A pulse electroplating multi-layer electromagnetic shielding composite film and its preparation method
Multi-layer Ni-Fe alloy electromagnetic shielding films are formed on the surface of SiC/Al composite materials through pulse electroplating technology, which solves the problem of insufficient electromagnetic signal shielding capability of SiC/Al composite materials, achieves efficient electromagnetic shielding effects and simplifies the operation process.
Patent Information
- Application Number
- CN202410046253.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-11
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-01-11
AI Technical Summary
In the existing technology, SiC/Al composite materials have limited electromagnetic signal shielding capabilities, and it is difficult to effectively form multi-layer thin metal electromagnetic shielding films, and the processing process is difficult to control.
Pulse electroplating technology is used to form a multi-layer Ni-Fe alloy electromagnetic shielding film on the surface of SiC/Al composite materials. By adjusting the pulse cathode current density and action time, and cycling different current densities, a nickel-iron alloy pulse electroplating layer is formed, and the nickel-iron alloy pulse electroplating layer is formed in a vacuum drying oven. Heat treatment is performed to enhance the bonding strength of the coating.
It significantly improves the electromagnetic shielding capability of the device, simplifies the operating process, achieves efficient multi-layer coating combination, and avoids the problems of coating cracking and reduced electromagnetic shielding effectiveness.
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of electromagnetic shielding functional film preparation, and specifically to an electromagnetic shielding composite film with multiple chemical components and thickness control that can meet the needs of electromagnetic shielding, and a preparation method thereof. Background Art
[0002] Silicon carbide reinforced aluminum matrix (SiC / Al) composite material is one of the metal matrix composite materials with high specific strength and specific stiffness. It has a wide range of applications in aerospace, instrumentation and other fields, and is also one of the research hotspots in the international materials community. Since the surface of SiC / Al composite materials has multiple components and interfaces, its application in aerospace instrumentation and other fields involves a large number of surface functionalization treatments, such as insulation treatment and electromagnetic shielding treatment. Therefore, one of the key technologies urgently needed for the widespread application of this new type of metal matrix composite material is the problem of surface functionalization.
[0003] At present, although SiC / Al composite materials have high specific strength and high specific stiffness, it is found that the ability of a single SiC / Al composite material to shield electromagnetic signals is limited when used in certain devices. In order to enhance its ability to shield electromagnetic signals, setting a shielding film layer is a good application solution. However, in the prior art, the electromagnetic shielding film layer, on the one hand, is difficult to control the process of processing the multiphase surface and interface of the SiC / Al composite material; on the other hand, there is currently no mature control measure to form a multi-layer effective thin metal electromagnetic shielding film on the surface of the SiC / Al composite material.
[0004] Therefore, there is an urgent need for a multi-layer electromagnetic shielding composite film and a preparation method thereof which is different from the prior art. Summary of the invention
[0005] The purpose of the present application is to provide a pulse electroplating multi-layer electromagnetic shielding composite film and a preparation method thereof, so as to solve the deficiencies and shortcomings existing in the prior art.
[0006] The embodiments of the present application can be implemented through the following technical solutions:
[0007] A method for preparing a pulse electroplating multi-layer electromagnetic shielding composite film comprises the following steps:
[0008] S1: performing chemical nickel plating on the surface of the substrate to be treated to obtain a nickel-plated base layer;
[0009] S2: Electroplating Ni-Fe alloy on the nickel-plated base layer by pulse electroplating in an electroplating solution, and cyclically changing different pulse cathode current densities at least twice during the pulse electroplating process to obtain a pulse electroplated electromagnetic shielding film having at least two layers of Ni-Fe alloy pulse electroplated layers;
[0010] S3: plating a Ni layer on the outer side of the pulse electroplated electromagnetic shielding film to obtain a composite alloy with an outer plating layer;
[0011] S4: The composite alloy with the outer coating is cleaned, placed in a vacuum drying oven after cleaning, and vacuum heated and dried to complete the internal stress removal and hydrogen removal treatment.
[0012] Further, in step S2, the pulse cathode current density is 1.5A / dm 2 -3A / dm 2 Each action lasts 1-10 minutes.
[0013] Further, in step S2, the components of the electroplating solution are: nickel sulfate, ferrous sulfate, sodium citrate, sodium chloride, boric acid, sodium dodecyl sulfate, saccharin, 1,4-butynediol, sodium benzenesulfinate;
[0014] The mass ratio of the nickel sulfate to the ferrous sulfate is 4:1 or 10:1.
[0015] Furthermore, when the mass percentage of nickel sulfate: ferrous sulfate is 4:1, the pH value of the electroplating solution is 3-3.5, the temperature is 54-58°C, and the different pulse cathode current densities are replaced at least twice, the main component of the nickel-iron alloy pulse electroplating layer obtained is Ni 64 Fe 36 , the mass percentage of nickel to iron is approximately 7:3.
[0016] Furthermore, when the mass percentage of nickel sulfate: ferrous sulfate is 10:1, the pH value of the electroplating solution is 3-3.5, the temperature is 54-58°C, and the different pulse cathode current densities are replaced at least twice, the main component of the nickel-iron alloy pulse electroplating layer obtained is Ni 85 Fe 15 , the mass percentage of nickel to iron is approximately 17:3.
[0017] The present application also provides a pulse electroplated multi-layer electromagnetic shielding composite film, which is prepared by the above-mentioned pulse electroplated multi-layer electromagnetic shielding composite film preparation method, wherein the pulse electroplated multi-layer electromagnetic shielding composite film is provided with a nickel-plated base layer, a pulse electroplated electromagnetic shielding film having at least two layers of Ni-Fe alloy pulse electroplated layers, and an outer plating layer in sequence from the inside to the outside, wherein the Ni-Fe alloy pulse electroplated layer is one of the following:
[0018] The mass percentage of Ni and Fe is about 7:3, and the main component is Ni 64 Fe 36 ;
[0019] The mass percentage of Ni and Fe is about 17:3, and the main component is Ni 85 Fe 15.
[0020] Furthermore, the thickness of each Ni-Fe alloy pulse electroplated layer in the pulse electroplated electromagnetic shielding film is within 1 to 2 microns, and the number of Ni-Fe alloy pulse electroplated layers does not exceed 70 layers.
[0021] The pulse electroplating multi-layer electromagnetic shielding composite film preparation method provided in the embodiment of the present application has at least the following beneficial effects:
[0022] Compared with the prior art, the pulse electroplating electromagnetic shielding film layer prepared by the preparation method of the present application has an interlayer interface that can greatly improve the electromagnetic shielding capability of the device. During the implementation process, the pulse current density during the deposition of each layer of Ni-Fe alloy in the composite film layer is adjusted to form an alloy gradient coating, and pulse electroplating of multilayer electroplated films is targeted. After the multilayer film is formed, an appropriate heat treatment process is performed to enhance the bonding strength of the coating. DETAILED DESCRIPTION
[0023] Hereinafter, the present application will be further described based on preferred embodiments.
[0024] The iron content in the pulse electroplating electromagnetic shielding film layer and the control of the pulse current density and practice are key issues. By referring to the formula control of iron content in "Multi-band electromagnetic wave shielding composite film layer and its preparation method and application, Chinese invention patent, ZL202010251138.4". The difference of the present invention is that it adopts the pulse electroplating method to change the size and action time of the cathode current density to form a multi-layer Ni-Fe alloy pulse electroplating layer (nickel-iron alloy pulse electroplating layer) to improve the electromagnetic shielding characteristics.
[0025] On the one hand, the present application provides a method for preparing a pulse electroplating multi-layer electromagnetic shielding composite film, comprising the following steps:
[0026] S1: performing chemical nickel plating on the surface of the substrate to be treated to obtain a nickel-plated base layer;
[0027] S2: Electroplating Ni-Fe alloy on the nickel-plated base layer by pulse electroplating in an electroplating solution, and cyclically changing different pulse cathode current densities at least twice during the pulse electroplating process to obtain a pulse electroplated electromagnetic shielding film having at least two layers of Ni-Fe alloy pulse electroplated layers;
[0028] S3: plating a Ni layer on the outer side of the pulse electroplating electromagnetic shielding film to obtain a composite alloy with an outer plating layer;
[0029] S4: The composite alloy with the outer coating is cleaned, placed in a vacuum drying oven after cleaning, and vacuum heated and dried to complete the internal stress removal and hydrogen removal treatment.
[0030] Specifically, in step S1, since the aluminum in the SiC / Al composite material matrix is continuously distributed in a three-dimensional network, the chemical nickel plating process refers to the existing mature aluminum alloy secondary zinc immersion pretreatment on the market, and then the chemical nickel plating operation is performed. This process adopts mature technology to make the surface of the composite material uniform, which is beneficial to the subsequent functional electroplating of Ni-Fe multilayer alloy.
[0031] In some preferred embodiments, after the multiple gradient coatings are completed, in order to reduce the internal stress of the multi-layer coatings and strengthen the bonding strength of the coatings, high-temperature heat treatment is performed.
[0032] In some preferred embodiments, the chemically plated nickel layer covers the surface of the SiC / Al composite material uniformly, and generally the thickness reaches about 10 microns.
[0033] In some preferred embodiments, in step S2, the components of the electroplating solution are: nickel sulfate, ferrous sulfate, sodium citrate, sodium chloride, boric acid, sodium dodecyl sulfate, saccharin, 1,4-butynediol, sodium benzenesulfinate; when the mass percentage of nickel sulfate: ferrous sulfate is 4:1, the pH value of the electroplating solution is 3-3.5, the temperature is 54-58°C, and after cyclic replacement of at least two different pulse cathode current densities, the main component of the nickel-iron alloy pulse electroplating layer obtained is Ni 64 Fe 36 , the mass percentage of nickel and iron is about 7:3; when the mass percentage of nickel sulfate: ferrous sulfate is 10:1, the pH value of the electroplating solution is 3-3.5, the temperature is 54-58℃, and after changing the pulse cathode current density at least twice, the main component of the nickel-iron alloy pulse electroplating layer is Ni 85 Fe 15 , the mass percentage of nickel to iron is approximately 17:3.
[0034] By adjusting the electroplating pulse current, a pulse electroplating electromagnetic shielding film with multiple Ni-Fe alloy pulse electroplating layers can be obtained. In order to avoid the mismatch of thermal expansion coefficients between the plating layers caused by the subsequent heat treatment, which causes large stress in the plating layer and easy cracking, each plating layer is controlled within 1 to 2 microns; at the same time, taking into account the impact on electromagnetic shielding performance, each plating layer is controlled within 1 to 2 microns, and the number of layers is preferably 70, which can obtain high electromagnetic shielding performance, and the plating layer will not crack due to excessive stress. Therefore, the thickness of each layer of the pulse electroplating electromagnetic shielding film is preferably 1 micron.
[0035] In some preferred embodiments, a Ni layer is plated on the outside of the pulse electroplated electromagnetic shielding film to meet the needs of corrosion protection and smoothness. Ni plating is used to complete multi-layer coating. In order to meet different electromagnetic shielding requirements, the plating thickness is adjusted accordingly.
[0036] The final step is to place the surface treated samples or devices into a vacuum drying oven for vacuum drying, stress relief, and dehydrogenation treatment to enhance the bonding strength of the coating.
[0037] On the other hand, the present application also provides a pulse electroplated multilayer electromagnetic shielding composite film prepared by the above method, which is provided with a nickel-plated base layer, a pulse electroplated electromagnetic shielding film having at least two layers of Ni-Fe alloy pulse electroplated layers, and an outer plating layer from the inside to the outside, wherein the Ni-Fe alloy pulse electroplated layer is one of the following:
[0038] The mass percentage of Ni and Fe is about 7:3, and the main component is Ni 64 Fe 36 ;
[0039] The mass percentage of Ni and Fe is about 17:3, and the main component is Ni 85 Fe 15 .
[0040] In some preferred embodiments, the thickness of each Ni—Fe alloy pulse electroplated layer in the pulse electroplated electromagnetic shielding film is within 1 to 2 microns, and the number of Ni—Fe alloy pulse electroplated layers does not exceed 70 layers.
[0041] It should be noted that, although the prior art "Multi-band electromagnetic wave shielding composite film layer and its preparation method and application, Chinese invention patent, ZL202010251138.4" can form an electromagnetic shielding composite film with multiple layers of Ni-Fe alloy pulse electroplating layer by replacing different electroplating solutions, the Ni-Fe alloy pulse electroplating layer in the prior art can only continuously replace the electroplating tank to achieve the combination of different coatings, and the total thickness of the obtained electroplated shielding film cannot exceed 70 microns (to avoid nodules or cracks in the coating), and the operation is cumbersome. On the other hand, if the coating is too thick, defects are likely to occur, and the electromagnetic shielding effectiveness will be reduced. The present application can achieve the combination of multiple layers of coating by setting the pulse signal of the power supply, and the composition of each coating layer remains consistent, and the electromagnetic shielding effectiveness can be improved. In addition, the present application has very high requirements on the characteristics of the coating. It is not possible to obtain a pulse electroplated electromagnetic shielding film layer with high-efficiency shielding function by adjusting the pulse cathode current density and the electroplating time at will, in order to meet the needs of electromagnetic shielding effectiveness in specific frequency bands required by military application scenarios. The combination of multiple plating layers can be achieved by only using the power supply setting, and there is no need to adjust the plating composition, which simplifies the operation, that is, more interface layers can be achieved, and the electromagnetic shielding effect can be improved. This adjustment of the current density of the electroplating power supply makes the density of the metal deposition of the plating layer different between each layer, thereby obtaining a layered interface. This method simplifies the operation process and significantly improves the electromagnetic shielding effect.
[0042] The present invention will be further described below in conjunction with the embodiments, taking the SiC / Al composite material as an example.
[0043] Example 1
[0044] A method for preparing a pulse electroplating multi-layer electromagnetic shielding composite film comprises the following steps:
[0045] S1: After the multiphase surface of the SiC / Al composite material is uniformly metallized, a secondary zinc immersion pretreatment is performed, and then chemical nickel plating is performed to deposit a chemical nickel plating layer on the surface of the SiC / Al composite material as an electroplating primer conductive layer to obtain a nickel-plated primer layer.
[0046] S2: Electroplating Ni-Fe alloy on the nickel-plated base layer by pulse electroplating in the electroplating solution, wherein the mass percentage of nickel sulfate: ferrous sulfate in the electroplating solution is 4:1, the pH value of the electroplating solution is 3, the temperature is 54°C, and the pulse cathode current density is adjusted to 3A / dm 2 After 1 minute of action, the cathode current density was changed to 1.5A / dm 2 After 1 minute of action, the composition of the Ni-Fe alloy pulse electroplated layer is close to that of Ni 64 Fe 36 The mass percentage of nickel to iron is about 7:3, and the cycle is repeated 60 times to form 60 layers of Ni-Fe alloy pulse electroplating layers, and a pulse electroplated electromagnetic shielding film with a total thickness of about 50 microns is obtained.
[0047] In some preferred embodiments, the components in the electroplating solution are: 160 g / L nickel sulfate, 40 g / L ferrous sulfate, 30 g / L sodium citrate, 25 g / L sodium chloride, 40 g / L boric acid, 0.2 g / L sodium dodecyl sulfate, 3 g / L saccharin, 0.3-0.5 g / L 1,4-butynediol, and 0.3-0.5 g / L sodium benzenesulfinate.
[0048] S3: Plating a Ni layer on the outer side of the pulse electroplating electromagnetic shielding film to obtain a composite alloy with an outer plating layer.
[0049] S4: The composite alloy with the outer coating is cleaned, washed with warm water and then with cold water, and then placed in a vacuum drying oven at 400°C, and taken out after vacuum heating and drying for 2 hours to complete the internal stress removal and hydrogen removal treatment. In this embodiment, the coating distribution method is: SiC / Al composite material-chemical nickel plating-electroplating Ni Fe=7:3 (cyclically regulating the pulse current density to form a multi-layer distribution)-electroplating a thin layer of Ni for corrosion protection.
[0050] In some preferred embodiments, in order to avoid changes in the coating due to excessively high temperature in step S4, the composite alloy with the outer coating can also be cleaned, washed with warm water and then with cold water, and placed in a vacuum drying oven at 200°C after cleaning. The vacuum heating and drying is completed within 4 hours to complete the removal of internal stress and dehydrogenation treatment.
[0051] Example 2
[0052] The difference between this embodiment and embodiment 1 is that the pulse cathode current density of the cyclic replacement in step S2 is different.
[0053] Specifically, S2: electroplating Ni-Fe alloy on the nickel-plated base layer by pulse electroplating in an electroplating solution, wherein the mass percentage of nickel sulfate: ferrous sulfate in the electroplating solution is 4:1, the pH value of the electroplating solution is 3.5, the temperature is 58°C, and the pulse cathode current density is first adjusted to 2A / dm in the electroplating solution. 2 After 1 minute of action, the cathode current density was changed to 3A / dm 2 After 1 minute of action, the alloy pulse electroplating layer composition is close to Fe 64 Ni 36 The mass percentage of nickel to iron is about 7:3, and the cycle is repeated 60 times to form 60 layers of Ni-Fe alloy pulse electroplating layers, and a pulse electroplated electromagnetic shielding film with a total thickness of about 50 microns is obtained.
[0054] The other steps and parameters are the same as those in Example 1 and will not be further described here.
[0055] The pulse electroplated multilayer electromagnetic shielding composite film obtained in Example 1 has an electromagnetic shielding effectiveness of a maximum value of 35dB at a frequency of 300MHz, while the electromagnetic shielding effectiveness of Example 2 has a maximum value of 60dB at a frequency of 200MHz. The difference lies in that the electromagnetic shielding capabilities are different under the action of electromagnetic wave field strengths of different frequencies.
[0056] Example 3
[0057] The difference between this embodiment and embodiment 1 is the electroplating solution formula in step S2. The ratio of nickel sulfate to ferrous sulfate in the electroplating solution is adjusted to 10:1, and other components remain unchanged. After adjusting the solution composition, the composition of the Ni-Fe alloy pulse electroplating layer obtained is close to that of Ni 85 Fe 15 , the mass percentage of nickel to iron is about 17:3. In order to match the requirements of electromagnetic shielding performance, other steps and parameters are the same as those in Example 1, and finally 60 layers of Ni-Fe alloy pulse electroplating layers are formed to obtain a pulse electroplated electromagnetic shielding film with a total thickness of about 60 microns;
[0058] Example 1 The pulse electroplating multi-layer electromagnetic shielding composite film obtained in Example 1 reaches a maximum electromagnetic shielding effectiveness of 35dB at a frequency of 300MHz, while the electromagnetic shielding effectiveness of Example 3 reaches a maximum electromagnetic shielding effectiveness of 57dB at a frequency of 200MHz. The difference lies in that the electromagnetic shielding capabilities are different under the action of electromagnetic wave field strengths of different frequencies.
[0059] Example 4
[0060] The difference between this embodiment and embodiment 1 lies in the pulse plating action time in step S2.
[0061] Specifically, S2: Electroplating Ni-Fe alloy on the nickel-plated base layer by pulse electroplating in the electroplating solution, wherein the pH value of the electroplating solution is 3, the temperature is 54°C, and the pulse cathode current density is adjusted to 3A / dm 2 After 10 minutes of action, the pulse cathode current density was changed to 1.5A / dm 2 After 10 minutes of action, the composition of the Ni-Fe alloy pulse electroplated layer is close to that of Ni 64 Fe 36 The mass percentage of nickel and iron is about 7:3, and the cycle is repeated 6 times to form 6 layers of Ni-Fe alloy pulse electroplating layers to obtain a pulse electroplated electromagnetic shielding film with a total thickness of about 70 microns.
[0062] The other steps and parameters are the same as those in Example 1.
[0063] The pulse electroplated multilayer electromagnetic shielding composite film obtained in Example 1 has an electromagnetic shielding effectiveness of a maximum value of 35dB at a frequency of 300MHz, while the pulse electroplated multilayer electromagnetic shielding composite film with a total thickness of about 70 microns in Example 4 has an electromagnetic shielding effectiveness of a maximum value of 26dB at a frequency of 200MHz.
[0064] The above is a detailed introduction to the specific implementation methods of the present application. For those skilled in the art, several improvements and modifications may be made to the present application without departing from the principles of the present application. These improvements and modifications also fall within the scope of protection of the claims of the present application.
Claims
1. A method for preparing a pulse electroplating multi-layer electromagnetic shielding composite film, characterized in that: The steps include: S1: performing chemical nickel plating on the surface of the substrate to be treated to obtain a nickel-plated base layer; S2: Electroplating Ni-Fe alloy on the nickel-plated base layer by pulse electroplating in an electroplating solution, and cyclically changing different pulse cathode current densities at least twice during the pulse electroplating process to obtain a pulse electroplated electromagnetic shielding film having at least two layers of Ni-Fe alloy pulse electroplated layers; S3: plating a Ni layer on the outer side of the pulse electroplated electromagnetic shielding film to obtain a composite alloy with an outer plating layer; S4: cleaning the composite alloy with the outer coating, placing it in a vacuum drying oven after cleaning, and vacuum heating and drying to complete the internal stress removal and hydrogen removal treatment; In step S2, the pulse cathode current density is 1.5A / dm 2 -3A / dm 2 , each action lasts 1-10 minutes; In step S2, the components of the electroplating solution are: nickel sulfate, ferrous sulfate, sodium citrate, sodium chloride, boric acid, sodium dodecyl sulfate, saccharin, 1,4-butynediol, and sodium benzenesulfinate; The mass ratio of the nickel sulfate to the ferrous sulfate is 4:1 or 10:
1.
2. The method for preparing a pulse electroplating multi-layer electromagnetic shielding composite film according to claim 1, characterized in that: When the mass percentage of nickel sulfate and ferrous sulfate is 4:1, the pH value of the electroplating solution is 3-3.5, the temperature is 54-58°C, and the pulse cathode current density is changed at least twice, the main component of the nickel-iron alloy pulse electroplating layer is Ni 64 Fe 36 The mass percentage of nickel to iron is 7:
3.
3. The method for preparing a pulse electroplating multi-layer electromagnetic shielding composite film according to claim 1, characterized in that: When the mass percentage of nickel sulfate and ferrous sulfate is 10:1, the pH value of the electroplating solution is 3-3.5, the temperature is 54-58°C, and the different pulse cathode current densities are replaced at least twice, the main component of the nickel-iron alloy pulse electroplating layer is Ni 85 Fe 15 The mass percentage of nickel to iron is 17:
3.
4. A pulse electroplated multi-layer electromagnetic shielding composite film, characterized in that: The method for preparing a pulse electroplated multilayer electromagnetic shielding composite film according to any one of claims 1 to 3 is used, wherein the pulse electroplated multilayer electromagnetic shielding composite film is provided with a nickel-plated base layer, a pulse electroplated electromagnetic shielding film having at least two layers of Ni-Fe alloy pulse electroplated layers, and an outer plating layer in sequence from the inside to the outside, wherein the Ni-Fe alloy pulse electroplated layer is one of the following: The mass percentage of Ni and Fe is 7:3, and the main component is Ni 64 Fe 36 ; The mass percentage of Ni and Fe is 17:3, and the main component is Ni 85 Fe 15 .
5. The pulse electroplating multi-layer electromagnetic shielding composite film according to claim 4, characterized in that: The thickness of each Ni-Fe alloy pulse electroplated layer in the pulse electroplated electromagnetic shielding film is within 1 to 2 microns, and the number of Ni-Fe alloy pulse electroplated layers does not exceed 70 layers.
Citation Information
Patent Citations
Giant magneto-impedance (GMI) thin film material and preparation method thereof
CN102231423A
Preparation method of iron-nickel alloy magnetic layer on surface of stainless steel fiber
CN103866364A
Electroplating Fe-Ni alloy magnetic shielding material and preparation method thereof
CN103898574A
Single-pulse electrodeposition method for Ni-Fe alloy magnetic coatings
CN105780068A
Electroplating method of electromagnetic shielding material
CN108070888A
Cited By
Multi-layer flexible soft magnetic thin film with high magnetic conductivity and preparation method and application of multi-layer flexible soft magnetic thin film
CN122136125A