Preparation method and application of 3D NASICON-type oxide ceramic skeleton

Through the preparation of 3D NASICON type oxide ceramic skeleton, the problems of lithium ion transmission obstruction and poor interface compatibility caused by the large surface energy of inorganic ceramic electrolytes are solved, achieving high conductivity and long life of lithium-ion batteries, and improving the overall performance of the battery. performance.

CN117886598BActive Publication Date: 2024-10-08HARBIN UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410082909.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-19
Publication Date
2024-10-08
Estimated Expiration
2044-01-19

AI Technical Summary

Technical Problem

The surface energy of existing inorganic ceramic electrolytes is relatively large, which results in blocked lithium ion transmission and poor interface compatibility, affecting the safety and performance of lithium-ion batteries.

Method used

Using the preparation method of 3D NASICON type oxide ceramic skeleton, ceramic sheets with porous structure are prepared through a combination of template removal method and high-temperature sintering, which provide continuous lithium ion transmission channels, increase conductivity and improve interface compatibility.

Benefits of technology

Significantly improve the ionic conductivity and cycle stability of lithium-ion batteries, extend the service life of the battery, and improve the electrochemical window and thermal stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117886598B_ABST
    Figure CN117886598B_ABST
Patent Text Reader

Abstract

A preparation method and application of a 3D NASICON-type oxide ceramic skeleton, which relates to a preparation method and application of a ceramic skeleton. The purpose of the present invention is to solve the problems of relatively large surface energy, easy agglomeration, obstruction of lithium ion transmission and poor interface compatibility of existing inorganic ceramic electrolytes. The present invention provides a method for preparing a three-dimensional skeleton of a NASICON-type oxide ceramic and applies it to lithium metal batteries; the invention prepares a LATP ceramic sheet with a 3D continuous pore structure by combining a de-templating method and high-temperature sintering. A 3D NASICON-type oxide ceramic skeleton is used as a solid electrolyte in an all-solid-state lithium metal battery. A 3D NASICON-type oxide ceramic skeleton provided by the present invention has high cycle stability and service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method and application of a ceramic skeleton. Background Art

[0002] With the rapid growth of population and rapid social development, human demand for energy has risen sharply. The main way for humans to obtain energy is the burning of fossil fuels. However, the burning of large amounts of fossil fuels will be accompanied by environmental pollution and energy depletion. Therefore, the development of clean and efficient new energy and the vigorous development of energy storage and conversion technologies are considered to be the most effective ways to alleviate the energy and ecological crisis. At present, energy storage devices such as lithium-ion batteries, supercapacitors, and fuel cells have triggered an unprecedented research boom due to their advantages such as green environmental protection and eco-friendliness. Lithium metal has an ultra-high specific capacity (3860mAhg –1 ), lower density (0.59gcm –3 ) and the lowest potential (−3.04 V vs H + / H2), is widely used as a promising anode candidate for the manufacture of high energy density batteries. The development of lithium-ion batteries (LIBs) not only provides a huge market for portable electronic devices, but also promotes the practical commercialization of new energy vehicles and electric ships. At the same time, LIBs reduce dependence on fossil fuels, reduce pollution to the ecological environment, and promote the use of clean energy. However, most commercial lithium-ion batteries currently use organic liquid electrolytes, which have serious safety issues due to their poor oxidation resistance, flammability and explosion, and poor compatibility with lithium metal anodes. Compared with liquid electrolytes, solid electrolytes (SSEs) are non-volatile, non-leaky, and non-flammable. Replacing liquid electrolytes with solid electrolytes is expected to fundamentally solve the safety problems of lithium batteries.

[0003] SSEs are mainly divided into three types: solid polymer electrolytes, inorganic ceramic electrolytes (ICEs) and solid composite electrolytes. ICEs have been widely studied due to their high room temperature ionic conductivity, high high voltage oxidation resistance and excellent mechanical stability. The most widely studied ICEs include NASICON type [Li 1+x Al x Ti 2-x (PO4)3, Li 1+ x Al x Ge 2-x (PO4)3], LISICON type (Li 1+x Zn 1-x GeO4), garnet type (Li7La3Zr2O 12 ), perovskite type (Li 0.34 La 0.51 TiO2.94 ), sulfide, LiPON, etc. NASICON solid electrolyte (LATP (Li 1.3 Al 0.3 Ti 1.7 (PO4)3) can conduct not only sodium ions but also lithium ions. This type of electrolyte has high ionic conductivity (close to 1mScm at room temperature). –1 ), low density (~2.9 g cm –3 ), excellent stability in water and air (due to the strong PO bond in the LATP structure), and relatively low price, so it has received widespread attention and research.

[0004] Since ceramic particles have a relatively large surface energy, they tend to agglomerate, which hinders the transmission of lithium ions. Summary of the invention

[0005] The purpose of the present invention is to solve the problems of relatively large surface energy, easy agglomeration, hindering lithium ion transmission and poor interface compatibility of existing inorganic ceramic electrolytes, and to provide a preparation method and application of a 3D NASICON type oxide ceramic skeleton.

[0006] A method for preparing a 3D NASICON-type oxide ceramic skeleton is specifically completed by the following steps:

[0007] 1. Preparation of ceramic sheets:

[0008] Li 1.3 Al 0.3 Ti 1.7 P3O 12 The ceramic powder and polyvinyl alcohol are mixed in a mortar and fully ground to obtain a mixed powder; the mixed powder is placed in a tablet pressing mold, and the tablet pressing mold is placed in a tablet pressing machine to press into a ceramic tablet;

[0009] 2. Calcination:

[0010] The bottom and the top of the ceramic sheet are respectively covered with the mixed powder prepared in step 1, and the mixture is placed in a crucible, and the crucible is placed in a muffle furnace for sintering. The sintering process is as follows: first, the muffle furnace is heated to 230°C to 240°C, sintered at 230°C to 240°C for 2h to 2.5h, then heated to 850°C to 900°C, sintered at 850°C to 900°C for 6h to 6.5h, then cooled to 200°C to 220°C, and then naturally cooled to room temperature and taken out to obtain an oxide ceramic skeleton;

[0011] 3. Polishing, cleaning and drying:

[0012] The surface of the oxide ceramic skeleton was polished smooth using sandpaper, then ultrasonically cleaned and dried to obtain a 3D NASICON-type oxide ceramic skeleton.

[0013] A 3D NASICON-type oxide ceramic skeleton is used as a solid electrolyte in all-solid-state lithium metal batteries.

[0014] Principle of the present invention:

[0015] The present invention provides a method for preparing a three-dimensional framework of NASICON-type oxide ceramics and applying it to lithium metal batteries; the invention prepares a LATP ceramic sheet with a 3D continuous pore structure by combining a template removal method with high-temperature sintering, and the porous electrolyte has several advantages; for example, the porous structure can relieve the stress generated during the electrochemical cycle; in addition, the pores can be infiltrated by different materials to meet the requirements of special applications, such as mixed electron / ion conductors and composite ion conductors; the three-dimensional framework can provide a continuous lithium ion rapid transmission channel, greatly improving the conductivity of the electrolyte; in addition, the solid electrolyte with a three-dimensional framework has good thermal stability and interface compatibility.

[0016] Advantages of the present invention:

[0017] Compared with the traditional commercial glass fiber separator (GF), the 3D NASICON oxide ceramic skeleton prepared by the present invention has an ionic conductivity of 1.67×10 –3 Scm –1 Increased to 2.57×10 –3 Scm –1 The ion migration number is increased from 0.05 to 0.31, and the electrochemical window is changed from 1.52V-4.3V to 0.2V-4.75V; a Li||Li symmetric battery assembled by a 3D NASICON oxide ceramic skeleton (LATP PVA) prepared by the present invention has a high conductivity at 0.1mAcm −2 The current density provided more than 4100 h of stable cycling during plating and stripping, and the assembled (lithium iron phosphate) LFP||Li full cell had 141 mAh g at a rate of 0.5 C. –1 The discharge specific capacity of the battery is 99.5%, and the capacity retention rate is 99.5% after 170 cycles. This indicates that the 3D N SICON oxide ceramic skeleton provided by the present invention has high cycle stability and service life. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1The scanning electron microscope image and XRD pattern of the LATP PVA prepared in Example 1, (a) and (d) are scanning electron microscope images of the cross section before cycling, (b) and (e) are scanning electron microscope images of the surface before cycling, (c) and (f) are appearance images, and (g) is the XRD spectrum of the LATP PVA prepared in Example 1;

[0019] Figure 2 (a) is the chronoamperometric curve of the lithium symmetric battery Li|GF|Li assembled with GF, (b) is the chronoamperometric curve of the lithium symmetric battery Li|LATP PVA|Li assembled with LATP PVA, and (c) is the chronoamperometric curve of the lithium symmetric battery Li|LATP PVA|Li assembled with LATP PVA at 0.1 mVs −1 (d) is the electrochemical voltage window curve of the lithium symmetric battery assembled with GF and the lithium symmetric battery assembled with LATP PVA at a scan rate of , (d) is the temperature-dependent ionic conductivity of GF and LATP PVA;

[0020] Figure 3 (a) is at 25 ℃, 0.1 mAcm −2 The constant current cycle curves of Li|GF|Li and Li|LATP PVA|Li symmetric batteries at a current density of 0.1 mA cm-1 at 40 °C. −2 The constant current cycling curve of Li|LATP PVA|Li symmetric battery at the current density of;

[0021] Figure 4 The electrochemical performance curve of LFP|LATP PVA|Li full battery assembled with LATP PVA at 0.5C rate;

[0022] Figure 5 Rate performance curve of LFP|LATP PVA|Li full cell assembled with LATP PVA at different current densities. DETAILED DESCRIPTION

[0023] Specific implementation method 1: This implementation method is a method for preparing a 3D NASICON type oxide ceramic skeleton, which is specifically completed according to the following steps:

[0024] 1. Preparation of ceramic sheets:

[0025] Li 1.3 Al 0.3 Ti 1.7 P3O 12 The ceramic powder and polyvinyl alcohol are mixed in a mortar and fully ground to obtain a mixed powder; the mixed powder is placed in a tablet pressing mold, and the tablet pressing mold is placed in a tablet pressing machine to press into a ceramic tablet;

[0026] 2. Calcination:

[0027] The bottom and the top of the ceramic sheet are respectively covered with the mixed powder prepared in step 1, and the mixture is placed in a crucible, and the crucible is placed in a muffle furnace for sintering. The sintering process is as follows: first, the muffle furnace is heated to 230°C to 240°C, sintered at 230°C to 240°C for 2h to 2.5h, then heated to 850°C to 900°C, sintered at 850°C to 900°C for 6h to 6.5h, then cooled to 200°C to 220°C, and then naturally cooled to room temperature and taken out to obtain an oxide ceramic skeleton;

[0028] 3. Polishing, cleaning and drying:

[0029] The surface of the oxide ceramic skeleton was polished smooth using sandpaper, then ultrasonically cleaned and dried to obtain a 3D NASICON-type oxide ceramic skeleton.

[0030] Specific implementation method 2: This implementation method is different from the specific implementation method 1 in that: the Li 1.3 Al 0.3 Ti 1.7 P3O 12 The mass ratio of ceramic powder to polyvinyl alcohol is 6:4. The other steps are the same as those in the first embodiment.

[0031] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that: the pressure of the tablet press described in step 1 is 250MPa-270MPa, and the holding time is 1min-1.5min. The other steps are the same as specific implementation method 1 or 2.

[0032] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that the diameter of the ceramic sheet in step 1 is 16 mm to 16.2 mm and the thickness is 1.4 mm to 1.45 mm. The other steps are the same as those of specific embodiments 1 to 3.

[0033] Specific embodiment 5: This embodiment differs from specific embodiments 1 to 4 in that the heating rate in step 2 is 2°C min –1 ~2.5℃min –1 The other steps are the same as those in Specific Embodiments 1 to 4.

[0034] Specific implementation method 6: The difference between this implementation method and specific implementation methods 1 to 5 is that the cooling rate described in step 2 is 5 ° C min –1 ~6℃min –1 The other steps are the same as those in Specific Embodiments 1 to 5.

[0035] Specific embodiment 7: This embodiment differs from specific embodiments 1 to 6 in that: in step 3, the surface of the oxide ceramic skeleton is polished smooth using 400-grit sandpaper, then ultrasonically cleaned in isopropanol for 3 to 5 times, and then dried in an oven at 80°C to 100°C for 12h to 24h to obtain a 3D NASICON oxide ceramic skeleton. The other steps are the same as those of specific embodiments 1 to 6.

[0036] Specific implementation example eight: This implementation example is a 3D NASICON-type oxide ceramic skeleton used as a solid electrolyte in an all-solid-state lithium metal battery.

[0037] Specific embodiment 9: The difference between this embodiment and specific embodiments 1 to 8 is that a 3D N SICON type oxide ceramic skeleton is used as a solid electrolyte, and the assembly of the all-solid-state lithium metal battery LFP | LATP PVA | Li is specifically completed in the following steps:

[0038] 1. Preparation of ionic liquid electrolyte containing LiTFSI:

[0039] Adding lithium bis(trifluoromethanesulfonyl imide) to 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl imide) salt to obtain an ionic liquid electrolyte containing LiTFSI;

[0040] The concentration of lithium bis(trifluoromethanesulfonyl)imide in the ionic liquid electrolyte containing LiTFSI in step 1 is 0.4 mol / L to 0.45 mol / L;

[0041] 2. Assemble the battery:

[0042] Prepare a negative electrode shell, place a spring, place a gasket, place a 12 mm lithium sheet, place a 3D NASICON oxide ceramic skeleton, drop 25 μL of ionic liquid electrolyte containing LiTFSI on both sides of the 3D NASICON oxide ceramic skeleton, then place 12 mm lithium iron phosphate, then cover the positive electrode shell, and put it into a button battery packaging machine to complete the packaging. The other steps are the same as those in specific embodiments one to eight.

[0043] Specific embodiment 10: This embodiment differs from specific embodiments 1 to 9 in that: a 3D N ASICON type oxide ceramic skeleton is used as a solid electrolyte to assemble a lithium-ion symmetric battery Li|LATP PVA|Li, which is specifically completed in the following steps:

[0044] 1. Preparation of ionic liquid electrolyte containing LiTFSI:

[0045] Adding lithium bis(trifluoromethanesulfonyl imide) to 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl imide) salt to obtain an ionic liquid electrolyte containing LiTFSI;

[0046] The concentration of lithium bis(trifluoromethanesulfonyl)imide in the ionic liquid electrolyte containing LiTFSI in step 1 is 0.4 mol / L to 0.45 mol / L;

[0047] 2. Assemble the battery:

[0048] Prepare a negative electrode shell, place a spring, place a gasket, place a 12 mm lithium sheet, place a 3D NASICON oxide ceramic skeleton, drop 25 μL of ionic liquid electrolyte containing LiTFSI on both sides of the 3D NASICON oxide ceramic skeleton, then place a 12 mm lithium sheet, then cover the positive electrode shell, and place it in a button battery packaging machine to complete the packaging. The other steps are the same as the specific embodiments one to nine.

[0049] The following examples are used to verify the beneficial effects of the present invention:

[0050] Example 1: A method for preparing a 3D NASICON-type oxide ceramic skeleton is specifically completed by the following steps:

[0051] 1. Preparation of ceramic sheets:

[0052] Li 1.3 Al 0.3 Ti 1.7 P3O 12 Ceramic powder (LATP) and polyvinyl alcohol (PVA) were mixed in a mortar and ground thoroughly to obtain a mixed powder; 400 mg of the mixed powder was placed in a tablet pressing mold, and the tablet pressing mold was placed in a manual tablet pressing machine with a pressure of 250 MPa and a holding time of 1 min to press into a ceramic sheet with a diameter of 16 mm and a thickness of 1.4 mm;

[0053] Li described in step 1 1.3 Al 0.3 Ti 1.7 P3O 12 The mass ratio of ceramic powder to polyvinyl alcohol is 6:4;

[0054] 2. Calcination:

[0055] The bottom and the top of the ceramic sheet are respectively covered with the mixed powder prepared in step 1, and then placed in a crucible, and then the crucible is placed in a muffle furnace for sintering. The sintering process is as follows: first, the muffle furnace is heated to 230°C, sintered at 230°C for 2h, then heated to 850°C, sintered at 850°C for 6h, then cooled to 200°C, and then naturally cooled to room temperature and taken out to obtain an oxide ceramic skeleton;

[0056] The heating rate in step 2 is 2°C min –1 ;

[0057] The cooling rate described in step 2 is 5°C min –1 ;

[0058] 3. Polishing, cleaning and drying:

[0059] The surface of the oxide ceramic skeleton was polished smooth using 400-mesh sandpaper, ultrasonically cleaned in isopropanol three times, and then dried in an oven at 80°C for 12 hours to obtain a 3D NASICON-type oxide ceramic skeleton (LATP PVA).

[0060] Assembling lithium symmetric battery I:

[0061] Using the 3D NASICON-type oxide ceramic framework (LATP PVA) prepared in Example 1 as a solid electrolyte, the assembly of the lithium symmetric battery Li|LATPPVA|Li is specifically completed in the following steps:

[0062] 1. Preparation of ionic liquid electrolyte containing LiTFSI:

[0063] Adding lithium bis(trifluoromethanesulfonyl imide) to 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl imide) salt to obtain an ionic liquid electrolyte containing LiTFSI;

[0064] The concentration of lithium bis(trifluoromethanesulfonyl)imide in the ionic liquid electrolyte containing LiTFSI in step 1 is 0.4 mol / L;

[0065] 2. Assemble the battery:

[0066] Prepare a negative electrode shell, place a spring, place a gasket, place a 12 mm lithium sheet, place a 3D NASICON-type oxide ceramic skeleton, add 25 μL of ionic liquid electrolyte containing LiTFSI on both sides of the 3D NASICON-type oxide ceramic skeleton, then place a 12 mm lithium sheet, then cover the positive electrode shell, and put it into a button battery packaging machine to complete the packaging.

[0067] Assembling lithium symmetric battery II: The difference between this method and assembling lithium symmetric battery I is that the 3D N ASICON type oxide ceramic framework (LATP PVA) prepared in Example 1 is replaced with a traditional commercial glass fiber separator (GF), and the other steps and parameters are the same as those of assembling lithium symmetric battery I to obtain a lithium symmetric battery Li|GF|Li.

[0068] Assembling the full battery Ⅰ:

[0069] Using the 3D NASICON-type oxide ceramic skeleton (LATP PVA) prepared in Example 1 as the solid electrolyte, the assembly of the LFP|LATPPVA|Li full battery is specifically completed in the following steps:

[0070] 1. Preparation of ionic liquid electrolyte containing LiTFSI:

[0071] Adding lithium bis(trifluoromethanesulfonyl imide) to 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl imide) salt to obtain an ionic liquid electrolyte containing LiTFSI;

[0072] The concentration of lithium bis(trifluoromethanesulfonyl)imide in the ionic liquid electrolyte containing LiTFSI in step 1 is 0.4 mol / L;

[0073] 2. Assemble the battery:

[0074] Prepare a negative electrode shell, place a spring, place a gasket, place a 12mm lithium sheet, place a 3D NASICON-type oxide ceramic skeleton, add 25μL of ionic liquid electrolyte containing LiTFSI on both sides of the 3D NASICON-type oxide ceramic skeleton, then place 12mm lithium iron phosphate, then cover the positive electrode shell, and put it into a button battery packaging machine to complete the packaging.

[0075] Figure 1 The scanning electron microscope image and XRD pattern of the LATP PVA prepared in Example 1, (a) and (d) are scanning electron microscope images of the cross section before cycling, (b) and (e) are scanning electron microscope images of the surface before cycling, (c) and (f) are appearance images, and (g) is the XRD spectrum of the LATP PVA prepared in Example 1;

[0076] The microscopic morphology of the LATP PVA prepared in Example 1 is shown in Figures (a, b). After sintering, the LATP PVA ceramic sheet prepared in Example 1 has uniform pores inside and on the surface, and the pore size is 20-40 μm. Figure 1 (g) is the XRD spectrum of LATP PVA prepared in Example 1, which is completely consistent with the standard crystal card PDF-035-0754 of LTP, and has no obvious impurity peak. The appearance of the prepared LATP PVA ceramic sheet prepared in Example 1 is as follows: Figure 1 (c, f), white in color, 1.35 cm in diameter, and 1.103 mm in thickness.

[0077] Figure 2 (a) is the chronoamperometric curve of the lithium symmetric battery Li|GF|Li assembled with GF, (b) is the chronoamperometric curve of the lithium symmetric battery Li|LATP PVA|Li assembled with LATP PVA, and (c) is the chronoamperometric curve of the lithium symmetric battery Li|LATP PVA|Li assembled with LATP PVA at 0.1 mVs −1(d) is the electrochemical voltage window curve of the lithium symmetric battery assembled with GF and the lithium symmetric battery assembled with LATP PVA at a scan rate of , (d) is the temperature-dependent ionic conductivity of GF and LATP PVA;

[0078] Figure 2 (a, b) show the calculated ion migration numbers of GF and LATP PVA. Compared with the traditional commercial GF separator, LATP PVA has a higher ion migration number. Among them, the ion migration number of GF is 0.05, while the ion migration number of LATP PVA is 0.32. This is because the solid electrolyte combines the functions of both liquid electrolyte and separator, acting as an ion conduction medium while also taking into account the function of the separator, preventing the occurrence of battery short circuit. Figure 2 (a, b) show the calculated ion migration numbers of GF and LATP PVA. Compared with the traditional commercial GF separator, LATP PVA has a higher ion migration number. Among them, the ion migration number of GF is 0.05, while the ion migration number of LATP PVA is 0.32. This is because the solid electrolyte combines the functions of both liquid electrolyte and separator, acting as an ion conduction medium while also taking into account the function of the separator, preventing the occurrence of battery short circuit.

[0079] By using a symmetrical lithium battery and −2 The interfacial stability of the prepared LATPPVA and GF toward Li metal was evaluated by cycling at a current density of . Figure 3 (a) shows that the polarization of the Li|GF|Li symmetric battery increases sharply after cycling for more than 240 hours, while the Li|LATP PVA|Li symmetric battery provides a cycle life of more than 4100 hours during the electroplating and stripping process, which is more than 17 times that of the Li|GF|Li symmetric battery. In addition, at 40°C, Li|LATP PVA|Li provides more than 2500 hours of stable and uninterrupted cycling during the electroplating and stripping process, which also shows that the ceramic electrolyte lithium symmetric battery of the present invention has an ultra-long cycle life in both room temperature and high temperature environments.

[0080] Figure 4 Figure 2 shows the charge / discharge cycle performance of the LFP|LATP PVA|Li full cell at 0.5 C. The LFP|LATPPVA|Li full cell exhibits a charge / discharge cycle performance of 141 mAh g −1 The initial discharge capacity of LFP|LATP PVA|Li battery has a capacity retention rate of >99.5% after 170 cycles. The high cycle stability and capacity retention rate of LFP|LATP PVA|Li battery are due to the large Young's modulus and good mechanical properties of the solid electrolyte, which can better inhibit the formation of lithium dendrites and prevent internal short circuits in the battery, as well as the strong chemical oxidation-reduction resistance of the solid electrolyte and the high efficiency of ion transmission between the positive and negative electrodes.

[0081] Figure 5 The rate performance curves of the LFP|LATP PVA|Li full cell at different current densities (0.05C, 0.1C, 0.2C, 0.3C, 0.5C) are shown, following a procedure of five charge and discharge cycles at room temperature. The initial discharge capacities of the LFP|LATP PVA|Li cell at 0.05C, 0.1C, 0.2C, 0.3C, 0.5C are 167.8, 160, 158.52, 152.86, and 147.55 mAh g −1 , the rate performance is good.

Claims

1. Application of a 3D NASICON-type oxide ceramic framework, characterized in that A 3D NASICON-type oxide ceramic skeleton is used as a solid electrolyte in all-solid-state lithium metal batteries; a Li|LATP PVA|Li symmetric cell assembled using a 3D NASICON-type oxide ceramic skeleton has a high conductivity at 0.1 mA cm −2 The current density provided more than 4100 h of stable cycling during plating and stripping, and the assembled LFP|LATP PVA|Li full cell had 141 mAh g at a rate of 0.5 C. –1 The discharge specific capacity of the battery is 99.5% after 170 cycles. The method for preparing a 3D NASICON-type oxide ceramic skeleton is specifically completed according to the following steps:

1. Preparation of ceramic sheets: Li 1.3 Al 0.3 Ti 1.7 P3O 12 The ceramic powder and polyvinyl alcohol are mixed in a mortar and fully ground to obtain a mixed powder; the mixed powder is placed in a tablet pressing mold, and the tablet pressing mold is placed in a tablet pressing machine to press into a ceramic tablet; Li described in step 1 1.3 Al 0.3 Ti 1.7 P3O 12 The mass ratio of ceramic powder to polyvinyl alcohol is 6:4; The pressure of the tablet press described in step 1 is 250MPa~270MPa, and the holding time is 1min~1.5min; The diameter of the ceramic sheet described in step 1 is 16 mm to 16.2 mm, and the thickness is 1.4 mm to 1.45 mm; 2. Calcination: The bottom and the top of the ceramic sheet are respectively covered with the mixed powder prepared in step 1, and the mixture is placed in a crucible, and the crucible is placed in a muffle furnace for sintering. The sintering process is as follows: first, the muffle furnace is heated to 230°C to 240°C, sintered at 230°C to 240°C for 2h to 2.5h, then heated to 850°C to 900°C, sintered at 850°C to 900°C for 6h to 6.5h, then cooled to 200°C to 220°C, and then naturally cooled to room temperature and taken out to obtain an oxide ceramic skeleton; The heating rate in step 2 is 2°C min –1 ~2.5℃min –1 ; The cooling rate described in step 2 is 5°C min –1 ~6℃min –1 ; 3. Polishing, cleaning and drying: The surface of the oxide ceramic skeleton was polished smooth using sandpaper, then ultrasonically cleaned and dried to obtain a 3D NASICON-type oxide ceramic skeleton.

2. The use of a 3D NASICON type oxide ceramic framework according to claim 1, characterized in that In step 3, the surface of the oxide ceramic skeleton is polished smooth using 400-mesh sandpaper, then ultrasonically cleaned in isopropanol for 3 to 5 times, and then dried in an oven at 80°C to 100°C for 12 h to 24 h to obtain a 3D NASICON-type oxide ceramic skeleton.

3. The use of a 3D NASICON type oxide ceramic framework according to claim 1, characterized in that A 3D NASICON-type oxide ceramic skeleton is used as a solid electrolyte to assemble an all-solid-state lithium metal battery LFP|LATP PVA|Li in the following steps:

1. Preparation of ionic liquid electrolyte containing LiTFSI: Adding lithium bis(trifluoromethanesulfonyl imide) to 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl imide) salt to obtain an ionic liquid electrolyte containing LiTFSI; The concentration of lithium bis(trifluoromethanesulfonyl)imide in the ionic liquid electrolyte containing LiTFSI in step 1 is 0.4 mol / L to 0.45 mol / L; 2. Assemble the battery: Prepare a negative electrode shell, place a spring, place a gasket, place a 12mm lithium sheet, place a 3D NASICON-type oxide ceramic skeleton, add 25μL of ionic liquid electrolyte containing LiTFSI on both sides of the 3D NASICON-type oxide ceramic skeleton, then place 12mm lithium iron phosphate, then cover the positive electrode shell, and put it into a button battery packaging machine to complete the packaging.

4. The use of a 3D NASICON type oxide ceramic framework according to claim 1, characterized in that A 3D NASICON-type oxide ceramic skeleton is used as a solid electrolyte to assemble a lithium-ion symmetric battery Li|LATP PVA|Li, which is specifically completed in the following steps:

1. Preparation of ionic liquid electrolyte containing LiTFSI: Adding lithium bis(trifluoromethanesulfonyl imide) to 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl imide) salt to obtain an ionic liquid electrolyte containing LiTFSI; The concentration of lithium bis(trifluoromethanesulfonyl)imide in the ionic liquid electrolyte containing LiTFSI in step 1 is 0.4 mol / L to 0.45 mol / L; 2. Assemble the battery: Prepare a negative electrode shell, place a spring, place a gasket, place a 12 mm lithium sheet, place a 3D NASICON-type oxide ceramic skeleton, add 25 μL of ionic liquid electrolyte containing LiTFSI on both sides of the 3D NASICON-type oxide ceramic skeleton, then place a 12 mm lithium sheet, then cover the positive electrode shell, and put it into a button battery packaging machine to complete the packaging.