

[0021] The present invention also provides a method for preparing a modified epoxy resin composite film, comprising mixing the above-mentioned epoxy resin, modified cellulose nanofiber composite material, polyethylene glycol PEG, a curing agent and a catalyst at 100-140° C., carrying out an ester exchange reaction, pouring the mixture into a mold, vacuum drying, curing, and cooling to room temperature to obtain a modified epoxy resin composite film.

[0022] The present invention also provides an anti-ultraviolet, anti-sagging, and wear-resistant epoxy mastic paint, comprising component A and component B, wherein:

[0023] Group A is composed of:

[0024]

[0025]

[0026] Group B is

[0027] Epoxy Curing Agent 160~180

[0028] Furthermore, the epoxy resin is: American Cytec 384; the epoxy curing agent is: American OlinDEH806; the anti-sagging agent is: BYK440.

[0029] The present invention also provides a method for preparing an anti-ultraviolet, anti-sagging and wear-resistant epoxy mastic paint, the steps of which are: according to the above formula,

[0030] Preparation of material A: firstly, the modified cellulose nanofiber composite material, wherein the mass ratio of molten PEG to liquid ammonia treated P-CNF powder is (2-14): (18-20), epoxy resin, deionized water and defoamer are mixed evenly, and then anti-rust additives: zinc phosphate, aluminum tripolyphosphate, pigments and fillers: titanium dioxide, yellow iron oxide, talcum powder and barium sulfate are added in sequence, and stirred at high speed, and finally, defoamer, anti-sagging additive and leveling agent are added and stirred;

[0031] The prepared epoxy thick paste material A and the epoxy curing agent in material B are mixed and stirred evenly according to the proportion, and deionized water is added to adjust the viscosity.

[0032] The present invention has the following advantages over the prior art:

[0033] (1) The present invention hydrolyzes wood pulp fiber SP with phosphoric acid and grafts more phosphoric acid groups on the fiber hydroxyl sites. During the liquid ammonia treatment process, the surface phosphoric acid groups are attacked by nucleophilic ammonia, producing P-CNF with surface ammonium phosphate groups. These groups absorb ultraviolet photons and convert them into low heat energy or short-wave electromagnetic waves, thereby improving the ultraviolet stability of epoxy resin.

[0034] (2) The present invention introduces PEG into P-CNF. On the one hand, the presence of PEG is expected to effectively prevent the agglomeration of P-CNF during the flocculation process, thereby obtaining P-CNF with smaller and more uniform particle size. On the other hand, coating P-CNF with PEG before curing the epoxy resin can not only ensure the dispersion of P-CNF in the epoxy matrix, but also introduce soft elastic segments into the composite material to achieve performance optimization of the brittle epoxy resin.

[0035] (3) The large number of hydroxyl groups on the surface of P-CNF can act as ester exchange sites in the epoxy-anhydride system and interact with the hydroxyl groups in the matrix, which is expected to enable the epoxy resin composite material to have excellent comprehensive properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 1 is the Fourier transform infrared spectrum of CNF and P-CNF of Example 1 of the present invention.

[0037] Figure 2 This is the microscopic morphology of the epoxy high build paint of Example 4 with excellent resistance to ultraviolet radiation, salt spray, sag resistance and mechanical properties before and after ultraviolet aging. 2(a) is ultraviolet aging for 250 hours, and 2(b) is ultraviolet aging for 800 hours.

[0038] Figure 3The morphology analysis diagram of the epoxy thick paste paint and pure epoxy resin with excellent ultraviolet radiation resistance, salt spray resistance, sag resistance and mechanical properties before and after ultraviolet aging in Example 4, 3 (a) is the liquid ammonia treated phosphorylated cellulose nanofiber PEG / P-CNF coated with polyethylene glycol PEG prepared in Example 2 with 40 parts added, and 3 (b) is pure epoxy resin. DETAILED DESCRIPTION

[0039] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.

[0040] Materials: Bleached kraft softwood pulp, Celgar Pulp Company, Canada. Bisphenol A epoxy resin (DER332) was purchased from Dow Chemical Company. According to the data provided by the epoxy resin manufacturer, the epoxy value of the epoxy resin is 0.51 mol / 100 g, i.e., 5.1×10 -3 mol / g. Polyethylene glycol 6000 (PEG): average molecular weight 5500-7000, crystallization point 54-57℃, purchased from Tianjin Damao Chemical Reagent Factory; Succinic anhydride: analytical grade, purchased from Shanghai MacLean Biochemical Co., Ltd.; Zinc acetylacetonate hydrate Zn(acac) 2 and zinc acetate were purchased from Shanghai MacLean Biochemical Co., Ltd.

[0041] No.2505 Vally beater, KRK Co., Ltd., Japan; AHPI-LOT2015 high pressure homogenizer, Antos Nanotechnology Co., Ltd., Canada; phosphoric acid (H3PO4, mass fraction 99.5%), sodium hydroxide (NaOH, mass fraction ≥ 96%) and urea, all of which were analytical grade, were purchased from Tianjin Jiangtian Chemical Co., Ltd.

[0042] Embodiment 1:

[0043] Phosphorylated cellulose nanofibers (P-CNF) treated with liquid ammonia:

[0044] The bleached kraft softwood pulp was evenly dispersed in water at 2% concentration, Vally beaten to a beating degree of 85°SR, and dried in an oven at 105°C to obtain wood pulp fiber SP. In a 100mL nitrogen-protected four-necked flask, 2g of the above-mentioned dried fiber was taken into the flask, and 20g of 10M phosphoric acid solution was added, the mass ratio of phosphoric acid solution to cellulose was 10:1, and heated to 140°C and stirred. These hydrolysis conditions were selected because the conditions for phosphoric acid hydrolysis of CNF reported previously were not harsh enough to completely cleave the amorphous region of CNF, thereby generating personalized CNF with the best surface phosphate group density. After 4h of reaction, the mixture was cooled and filtered, and the precipitate was washed with isopropanol and 0.1mol / L hydrochloric acid. The precipitate was placed in liquid ammonia, and the phosphorylated cellulose nanofibers (P-CNF) were treated with liquid ammonia to a pH value of 7.0. The resulting suspension was stirred at room temperature and centrifuged at 4000rpm for 20 minutes. The collected P-CNC was suspended in anhydrous ethanol and ultrasonically cleaned in an ultrasonic cleaner at 37kHz for 10 minutes to obtain liquid ammonia-treated phosphorylated cellulose nanofibers (P-CNFs), which were then subjected to high-pressure homogenization and freeze-dried to obtain phosphorylated-modified cellulose nanofibrils (P-CNFs).

[0045] like Figure 1 As shown in Figure 2, the functional groups of CNF and P-CNF were investigated using Fourier transform infrared spectroscopy to demonstrate the successful introduction of new functional groups during phosphoric acid hydrolysis and liquid ammonia treatment. -1 The spectral range is 4.0 cm -1 The total number of scans was 32. Among them, some peaks included those at 3600 and 3000 cm -1 The intensity of this peak broadens after phosphorylation and liquid ammonia treatment, which may indicate the overlap of -OH and NH groups in P-CNF. -1 , attributed to the CH groups in cellulose, this peak also becomes broader in P-CNF, indicating that NH + Overlapping with CH peak. Cellulose peaks at 1160 and 1128 cm -1 The other characteristic peaks are attributed to the asymmetric COC stretching of the β-1→4)-glycosidic bonds in the cellulose chain. In the P-CNF spectrum, 1235 cm -1 The small peak at 665 cm -1 The new peak at 614 cm corresponds to the NH stretching vibration, which indicates that the ammonium phosphate group was successfully introduced during the liquid ammonia treatment. -1 The peak at represents the PO 3- Bending vibration of OPO in the group.

[0046] Embodiment 2:

[0047] Preparation of PEG / P-CNF coated with liquid ammonia treated phosphorylated cellulose nanofibers:

[0048] This embodiment uses a solution blending method to prepare polyethylene glycol PEG coated liquid ammonia treated phosphorylated cellulose nanofibers PEG / P-CNF. First, a certain amount of liquid ammonia treated P-CNF is dispersed in a 14wt.% NaOH aqueous solution and precooled for a period of time, and then a precooled 24wt.% urea solution is added to the solution and stirred rapidly to obtain a liquid ammonia treated P-CNF solution, and further centrifuged to remove bubbles and insolubles to obtain a saturated liquid ammonia treated P-CNF solution. At room temperature, a 10wt.% PEG solution is prepared using deionized water as a solvent. The saturated liquid ammonia treated P-CNF solution is mixed evenly with the 10wt.% PEG solution in a mass ratio of 1:4 and stirred for 30min to obtain a uniform mixed solution. Then, a large amount of ethanol is added to precipitate it. Ethanol is a poor solvent for the two substances and can trigger the coprecipitation process. When excess ethanol is added, the liquid ammonia treated P-CNF entrained with PEG precipitates out of the system. The presence of PEG can effectively prevent the aggregation caused by the interaction of hydroxyl groups between the molecular chains of liquid ammonia-treated P-CNF during the precipitation process. However, without PEG, when the hydrates (NaOH and urea hydrates) that shield the hydrogen bonds between the cellulose molecular chains in the solution are destroyed, the hydrogen bonds between the cellulose will be reformed and large particles will be generated, which further leads to the difficulty of dispersing the liquid ammonia-treated P-CNF in the epoxy matrix. The obtained P-CNF / PEG coprecipitate was washed with deionized water and assisted by ultrasonic cleaning and stirring, so that part of the precipitated PEG was redissolved and removed. The obtained P-CNF / PEG coprecipitate was dispersed in water to obtain a suspension. The required PEG was heated to 70°C to melt it, and then added to the above-mentioned P-CNF / PEG coprecipitate suspension, so that the molten PEG was wrapped on the surface of the liquid ammonia-treated P-CNF / PEG coprecipitate. The obtained suspension was stirred at room temperature and centrifuged at 4000 rpm for 20 minutes to obtain liquid ammonia treated phosphorylated cellulose nanofibers PEG / P-CNF coated with polyethylene glycol PEG, which were then subjected to high pressure homogenization and freeze-dried to obtain liquid ammonia treated phosphorylated cellulose nanofibers PEG / P-CNF particles coated with polyethylene glycol PEG. The polyethylene glycol PEG coating is to prevent the agglomeration of liquid ammonia treated P-CNF / PEG during the drying process, thereby further improving the dispersion of liquid ammonia treated P-CNF / PEG in the epoxy matrix. At the same time, a certain amount of PEG is used to coat P-CNF / PEG, and PEG can be used as a template to well fix the refined P-CNF, which is conducive to the uniform dispersion of phosphorylated cellulose nanofibers when mixing with epoxy monomers at high temperature to prepare liquid ammonia treated phosphorylated cellulose nanofibers (P-CNF) / epoxy resin composites (EP / PEG / P-CNF).

[0049] Embodiment 3:

[0050] Preparation of liquid ammonia treated phosphorylated cellulose nanofiber (P-CNF) / epoxy resin composites:

[0051] This example uses an in-situ polymerization method to prepare a liquid ammonia treated phosphorylated cellulose nanofiber (P-CNF) / epoxy resin composite material EP / PEG / P-CNF. According to the mass formula in Table 1, the specific preparation method is as follows: the curing agent is succinic anhydride, the resin is bisphenol A type epoxy resin, polyethylene glycol PEG, and the catalyst is acetylacetonate zinc hydrate Zn(acac) 2 and zinc acetate, the liquid ammonia treated phosphorylated cellulose nanofibers PEG / P-CNF coated with polyethylene glycol PEG prepared in Example 2. The amount of materials added is: the amount of succinic anhydride is based on the molar ratio of anhydride group: epoxy group = 1:2, Zn(acac) 2 The dosage is 10 mol% of succinic anhydride, the dosage of zinc acetate is 15 mol% of anhydride, and the dosage of PEG is added according to the formula in Table 1. The liquid ammonia treated phosphorylated cellulose nanofibers PEG / P-CNF coated with polyethylene glycol PEG are added according to the formula in Table 1. According to the formula in Table 1: All ingredients are stirred and mixed evenly at 120°C. Then immediately pour it into the mold, put it in a vacuum drying oven, defoam at 100°C for 1h, and finally cure it at 120°C for 6h, and the sample is naturally cooled to room temperature. The sample without P-CNF is named EP-xPEG, where x represents the mass percentage of PEG (0%, 10%, 20%, 30% and 40%). In addition, the PEG / P-CNF prepared in Example 2 was added to the EP-20PEG system, and the resulting sample was called PEG / yP-CNF, where y represents the content of PEG / P-CNF in the composite material as y weight percentage (2%, 4%, 6%, 8% and 12%). The pure sample without PEG and PEG / P-CNF was called EP. The preparation process of Table 1 is the same.

[0052] Table 1 Formulation of epoxy composite materials

[0053] sample PEG Succinic anhydride E51 Zn(acac)2 Zinc acetate P-CNF EP 0 20.48 79.76 5.36 5.60 _ EP-10PEG 10 18.57 72.32 4.86 5.08 _ EP-20PEG 20 16.62 64.72 4.35 4.54 _ EP-30PEG 30 14.71 57.29 3.85 4.02 _ EP-40PEG 40 12.80 49.85 3.35 3.50 _ PEG / 2P-CNF 20 16.62 64.72 4.35 4.54 2.18 PEG / 4P-CNF 20 16.62 64.72 4.35 4.54 4.45 PEG / 6P-CNF 20 16.62 64.72 4.35 4.54 6.82 PEG / 8P-CNF 20 16.62 64.72 4.35 4.54 9.29 PEG / 12P-CNF 20 16.62 64.72 4.35 4.54 14.57

[0054] Testing of mechanical properties of epoxy resin composite materials;

[0055] The cured epoxy resin samples were subjected to tensile and bending tests at room temperature on a universal electronic testing machine (Zwick / Roell Z010, Zwick / Roell, Germany). The tensile speed was 5 mm / min and the lowering speed of the bending indenter was 5 mm / min. The impact test was performed on an Izod impact tester using a 2.75 J pendulum.

[0056] Table 2 Mechanical statistics of epoxy composites

[0057]

[0058] The addition of PEG to the epoxy system synthesized from epoxy resin and succinic anhydride can solve the brittleness problem of epoxy composites. First, the effect of PEG content on mechanical properties was simply evaluated. As shown in Table 2, with the increase of PEG content, the tensile strength, flexural strength, flexural modulus and unnotched impact strength of the epoxy composite material decreased significantly, and the notched impact strength increased slightly. This result shows that the addition of PEG alone does not improve toughness well, but also significantly reduces other mechanical properties. Therefore, the polyethylene glycol PEG-coated liquid ammonia-treated phosphorylated cellulose nanofiber PEG / P-CNF of Example 2 was introduced into the epoxy polymer system containing 20% ​​PEG, wherein the mass ratio of molten PEG to liquid ammonia-treated P-CNF powder was 1:10 for further study. As shown in Table 2, after adding the polyethylene glycol PEG-coated liquid ammonia-treated phosphorylated cellulose nanofiber PEG / P-CNF, various mechanical performance parameters were significantly improved; Table 2 lists the corresponding data and the data of the comparative samples. When the PEG / P-CNF content increases, the tensile strength, flexural strength, flexural modulus and unnotched impact strength of the composite material first increase and then decrease, and the notched impact strength increases slightly with little change. When the PEG / P-CNF content is 4wt.%, the tensile strength, flexural strength and flexural modulus of the composite material reach 56.9 MPa, 80.6 MPa and 2410 MPa, respectively. Compared with the EP-20PEG sample (without PEG / P-CNF), it is equivalent to an increase of 94%, 112% and 49%. At the same time, the unnotched impact strength of 4P-CNF also reached 23.6kJ / m2, which is significantly higher than 16.3kJ / m2 of EP. 2 and EP-20PEG's 12.1 kJ / m 2 , increased by 45% and 95% respectively. However, excessive addition of PEG / P-CNF will lead to a decrease in mechanical properties. The reason may be that too many hydroxyl groups on the cellulose surface affect the cross-linking density of the system. In general, the composite material was prepared by dispersing phosphorylated cellulose nanofibers treated with liquid ammonia coated with PEG in an epoxy matrix. The addition of PEG alone not only fails to significantly improve the toughness of the composite material, but also significantly deteriorates the tensile strength, flexural strength, etc.; however, with the addition of PEG / P-CNF, all parameters of the mechanical properties increased significantly, and the addition amount between 2% and 6% is more appropriate. The unnotched impact strength of the composite material sample containing 4% PEG / P-CNF reached 23.6k J / m 2 , which is 95% higher than that of the EP-20PEG sample without PEG / P-CNF added.

[0059] Embodiment 4:

[0060] Preparation of epoxy high build paint with excellent UV radiation resistance, salt spray resistance, sagging resistance and mechanical properties:

[0061] (1) Selection and screening of raw materials: ① Epoxy resin: American Cytec 384; ② Antirust additives: zinc phosphate, aluminum tripolyphosphate; ③ Pigments and fillers: titanium dioxide, yellow iron oxide, barium sulfate, talcum powder; ④ Epoxy curing agent: American OlinDEH806; ⑤ Anti-sagging additives: BYK420, BYK440, German Mingling PUR-64; ⑤ Liquid ammonia-treated phosphorylated cellulose nanofiber PEG / P-CNF coated with polyethylene glycol PEG prepared in Example 2, wherein the mass ratio of molten PEG to liquid ammonia-treated P-CNF powder is 1:10. An epoxy high build paint with excellent ultraviolet radiation resistance, salt spray resistance, anti-sagging and mechanical properties was prepared by screening the above materials.

[0062] (2) Components of epoxy high build paint:

[0063] Component A

[0064]

[0065]

[0066] Component B

[0067] Epoxy Curing Agent 160~180

[0068] (3) Preparation method of epoxy thick paste paint: Preparation of epoxy thick paste paint A: First, epoxy resin, polyethylene glycol PEG prepared in Example 2, liquid ammonia-treated phosphorylated cellulose nanofiber PEG / P-CNF, deionized water and defoaming agent are stirred at a speed of 500 r / min for 10 min. After stirring evenly, anti-rust additives: zinc phosphate, aluminum tripolyphosphate, color fillers: titanium dioxide, yellow iron oxide, talcum powder and barium sulfate are added in sequence, and the speed is increased to 1500 r / min and stirred for 1 hour. Finally, defoaming agent, anti-sagging agent and leveling agent are added, and stirred at 500 r / min for 10 min.

[0069] Preparation of epoxy high build paint: Mix the prepared epoxy high build paint material A and the epoxy curing agent in material B according to the ratio and stir evenly, then add deionized water according to the total weight of material A and material B to adjust the viscosity according to the actual needs of the project. Use a brush to evenly apply the prepared epoxy high build paint on the substrates such as tinplate and steel plate that have been sanded and wiped with alcohol, and place it in a constant temperature box at 25℃±3℃ for 24 hours to form a water-based epoxy primer coating, and then maintain it for the specified time before performing the next performance test.

[0070] (4) The photostability of pure epoxy (i.e., the liquid ammonia-treated phosphorylated cellulose nanofibers PEG / P-CNF coated with polyethylene glycol PEG prepared in Example 2 without addition) and the liquid ammonia-treated phosphorylated cellulose nanofibers PEG / P-CNF coated with polyethylene glycol PEG prepared in Example 2 with addition of 40 parts of the liquid ammonia-treated phosphorylated cellulose nanofibers PEG / P-CNF with addition of 40 parts of the polyethylene glycol PEG prepared in Example 2) was studied in the anti-aging mechanism. The laboratory artificial accelerated ultraviolet aging method was adopted in accordance with the standard GB / T 14522-2008, and the ZN-P type ultraviolet weathering test box of Wuxi Sunan Testing Equipment Co., Ltd. was used, and the ultraviolet irradiance (λ=340 nm) was 0.68 W / m 2 , in a Q-SUN xenon lamp test chamber (Xe-3) at a temperature of 50°C, exposed to UV light for 250 hours, 500 hours, and up to 800 hours without water spraying. A JSM-IT300 scanning electron microscope was used to observe the morphology of the samples before and after UV aging and the tensile-tensile fatigue fracture morphology of the samples, with a magnification of 500 times. The tensile-tensile fatigue test instrument is Instron 1341 electro-hydraulic servo universal material testing machine of Instron Company, and the test standard adopted is GB / T16779-2008. The experiment adopts stress control and selects four stress levels: 80%, 70%, 60%, 50%, the frequency is 10Hz, and the stress ratio R=0.1.

[0071] like Figure 2 As shown, it is a microscopic morphology of the phosphorylated cellulose nanofiber PEG / P-CNF treated with liquid ammonia after adding 40 parts of polyethylene glycol PEG prepared in Example 2, wherein Figure 2 (a) and Figure 2 (b) The tensile fracture morphology of the samples after UV aging for 250h and 800h, respectively. Figure 2 It can be seen from (a) that the surface of the composite material aged for 250 h is smooth, the texture is relatively solid, and the arrangement is relatively orderly. Figure 2 (b) After 800 h of UV aging, no cracks or defects were produced on the surface of the composite material, indicating that UV aging has little effect on the composite material; however, in the control example, the pure epoxy resin, American Cytec 384 matrix, showed relatively serious damage, part of the epoxy resin fell off, and a relatively large number of fragments and holes were produced.

[0072] Morphological analysis: Figure 3 As shown in the figure, the color of the phosphorylated cellulose nanofiber PEG / P-CNF and the pure epoxy resin sample treated with liquid ammonia treated with 40 parts of polyethylene glycol PEG prepared in Example 2 changes with the increase of UV aging time. Figure 3 It can be seen from (a) that as the aging time increases, the color of the composite material gradually deepens, and the distribution of the darkened color area gradually expands to the entire composite material surface as the aging time increases; Figure 3(b) With the increase of aging time, the color change of pure epoxy resin is more obvious, and the color of the whole sample is completely darkened. This is mainly because the surface resin of the UV irradiated surface undergoes a photo-oxidative aging reaction. The ultraviolet rays break the epoxy resin chain segments to generate active free radicals, which react with oxygen in the air to generate new chromophores, causing the color of the sample to change. The 40 parts of PEG / P-CNF in the reinforcing phase of the composite material has good chemical stability and can delay the further penetration of UV oxidative damage.

[0073] (5) Comparison of the effect of rheological additives on sagging. It can be seen from the table that when the anti-sagging additives are BYK420 and BYK440, the coating does not sag when the wet film thickness is 700um or 800um, and the anti-sagging performance is good. Therefore, the coating can use BYK420 or BYK440 as the anti-sagging additive.

[0074] Table 3 Comparison of the effects of rheological additives on sagging

[0075]

[0076] Effect of different rheological additives on coating properties. As can be seen from Table 4, when the anti-sagging additives are BYK420 and BYK440, the adhesion, flexibility, impact strength and salt spray test effects are better.

[0077] Table 4 Effect of different rheological additives on coating properties

[0078]

[0079]

[0080] Effect of rheological additive amount on performance. From the above experiments, BYK440 is a better anti-sagging additive. Therefore, BYK440 is used as an anti-sagging additive to test its butanone scrubbing, salt spray test and salt water resistance test with different addition amounts. The experiment confirms that the best addition amount of anti-sagging additive BYK440 is 5-10%.

[0081] Table 5 Effect of rheological additive addition on performance

[0082]

[0083] The above is a preferred embodiment of the present invention, but the embodiment of the present invention is not limited to the above content. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing liquid ammonia-treated phosphorylated cellulose nanofibers PEG / P-CNF coated with polyethylene glycol (PEG), Features: The steps include: S1: hydrolyze wood pulp fiber SP with phosphoric acid, cool, filter, and obtain phosphorylated cellulose nanofiber P-CNF precipitate, then treat the phosphorylated cellulose nanofiber P-CNF precipitate with liquid ammonia until the pH reaches 7.0, centrifuge, wash the precipitate, high pressure homogenize, and freeze-dry to obtain liquid ammonia treated phosphorylated cellulose nanofiber P-CNF powder; The wood pulp fiber SP is a 2% concentrated slurry of coniferous wood pulp mixed with water, beaten to a beating degree of 85° SR, and dried to obtain the wood pulp fiber SP; The phosphoric acid is a 10M phosphoric acid solution, the mass ratio of the phosphoric acid solution to the cellulose SP is 10-15:1, the hydrolysis temperature is 110-140° C., and the hydrolysis time is 4 hours; S2: Disperse liquid ammonia treated phosphorylated cellulose nanofiber P-CNF powder in NaOH and urea aqueous solution, filter to obtain saturated liquid ammonia treated phosphorylated cellulose nanofiber P-CNF solution, add polyethylene glycol PEG aqueous solution to the saturated liquid ammonia treated phosphorylated cellulose nanofiber P-CNF solution, stir, then add poor solvent ethanol, co-precipitate liquid ammonia treated phosphorylated cellulose nanofiber P-CNF and polyethylene glycol PEG to obtain co-precipitate, wash the precipitate, disperse it with water, add molten PEG to coat the precipitate, centrifuge, high pressure homogenize, freeze-dry to obtain liquid ammonia treated phosphorylated cellulose nanofiber PEG / P-CNF coated with polyethylene glycol PEG; The NaOH aqueous solution is a 14 wt.% NaOH aqueous solution, and the urea solution is a 24 wt.% pre-cooled urea solution; Liquid ammonia treated phosphorylated cellulose nanofiber P-CNF powder is dispersed in a NaOH aqueous solution and then precooled, and then a urea solution is added and filtered to obtain a saturated liquid ammonia treated phosphorylated cellulose nanofiber P-CNF solution; The PEG aqueous solution is a 10 wt.% PEG aqueous solution; The saturated liquid ammonia treated phosphorylated cellulose nanofiber P-CNF solution and the PEG solution are mixed at a mass ratio of 1:4; The mass ratio of the molten PEG to the liquid ammonia treated phosphorylated cellulose nanofiber P-CNF powder is 2-14:18-20.

2. A modified cellulose nanofiber composite material, Features: The modified cellulose nanofiber composite material is prepared by the preparation method of the polyethylene glycol PEG-coated liquid ammonia-treated phosphorylated cellulose nanofiber PEG / P-CNF according to claim 1.

3. A modified epoxy resin composite film, It is characterized in that The modified epoxy resin composite film is obtained by an ester exchange reaction of epoxy resin, the modified cellulose nanofiber composite material according to claim 2, polyethylene glycol PEG, a curing agent and a catalyst; The epoxy resin is bisphenol A epoxy resin; the curing agent is succinic anhydride, and the amount of succinic anhydride is anhydride group: epoxy group = 1:2; The polyethylene glycol PEG is 10%-40% of the total feed amount by weight; The modified cellulose nanofiber composite material is 2% to 6% of the total feed amount by weight; The catalyst is zinc acetylacetonate hydrate Zn(acac) 2 and zinc acetate, and Zn(acac) 2 The amount of zinc acetate used is 10 mol% of succinic anhydride, and the amount of zinc acetate used is 15 mol% of the anhydride.

4. The modified epoxy resin composite film according to claim 3, It is characterized in that The polyethylene glycol PEG is 20% of the total feed amount by weight; The modified cellulose nanofiber composite material accounts for 4% of the total feed amount by weight.

5. A method for preparing the modified epoxy resin composite film according to claim 3, It is characterized in that The epoxy resin, modified cellulose nanofiber composite material, polyethylene glycol PEG, curing agent and catalyst are mixed at 100-140°C, subjected to ester exchange reaction, poured into a mold, vacuum dried, cured, and cooled to room temperature to obtain a modified epoxy resin composite film. 6.An anti-UV, anti-sagging, wear-resistant epoxy high build paint, Features: It contains component A and component B, wherein: 。 7. The anti-ultraviolet, anti-sagging and wear-resistant epoxy mastic paint according to claim 6, Features: The epoxy resin is: American Cytec 384; The epoxy curing agent is: American OlinDEH806; The anti-sagging agent is BYK440.