Mineral admixture for improving mixing efficiency of ultra-high performance concrete and ultra-high performance concrete using the same
By using mineral admixtures of fly ash, calcium carbonate powder and nanoparticles in ultra-high performance concrete to optimize particle dispersion and filling, the problem of too long mixing time of UHPC is solved, and the mixing efficiency and mechanical properties are improved.
Patent Information
- Application Number
- CN202211438285.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-16
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-11-16
AI Technical Summary
The mixing time of ultra-high performance concrete (UHPC) is too long, resulting in low production efficiency and hindering its large-scale promotion and application.
A mineral admixture is used, including fly ash, calcium carbonate powder and nanoparticles. Through reasonable component ratio and particle size distribution, the particle dispersion and filling effect is optimized, and the slurry discharging time and total mixing time are shortened.
Significantly shortens the mixing time of UHPC, improves preparation efficiency and construction performance, reduces material costs and carbon dioxide emissions, and improves 28d compressive strength.
Smart Images

Figure CN117886529B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of building materials, and in particular, relates to a mineral admixture for improving the mixing efficiency of ultra-high performance concrete, and ultra-high performance concrete using the mineral admixture. Background Art
[0002] Ultra-high performance concrete (UHPC) is a new type of green, environmentally friendly, material-saving and energy-saving building material designed and prepared based on the principles of the most densely packed particles, a water-cement ratio of less than 0.25 and fiber reinforcement, and has the characteristics of ultra-high strength, metal-like tensile strengthening characteristics, and ultra-high durability. Compared with ordinary concrete and high-performance concrete, the UHPC system uses a large amount of ultra-fine powder and utilizes the electrostatic effect and steric hindrance effect of high-efficiency water reducers to achieve the most densely packed particles at extremely low water-cement ratios. However, in order to achieve full dispersion of each component and form a stable flowing slurry, the mixing time of UHPC is significantly longer than that of other cement-based materials.
[0003] At present, the mixing time of UHPC at home and abroad is basically 8min to 20min, and can even reach 30min. Among them, the UHPC mixing time recommended by the European SAMARIS project is about 10min; the UHPC mixing time recommended by Lafarge is 17min; the mixing time recommended in the domestic reactive powder concrete national standard (GB / T 31387-2015) is 16min; and the total mixing time recommended in the ultra-high performance concrete standard (T / CBMF 37-2018) of the China Building Materials Association is also close to 15min. Long-term mixing will not only increase the temperature of the mixture, increase the air content, and cause the longer fibers to agglomerate, but also reduce production efficiency, thereby hindering the large-scale promotion and application of UHPC.
[0004] How to shorten the mixing time has become a key issue for the industrial application of UHPC. Currently, the mixing time of UHPC is basically shortened by designing or improving the mixing device and mixing process, such as patents CN 201910637489, CN 201910637490 and CN201910611979. As for the UHPC material itself, only some studies have found that the mixing time can be shortened by adding coarse aggregate or admixtures; and there are almost no research reports on other improvements such as mineral admixtures to achieve this goal, which is extremely unfavorable for improving the available performance and ease of use of UHPC.
[0005] Therefore, it is urgent to develop mineral admixtures that can shorten the mixing time to improve the preparation efficiency of UHPC. Summary of the invention
[0006] In view of the current problem of long mixing time of ultra-high performance concrete, the present invention proposes a mineral admixture for improving the mixing efficiency of ultra-high performance concrete. Applying it to ultra-high performance concrete can shorten the slurry discharge time and significantly reduce the total mixing time of ultra-high performance concrete.
[0007] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is:
[0008] A mineral admixture for improving the mixing efficiency of ultra-high performance concrete, comprising the following components in the following mass proportions:
[0009] Fly ash 10% to 40%;
[0010] Calcium carbonate powder 39%~85%;
[0011] Nanoparticles 5% to 20%;
[0012] The fly ash is a mixture of 0-70% Class I fly ash and 30%-100% ultrafine fly ash; the fineness of Class I fly ash is such that the residue on a 45μm square sieve does not exceed 10%, while the average particle size of ultrafine fly ash is 1μm-5μm; the percentages of Class I fly ash and ultrafine fly ash are their mass proportions of the total fly ash.
[0013] The density of calcium carbonate powder is not less than 2.6kg / m 3 , with an average particle size of 1μm to 20μm; it is formed by mixing 10% to 50% of small-sized calcium carbonate powder (particle size of 1μm to 5μm) and 50% to 90% of large-sized calcium carbonate powder (particle size of 5μm to 20μm); the percentages of the above-mentioned small-sized calcium carbonate powder and large-sized calcium carbonate powder are their mass proportions of the total amount of calcium carbonate powder.
[0014] Fly ash is spherical in shape and plays a rolling role in the system, which is conducive to the uniform dispersion of particles. Among them, ultrafine fly ash is used to fill small-scale voids and release free water, while the coarser particle size of Class I fly ash can prevent the total surface energy of the powder particles from being too large, weakening the adsorption capacity of water and water reducer and the particle agglomeration effect. However, since ultrafine fly ash is a micron-sized particle, its surface energy is relatively small compared to the extremely high surface energy of nanoparticles, and based on the rolling effect of spherical particles, only ultrafine fly ash can be used; therefore, the mass ratio of Class I fly ash and ultrafine fly ash is controlled to 0-0.7:0.3-1, which can effectively play the above role. However, the proportion of Class I fly ash should not be too high to prevent it from being unable to effectively fill voids and release free water, and the rolling effect of Class I fly ash is weaker than that of ultrafine fly ash, and the effect is also poor.
[0015] The particle characteristics of calcium carbonate powder (higher zeta potential, stronger repulsion between particles) have strong self-dispersion ability, which is conducive to the uniform dispersion of particles in the system. Among them, small-sized calcium carbonate powder with a particle size of 1μm to 5μm is used to fill small-scale voids and release free water, while the coarser particle size of large-sized calcium carbonate powder with a particle size of 5μm to 20μm can prevent the total surface energy of the powder particles from being too large, weakening the adsorption capacity of water and water reducer and the particle agglomeration effect. At the same time, although small-sized calcium carbonate powder is also a micron-sized particle, its surface energy is relatively small compared to nanoparticles, but the irregular particle shape is not conducive to the rapid dispersion of particles, and only small-sized calcium carbonate powder cannot be used; therefore, the mass ratio of large-sized calcium carbonate powder to small-sized calcium carbonate powder is controlled to 0.1-0.5:0.5-0.9, so that the above effects can be effectively exerted. However, the proportion of large-sized calcium carbonate powder should not be too high, because it cannot effectively fill the voids, and the coarser the particles, the more obvious the negative effects of its irregular particle shape.
[0016] At the same time, the use of non-nano calcium carbonate powder with the above-mentioned special size and ratio can also avoid the disadvantages of nano calcium carbonate powder, which has a huge specific surface area and irregular particle shape, resulting in strong adsorption and large friction, which is not conducive to particle dispersion and has a poor effect.
[0017] Nanoparticles are used to fill nanoscale voids and further release free water; however, their dosage should not be too high to prevent excessive surface energy, which would aggravate the adsorption of water and water reducers and particle agglomeration.
[0018] Preferably, the nanoparticles are spherical nanoparticles, and can be selected from any one of silica fume and titanium powder or a mixture of the two. The average particle size of the silica fume is 0.1 μm to 0.9 μm, and the specific surface area is greater than 18000 m 2 / kg; the average particle size of titanium powder is 0.2μm~1.3μm, and the specific surface area is greater than 12000m 2 / kg.
[0019] As a preferred embodiment, the mineral admixture of the present invention may further include at least one of the following components in the following mass proportions:
[0020]
[0021] Specifically, the powder dispersant is a mixture of sodium tripolyphosphate and sodium dodecylbenzene sulfonate in a mass ratio of 1 to 1.2:1; the superplasticizer is a powder polycarboxylic acid water-reducing agent with a water reduction rate of not less than 30%; the hydrophobic agent is a silicone powder hydrophobic agent; and the air-entraining agent is a sodium rosin acid powder air-entraining agent.
[0022] Another object of the present invention is to provide an ultra-high performance concrete having the above-mentioned mineral admixture, by adding an equal volume or mass of the mineral admixture to the concrete cementitious material instead of cement or silica fume, and ensuring that the added amount accounts for 10% to 20% of the total mass of the concrete cementitious material, so as to obtain ultra-high performance concrete.
[0023] Beneficial effects of the present invention:
[0024] 1) The mineral admixture for improving the mixing efficiency of ultra-high performance concrete provided by the present invention uses a large amount of low-quality, low-cost and high-yield solid waste materials, namely fly ash and calcium carbonate powder. When applied to UHPC, it can not only reduce the amount of cement and silica fume, but also further reduce the UHPC material cost and carbon dioxide emissions.
[0025] 2) The mineral admixture for improving the mixing efficiency of ultra-high performance concrete provided by the present invention can shorten the slurry discharge time by 20% to 88% after being applied to UHPC, greatly improving the mixing efficiency of UHPC; it can also reduce the viscosity of the UHPC mixture by more than 20% and increase the 28d compressive strength by 1% to 10%, thereby achieving a comprehensive improvement in the preparation efficiency, construction performance and mechanical properties of ultra-high performance concrete.
[0026] 3) The mineral admixture for improving the mixing efficiency of ultra-high performance concrete provided by the present invention only needs to mix the various component materials evenly, and is simple and easy to prepare and easy to promote and use. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is a diagram for determining the slurry discharge state of ultra-high performance concrete in Application Example 1 of the present invention. DETAILED DESCRIPTION
[0028] The present invention will be further explained below in conjunction with specific embodiments, but those skilled in the art will understand that the following embodiments are merely specific examples and are not intended to limit the present invention in its entirety.
[0029] In the following embodiments and comparative examples, the fineness of "Class I fly ash" is such that the residue on a 45 μm square sieve does not exceed 10%.
[0030] The average particle size of "ultrafine fly ash" is 3μm to 5μm.
[0031] The average particle size of "silica fume" is about 0.20μm, and the specific surface area is 20200m 2 / kg or so.
[0032] The average particle size of "titanium powder" is about 0.35μm, and the specific surface area is 19000m 2 / kg or so.
[0033] The density of "calcium carbonate powder" is 2.72kg / m 3 The average particle sizes are 1 μm to 5 μm (small-sized calcium carbonate powder) and 5 μm to 20 μm (large-sized calcium carbonate powder).
[0034] "Superplasticizer" is a powdered polycarboxylic acid high-performance water-reducing agent produced by Jiangsu Subote Company, with a water reduction rate of not less than 30%.
[0035] "Water repellent" is a modified polysiloxane powder water repellent.
[0036] “Air entraining agent” is sodium rosin acid powder air entraining agent.
[0037] Example 1
[0038] The present embodiment provides a mineral admixture for improving the mixing efficiency of ultra-high performance concrete, which is a mixture of the following substances in percentage by mass:
[0039] Fly ash: 30%;
[0040] Silica fume: 10%;
[0041] Calcium carbonate powder: 60%.
[0042] Among them, fly ash is a mixture of Class I fly ash and ultrafine fly ash in a mass ratio of 7:3; calcium carbonate powder is a mixture of small-sized calcium carbonate powder and large-sized calcium carbonate powder of equal mass.
[0043] Example 2
[0044] The present embodiment provides a mineral admixture for improving the mixing efficiency of ultra-high performance concrete, which is a mixture of the following substances in percentage by mass:
[0045] Fly ash: 20%;
[0046] Nanoparticles: 8%;
[0047] Calcium carbonate powder: 71.9%;
[0048] Water repellent: 0.1%.
[0049] Among them, fly ash is a mixture of equal masses of Class I fly ash and ultrafine fly ash; nanoparticles are a mixture of silica ash and titanium powder in a mass ratio of 5:3; calcium carbonate powder is a mixture of small-sized calcium carbonate powder and large-sized calcium carbonate powder in a mass ratio of 7:3.
[0050] Example 3
[0051] The present embodiment provides a mineral admixture for improving the mixing efficiency of ultra-high performance concrete, which is a mixture of the following substances in percentage by mass:
[0052] Ultrafine fly ash: 10%;
[0053] Silica fume: 15%;
[0054] Calcium carbonate powder: 74.5%;
[0055] Powder dispersant: 0.3%;
[0056] Water repellent: 0.2%.
[0057] The calcium carbonate powder is a mixture of small-sized calcium carbonate powder and large-sized calcium carbonate powder in a mass ratio of 7:3; the powder dispersant is a mixture of equal masses of sodium tripolyphosphate and sodium dodecylbenzene sulfonate.
[0058] Example 4
[0059] The present embodiment provides a mineral admixture for improving the mixing efficiency of ultra-high performance concrete, which is a mixture of the following substances in percentage by mass:
[0060] Ultrafine fly ash: 40%;
[0061] Nanoparticles: 20%;
[0062] Calcium carbonate powder: 39%;
[0063] Powder dispersant: 0.35%;
[0064] Superplasticizer: 0.4%;
[0065] Water repellent: 0.2%;
[0066] Air entraining agent: 0.05%.
[0067] Among them, the calcium carbonate powder is a mixture of small-sized calcium carbonate powder and large-sized calcium carbonate powder in a mass ratio of 9:1; the nanoparticles are a mixture of equal masses of silica fume and titanium powder; and the powder dispersant is a mixture of sodium tripolyphosphate and sodium dodecylbenzene sulfonate in a mass ratio of 1:1.2.
[0068] In order to verify the excellent performance of the above-mentioned mineral admixture in the present invention, the following comparative experiment was conducted. The comparative experiment was based on the components in the above-mentioned Example 4, and the particle size of fly ash particles (Comparative Examples 1 and 2), the particle size of calcium carbonate powder particles (Comparative Examples 3 and 4), the amount of fly ash (Comparative Examples 5 and 6), the amount of calcium carbonate powder (Comparative Examples 7 and 8) and the amount of nanoparticles (Comparative Examples 9 and 10) were changed respectively to illustrate the importance of the above-mentioned components and their contents and properties.
[0069] Comparative Example 1
[0070] The similarities between this comparative example and Example 4 are not described here, and only the differences from Example 4 are described. The difference between Comparative Example 1 and Example 4 is that the ultrafine fly ash is replaced with an equal amount of Class I fly ash, that is, the fly ash component is composed of 100% Class I fly ash; the rest is as shown in Example 4, and a first comparative mineral admixture is provided.
[0071] Comparative Example 2
[0072] The similarities between this comparative example and Example 4 are not described here, and only the differences from Example 4 are described. The difference between Comparative Example 2 and Example 4 is that the ultrafine fly ash is replaced by a mixture of Class I fly ash and ultrafine fly ash in an equal amount at a mass ratio of 8:2, that is, the fly ash component is a mixture of Class I fly ash and ultrafine fly ash in a mass ratio of 8:2; the rest is as shown in Example 4, and a second comparative mineral admixture is provided.
[0073] Comparative Example 3
[0074] The similarities between this comparative example and Example 4 are not described here, and only the differences from Example 4 are described. The difference between Comparative Example 3 and Example 4 is that the small-sized calcium carbonate powder is replaced by large-sized calcium carbonate powder in equal amounts, that is, the calcium carbonate powder component is composed of 100% large-sized calcium carbonate powder; the rest is as shown in Example 4, and a third comparative mineral admixture is provided.
[0075] Comparative Example 4
[0076] The similarities between this comparative example and Example 4 are not described here, and only the differences from Example 4 are described. The difference between Comparative Example 4 and Example 4 is that the calcium carbonate powder is replaced by a mixture of equal amounts of small-sized calcium carbonate powder and large-sized calcium carbonate powder in a mass ratio of 3:7, that is, the calcium carbonate powder component is a mixture of small-sized calcium carbonate powder and large-sized calcium carbonate powder in a mass ratio of 3:7; the rest is as shown in Example 4, and a fourth comparative mineral admixture is provided.
[0077] Comparative Example 5
[0078] The similarities between this comparative example and Example 4 are not described here, and only the differences from Example 4 are described. The difference between Comparative Example 5 and Example 4 is that fly ash is replaced by an equal amount of calcium carbonate powder, that is, the system does not contain fly ash; the rest is as shown in Example 4, providing a fifth comparative mineral admixture.
[0079] Comparative Example 6
[0080] The similarities between this comparative example and Example 4 are not described here, and only the differences from Example 4 are described. The difference between Comparative Example 6 and Example 4 is that 10% of calcium carbonate powder is replaced with an equal amount of ultrafine fly ash, that is, the system includes 50% ultrafine fly ash, 26.1% small-sized calcium carbonate powder and 2.9% large-sized calcium carbonate powder; the rest is as shown in Example 4, providing a sixth comparative mineral admixture.
[0081] Comparative Example 7
[0082] The similarities between this comparative example and Example 4 are not described here, and only the differences from Example 4 are described. The difference between Comparative Example 7 and Example 4 is that the calcium carbonate powder is replaced with an equal amount of ultrafine fly ash, that is, the system does not contain calcium carbonate powder; the rest is as shown in Example 4, providing a seventh comparative mineral admixture.
[0083] Comparative Example 8
[0084] The similarities between this comparative example and Example 4 are not described here, and only the differences from Example 4 are described. The difference between Comparative Example 8 and Example 4 is that 36% of the ultrafine fly ash and 15% of the nanoparticles are replaced with an equal amount of calcium carbonate powder, that is, the system includes 4% of ultrafine fly ash, 5% of nanoparticles, 81% of small-sized calcium carbonate powder and 9% of large-sized calcium carbonate powder; the rest is as shown in Example 4, providing an eighth comparative mineral admixture.
[0085] Comparative Example 9
[0086] The similarities between this comparative example and Example 4 are not described here, and only the differences from Example 4 are described. The difference between Comparative Example 9 and Example 4 is that the nanoparticles are replaced with an equal amount of calcium carbonate powder, that is, the system does not contain nanoparticles; the rest is as shown in Example 4, providing a ninth comparative mineral admixture.
[0087] Comparative Example 10
[0088] The similarities between this comparative example and Example 4 are not described here, and only the differences from Example 4 are described. The difference between Comparative Example 10 and Example 4 is that 10% of ultrafine fly ash is replaced by an equal amount of nanoparticles, that is, the system includes 30% of ultrafine fly ash and 30% of nanoparticles; the rest is as shown in Example 4, providing a tenth comparative mineral admixture.
[0089] Comparative Example 11
[0090] The similarities between this comparative example and Example 4 are not described here, and only the differences from Example 4 are described. The difference between Comparative Example 11 and Example 4 is that all calcium carbonate powder is replaced with an equal amount of small-sized calcium carbonate powder, that is, the system includes 39% of small-sized calcium carbonate powder but does not contain large-sized calcium carbonate powder; the rest is as shown in Example 4, providing an eleventh comparative mineral admixture.
[0091] The mineral admixture provided by the present invention is particularly suitable for use in UHPC to improve its mixing efficiency. At the same time, in order to verify the effect of the mineral admixtures provided in the above embodiments after being applied to UHPC, the following application examples are provided.
[0092] Application Example 1
[0093] In this application example, the mineral admixtures provided in the above embodiments are used to replace cement in equal amounts according to the mix ratio of the benchmark concrete in Table 1 below, thereby obtaining four types of UHPC.
[0094] Table 1 Mix ratio of benchmark concrete and four types of UHPC
[0095] Unit: kg / m 3
[0096]
[0097] That is, in this application example, each mineral admixture provided by the present invention is added in an amount of 15% to replace cement, thereby obtaining UHPC.
[0098] At the same time, the same method is used to replace cement with the comparative mineral admixtures provided in the above comparative examples in equal amounts, thereby obtaining comparative UHPC.
[0099] The performance of UHPC obtained by applying the mineral admixtures provided in the above-mentioned embodiments of the present invention and the comparative examples was tested in terms of slurry discharge time, total stirring time, fluidity, viscosity, strength comparison, etc.
[0100] The slurry discharge time is the time from the time when water is added until the time when small balls with a diameter of 2mm to 3mm and a shiny surface appear in the stirring pot. Figure 1The judgment criteria for the slurry state are shown in the figure. The total mixing time is the time from the water addition time until the fibers are fully dispersed, wrapped, and no agglomeration occurs (excluding the time of adding fibers); the fluidity test method refers to GB / T 50080-2016 "Standard for Test Methods for Performance of Ordinary Concrete Mixtures"; the viscosity of concrete can be reflected by the collapse time. The longer the time, the greater the viscosity of the concrete. The inverted slump cone emptying test refers to GB / T 50080-2016 "Standard for Test Methods for Performance of Ordinary Concrete Mixtures"; the compressive strength test method refers to GB / T 31387-2015 "Reactive Powder Concrete", and the 28d strength is tested.
[0101] The performance test results of each UHPC and the comparative UHPC provided in this application example are shown in Table 2 below.
[0102] Table 2 Performance test results of various UHPC (equivalent replacement of cement) and comparative UHPC
[0103]
[0104]
[0105] The performance data of UHPC (equivalent replacement of cement) obtained by using the mineral admixtures of Examples 1 to 4 in Table 2 show that when the mineral admixture for improving mixing efficiency of the present invention is used to replace cement, the slurry discharge time of UHPC can be significantly reduced. The mineral admixture can shorten the slurry discharge time by 41.7% to 80% and shorten the total mixing time by 36.4% to 72.7% at a dosage of 15%. In addition, the mineral admixture can also improve the fluidity of the UHPC mixture by 3.4% to 29.3%, reduce the viscosity by 31.2% to 68.8%, and increase the 28d compressive strength by 5% to 10%.
[0106] However, from the performance data of the comparative UHPC obtained by using the comparative mineral admixtures of Comparative Examples 1 to 11, it can be seen that: when all coarser Class I fly ash and large-sized calcium carbonate powder with a size of 5μm to 20μm are used, although the viscosity of the mixture is reduced due to the decrease in the proportion of ultrafine powder, the filling effect of fine particles is weakened, and free water cannot be effectively released to increase the density of the matrix, which in turn leads to extended slurry discharge time and stirring time and reduced compressive strength; while supplementing a certain proportion of ultrafine fly ash and small-sized calcium carbonate powder with a size of 1μm to 5μm can improve the adverse effects on slurry discharge time and stirring time to a certain extent, but the compressive strength still shows a downward trend. When the amount of fly ash and calcium carbonate powder exceeds the specified range, although the slurry discharge time and stirring time are shortened, the excessive reduction in the viscosity of the mixture and the increase in the inert components cause the settlement of the fibers and aggregates in the UHPC, and the uneven distribution of the phases in the hardened UHPC, resulting in a reduction in the most basic and important performance indicator of UHPC - the compressive strength (using the comparative mineral admixtures described in Comparative Examples 5 to 8 and 11).
[0107] In addition, for nanoparticles, when the mineral admixture does not contain nanoparticles, since the UHPC mix contains silica fume, at this time, although there is a negative impact on it, it is not obvious, and the slurry discharge time and stirring time only increase by about 10%; when the nanoparticle content in the invented admixture exceeds 30%, due to the substantial increase in the specific surface energy of the particles, the particle agglomeration effect is enhanced, and the adsorption of water and water reducer is obvious. At this time, it is not conducive to the uniform dispersion of the particles to form a stable suspension system. Therefore, its slurry discharge time and stirring time are also significantly extended (using the comparative mineral admixtures described in Comparative Examples 9 to 10).
[0108] Application Example 2
[0109] In this application example, the mineral admixtures provided in the above embodiments are used to replace silica fume in equal amounts according to the mix ratio of the benchmark concrete in Table 3 below, thereby obtaining another four types of UHPC.
[0110] Table 2 Mix ratio of benchmark concrete and four types of UHPC
[0111] Unit: kg / m 3
[0112]
[0113] That is, in this application example, the mineral admixtures provided by the present invention are added in an amount of 15% to replace silica fume, thereby obtaining UHPC.
[0114] At the same time, the same method is used to replace the silica fume with the comparative mineral admixtures provided in the above comparative examples in equal amounts, thereby obtaining comparative UHPC.
[0115] The UHPCs and comparative UHPCs in this application example were tested using the same method as in the above application example 1, and the performance test results are shown in Table 4 below.
[0116] Table 4 Performance test results of various UHPC (equivalent replacement of silica fume) and comparative UHPC
[0117]
[0118]
[0119] The performance data of the UHPC obtained by using the mineral admixtures of Examples 1 to 4 in Table 4 (replacing silica fume in equal amounts) show that when the mineral admixture for improving mixing efficiency of the present invention is used to replace silica fume, the slurry discharge time of UHPC can be significantly reduced. The mineral admixture can shorten the slurry discharge time by 20.0% to 83.3% and shorten the total mixing time by 28.2% to 75.5% at a dosage of 15%. In addition, the admixture can also reduce the viscosity of the ultra-high performance concrete mixture by 12.3% to 61.0% and increase the 28d compressive strength by 1.4% to 6.6%.
[0120] However, from the performance data of the comparative UHPC obtained by using the comparative mineral admixtures of Comparative Examples 1 to 11, it can be seen that: due to the replacement of silica fume at this time, the nano-sized particles in the entire mix ratio are greatly reduced. When all coarser Class I fly ash and large-sized calcium carbonate powder with a size of 5μm to 20μm are used, although the viscosity of the mixture is reduced due to the decrease in the proportion of ultrafine powder, the filling effect of the micro-nano particles is weakened, the active components are reduced, and the free water cannot be effectively released to increase the density of the matrix, resulting in extended slurry discharge time and stirring time and reduced compressive strength, and the negative effect is stronger than when replacing cement; supplementing a certain proportion of ultrafine fly ash and small-sized calcium carbonate powder with a size of 1μm to 5μm can improve the adverse effects on slurry discharge time and stirring time to a certain extent, but the overall adverse effects are still very significant. When the amount of fly ash and calcium carbonate powder exceeds the prescribed range, although the negative effect on the slurry discharge time and mixing time is weak, due to the excessively high content of inert components, its adverse effect on the compressive strength of UHPC is more significant (using the comparative mineral admixtures described in Comparative Examples 5 to 8 and 11).
[0121] In addition, for nanoparticles, when the mineral admixture does not contain nanoparticles, since the UHPC mix also does not contain silica fume, at this time, the admixture has a significant adverse effect on the slurry discharge time, stirring time and strength; and when the content of nanoparticles in the mineral admixture exceeds 30%, due to the increase in nanoparticles, the active components and filling effect are improved, and at this time, the adverse effects on the slurry discharge time, stirring time and strength basically disappear. However, nanoparticles are very easy to agglomerate and have extremely high surface energy, so the dosage cannot be too high (using the comparative mineral admixtures described in Comparative Examples 9 to 10).
[0122] In summary, the "mineral admixture for improving the mixing efficiency of ultra-high performance concrete" of the present invention is reasonably matched through effective filling of different particle sizes, reasonable control of the total surface energy of particles, and the ball effect of particle shape and the self-dispersion effect of particle surface characteristics, so as to shorten the slurry discharge time and mixing time, effectively reduce the viscosity of UHPC, and improve the mechanical properties. These components influence each other in matching, and do not exist independently.
[0123] While the invention has been shown and described with reference to the particular embodiments, it will be understood by those skilled in the art that various changes in form and details may be made therein without departing from the spirit and scope of the invention as defined by the claims and their equivalents.
Claims
1. A mineral admixture for improving the mixing efficiency of ultra-high performance concrete, It is characterized in that The composition comprises the following components in the following weight proportions, with the total weight of the mineral admixture being 100%: Fly ash 10%~40%; Calcium carbonate powder 39%~85%; Nanoparticles 5%~20%; The fly ash is a mixture of 0-70% of Class I fly ash and 30%-100% of ultrafine fly ash; wherein the Class I fly ash has a fineness of 45 μm square mesh sieve residue of no more than 10%, and the ultrafine fly ash has an average particle size of 1 μm-5 μm; the percentages of the Class I fly ash and the ultrafine fly ash are both calculated based on the total mass of the fly ash; The density of the calcium carbonate powder is not less than 2.6 kg / m 3 , with an average particle size of 1 μm to 20 μm; the calcium carbonate powder is formed by mixing 10% to 50% of small-sized calcium carbonate powder with a particle size of 1 μm to 5 μm and 50% to 90% of large-sized calcium carbonate powder with a particle size of 5 μm to 20 μm; the percentages of the small-sized calcium carbonate powder and the large-sized calcium carbonate powder are both calculated based on the total mass of the calcium carbonate powder; The nanoparticles are selected from silica fume and / or titanium powder; wherein the average particle size of the silica fume is 0.1 μm to 0.9 μm, and the specific surface area is greater than 18000 m 2 / kg; the average particle size of titanium powder is 0.2 μm~1.3 μm, and the specific surface area is greater than 12000 m 2 / kg.
2. The mineral admixture according to claim 1, It is characterized in that The nanoparticles are spherical nanoparticles.
3. A mineral admixture for improving the mixing efficiency of ultra-high performance concrete, It is characterized in that It includes the following components in proportion by mass: Fly ash 10%~40%; Calcium carbonate powder 39%~85%; Nanoparticles 5%~20%; And at least one of the following components in the following mass proportions: Powder dispersant does not exceed 0.35%; Superplasticizer does not exceed 0.4%; The water repellent does not exceed 0.2%; Air entraining agent shall not exceed 0.05%; The total mass of the mineral admixture is 100%; The fly ash is a mixture of 0-70% of Class I fly ash and 30%-100% of ultrafine fly ash; wherein the Class I fly ash has a fineness of 45 μm square mesh sieve residue of no more than 10%, and the ultrafine fly ash has an average particle size of 1 μm-5 μm; the percentages of the Class I fly ash and the ultrafine fly ash are both calculated based on the total mass of the fly ash; The density of the calcium carbonate powder is not less than 2.6 kg / m 3 , with an average particle size of 1 μm to 20 μm; the calcium carbonate powder is formed by mixing 10% to 50% of small-sized calcium carbonate powder with a particle size of 1 μm to 5 μm and 50% to 90% of large-sized calcium carbonate powder with a particle size of 5 μm to 20 μm; the percentages of the small-sized calcium carbonate powder and the large-sized calcium carbonate powder are both calculated based on the total mass of the calcium carbonate powder; The nanoparticles are selected from silica fume and / or titanium powder; wherein the average particle size of the silica fume is 0.1 μm to 0.9 μm, and the specific surface area is greater than 18000 m 2 / kg; the average particle size of titanium powder is 0.2 μm~1.3 μm, and the specific surface area is greater than 12000 m 2 / kg.
4. The mineral admixture according to claim 3, It is characterized in that The nanoparticles are spherical nanoparticles.
5. The mineral admixture according to claim 3 or 4, It is characterized in that The powder dispersant is a mixture of sodium tripolyphosphate and sodium dodecylbenzene sulfonate in a mass ratio of 1 to 1.2:1; the superplasticizer is a powder polycarboxylic acid water reducer with a water reduction rate of not less than 30%; the hydrophobic agent is an organosilicon powder hydrophobic agent; and the air entraining agent is a sodium rosin acid powder air entraining agent.
6. An ultra-high performance concrete with high mixing efficiency, It is characterized in that The mineral admixture described in any one of claims 1 to 5 is added to the concrete cementitious material in an equal volume or mass to replace cement, or in an equal volume or mass to replace silica fume; wherein the mass of the mineral admixture is 10% to 20% of the total mass of the concrete cementitious material.
Citation Information
Patent Citations
Ultra high performance concrete stirring technology
CN110240452A
Vacuum stirring process for ultra-high-performance concrete
CN110281392A
Ultra-high performance concrete vacuum variable-frequency type stirring process
CN110317022A
Viscosity modifier for high or ultrahigh-strength concrete
CN103145360A
High-performance concrete slurry-shaped admixture mixed by CaCO3 having multi-scale particle sizes
CN108546009A
Cited By
Nanometer seed crystal additive for UHPC (Ultra High Performance Concrete) and preparation method of nanometer seed crystal additive
CN119797805A
A nanocrystal seed additive for UHPC and its preparation method
CN119797805B