A formation method for lithium-ion batteries

By controlling the pressure, current, temperature, and SOC during the lithium-ion battery formation process, and employing a process of three charging cycles, one discharging cycle, and then a fourth charging cycle, the problem of incomplete lithium removal from the positive electrode lithium replenishment material was solved, thereby improving the battery's high-temperature storage and cycle performance.

CN117895112BActive Publication Date: 2026-11-17HUIZHOU LIWINON NEW ENERGY TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311837856.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-28
Publication Date
2026-11-17
Estimated Expiration
2043-12-28

AI Technical Summary

Technical Problem

In the existing lithium-ion battery formation process, the lithium removal of the positive electrode replenishment material is incomplete, which leads to the degradation of battery performance during high-temperature storage and cycle operation, and also causes gas generation problems.

Method used

The formation process employs three charging cycles, one discharging cycle, and a fourth charging cycle. By controlling the pressure, current, temperature, and SOC during the formation process, the lithium replenishment agent is completely delithiated during the formation stage. A dense SEI film is generated through low-current charging, reducing gas production.

Benefits of technology

It improves the high-temperature storage and cycle performance of lithium-ion batteries, reduces gas production during the formation stage, and enhances the high-temperature cycle and storage performance of the batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure BDA0004638084250000051
    Figure BDA0004638084250000051
  • Figure BDA0004638084250000101
    Figure BDA0004638084250000101
Patent Text Reader

Abstract

This invention belongs to the field of lithium-ion battery processing technology, specifically relating to a lithium-ion battery formation method. The invention employs a formation process of three charges, one discharge, and then a fourth charge; the third charge current > the first charge current > the second charge current. This combination improves the delithiation efficiency of the lithium-replenishing material during the formation stage, and releases oxygen from the lithium-replenishing agent during this stage, maximizing oxygen desorption and gas generation. This improves the battery's high-temperature cycling and high-temperature storage gas generation issues, enhancing its high-temperature cycling performance. Furthermore, this invention controls the delithiation efficiency by adjusting the pressure, current, temperature, and SOC during the formation charge and discharge process, ensuring complete delithiation of the lithium-replenishing agent on the positive electrode side at the delithiation plateau. In summary, the formation process steps of this invention are interconnected and mutually influential, collectively improving the delithiation and gas generation issues of the lithium-replenishing material and enhancing high-temperature storage and cycling performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of lithium-ion battery processing technology, and specifically relates to a method for the formation of lithium-ion batteries. Background Technology

[0002] Currently, combining cathode lithium supplementation with oxide-based materials (silicon oxide, tin oxide) and amorphous carbon anodes can improve battery energy density. This mainly involves adding a high-capacity, low-initial-efficiency cathode lithium supplementation material to compensate for lithium-ion consumption. This method effectively avoids safety risks and complex manufacturing processes. However, commonly used cathode lithium supplementation materials include metal oxides / nitrides, such as Li3N, Li5FeO4, Li2O, and Li6CoO4. These materials generate gas due to the decomposition of the lithium supplement, which can negatively impact subsequent battery performance.

[0003] Existing formation methods typically employ large charging currents and cutoff voltages to ensure both production efficiency and stable performance of dense SEI film-structured batteries. However, the large charging current and high cutoff voltage prevent the lithium additives in the initial cathode from being completely extracted during the formation stage, leading to a decline in subsequent cycle and storage gas generation performance. Summary of the Invention

[0004] The following is an overview of the subject matter described in detail herein. This overview is not intended to limit the scope of the claims.

[0005] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention proposes a formation method for lithium-ion batteries. The formation process steps of the present invention are interconnected and mutually influential, and can collectively improve the delithiation and gas generation of lithium-replenishing materials, thereby enhancing high-temperature storage and high-temperature cycling performance.

[0006] To achieve the above objectives, the present invention adopts the following technical solution:

[0007] This invention provides a method for forming a lithium-ion battery, wherein the positive electrode material of the lithium-ion battery includes an active material and a lithium replenishing agent, and the method includes the following steps:

[0008] S1. Under a pressure of 1.1 MPa to 1.6 MPa, the lithium-ion battery is injected with liquid and then formed.

[0009] S2. The lithium-ion battery is hot-pressed at 75℃~90℃;

[0010] S3. Charge at a constant current of 0.03C to 0.1C until 30% to 40% SOC;

[0011] S4. Charge at a constant current of 0.01C to 0.045C until 60% to 80% SOC;

[0012] S5. Charge at a constant current of 0.1C to 1.2C until 100% to 120% SOC;

[0013] S6. Perform constant current discharge to 0%~10% SOC;

[0014] S7. Charge at a constant current and constant voltage of 0.1C to 1.5C until 70% to 90% SOC;

[0015] Wherein, the current in step S5 is greater than the current in step S3, which is greater than the current in step S4.

[0016] From a technical perspective, this invention employs a formation process involving three charges, one discharge, and a fourth charge, with control over the current magnitude for each charge. Furthermore, this invention also controls factors such as pressure, current, temperature, and state of charge (SOC) during the formation and discharge process. The inventors discovered that these formation process steps are interconnected and influence each other, ultimately significantly impacting the delithiation and gas generation phenomena, high-temperature storage, and high-temperature cycling performance of the lithium-replenishing material. Specifically:

[0017] (1) In step S1 of the present invention, after the lithium-ion battery is injected with electrolyte, it is formed under a preset pressure of 1.1 MPa to 1.6 MPa. Under this pressure, the formation interface is better, and the gas generated during subsequent charging and discharging can be discharged into the gas bag in time, avoiding side reactions between the oxygen generated by the lithium replenishment agent and the electrolyte. Conversely, if the pressure is too high, the electrolyte will be squeezed out of the gas bag, resulting in insufficient wettability and severe lithium plating in the battery.

[0018] (2) In step S2 of the present invention, hot pressing at 75°C to 90°C is beneficial to battery shaping and prevents the battery from becoming soft in subsequent steps.

[0019] (3) In steps S3 to S5 of the present invention, the reason for first charging with a small current in S3, and then continuing to reduce the charging current in S4, followed by constant charging with a large current in S5 (i.e., the third charging current > the first charging current > the second charging current) is that: the small current formation is to generate a dense SEI film on the negative electrode side, and at the same time, the lithium replenishing agent has a better delithiation effect. Moreover, according to the characteristics of the lithium replenishing material, the lithium replenishing agent will release oxygen on both delithiation platforms, with more oxygen released on the second platform. Therefore, a smaller current (i.e., the second current density is less than the first current density) is used to allow the lithium replenishing material to release oxygen and reduce storage gas generation. In order to improve the delithiation efficiency, a larger current is used for the third charging, but it must be lower than 1.2C. Otherwise, the polarization will be too large, the SEI film density will be low, and it may even affect the delithiation efficiency in subsequent discharge and recharging. In steps S3 to S5 of the present invention, the charging SOC has the advantage of increasing gradually. It should be noted that the formation SOC in each charging stage should be controlled within a certain range. If it is lower than the protection range, the lithium replenishment agent will not completely delithiate, the battery will produce gas and affect the battery capacity.

[0020] (4) In step S6 of the present invention, further delithiation can be achieved by discharging to the range of 0% to 10% SOC.

[0021] (5) In step S7 of the present invention, the temperature is raised to 70°C to 90°C for charging in order to make the residual alkali on the surface of the lithium replenishing agent and the lithium replenishing agent delithiation reaction more complete; below this range, the delithiation effect of the material and the reaction of the residual alkali are insufficient.

[0022] In some embodiments of the present invention, in step S1, the pressure is 1.1 MPa to 1.6 MPa, including but not limited to: 1.1 MPa to 1.5 MPa, 1.1 MPa to 1.4 MPa, 1.1 MPa to 1.3 MPa, 1.1 MPa to 1.2 MPa, 1.2 MPa to 1.6 MPa, 1.2 MPa to 1.5 MPa, 1.2 MPa to 1.4 MPa, 1.2 MPa to 1.3 MPa, and 1.2 MPa.

[0023] In some embodiments of the present invention, in step S2, the temperature of the hot pressing is 75°C to 90°C, including but not limited to: 75°C to 85°C, 75°C to 80°C, 80°C to 90°C, 80°C to 85°C, and 80°C.

[0024] In some embodiments of the present invention, in step S2, the hot pressing time is 5 min to 20 min, including but not limited to: 5 min to 15 min, 5 min to 10 min, 10 min to 20 min, 10 min to 15 min, and 10 min.

[0025] In some embodiments of the present invention, in step S3, the current is 0.03C to 0.1C, including but not limited to: 0.05C to 0.1C, 0.04C to 0.06C, 0.08C to 0.1C, 0.05C, and 0.1C.

[0026] In some embodiments of the present invention, in step S3, the charge is brought to 30% to 40% SOC, including but not limited to: 35% to 40% SOC, 30% SOC, 35% SOC, and 40% SOC.

[0027] In some embodiments of the present invention, in step S3, the charging cutoff current is 0.01 to 0.03C, including but not limited to: 0.01 to 0.02C, 0.02 to 0.03C, and 0.02C.

[0028] In some embodiments of the present invention, in step S4, the current is 0.01C to 0.045C, including but not limited to: 0.02C to 0.045C, 0.01C to 0.03C, 0.04C to 0.045C, 0.02C, and 0.045C.

[0029] In some embodiments of the present invention, in step S4, the charge is brought to 60% to 80% SOC, including but not limited to: 60% to 75% SOC, 60% to 70% SOC, 60% to 65% SOC, 65% to 80% SOC, 65% to 75% SOC, 65% to 70% SOC, 70% to 80% SOC, 70% to 75% SOC, 75% to 80% SOC, 60% SOC, 65% SOC, 70% SOC, 75% SOC, and 80% SOC.

[0030] In some embodiments of the present invention, in step S5, the current is 0.1C to 1.2C, including but not limited to: 0.1C to 1.0C, 0.2C to 0.8C, 0.4C to 0.6C, and 0.5C.

[0031] In some embodiments of the present invention, in step S5, the charge is brought to 100% to 120% SOC, including but not limited to: 100% to 115% SOC, 100% to 110% SOC, 100% to 105% SOC, 105% to 120% SOC, 105% to 115% SOC, 105% to 110% SOC, 110% to 120% SOC, 110% to 115% SOC, 115% to 120% SOC, 100% SOC, 105% SOC, 110% SOC, 115% SOC, and 120% SOC.

[0032] In some embodiments of the present invention, in step S5, the charging cutoff current is 0.01 to 0.03C, including but not limited to: 0.01 to 0.02C, 0.02 to 0.03C, and 0.02C.

[0033] In some embodiments of the present invention, in step S5, the resting period after charging for 5 to 20 minutes includes, but is not limited to, 5 to 15 minutes, 5 to 10 minutes, 10 to 20 minutes, 10 to 15 minutes, and 10 minutes. The purpose of resting is to allow the battery to stabilize.

[0034] In some embodiments of the present invention, in step S6, a constant current discharge is performed at a current of 0.3–1.8C to 0%–10% SOC. The current range of 0.3–1.8C includes, but is not limited to: 0.3–1.5C, 0.3–1.0C, 1.0–1.8C, 1.2–1.8C, 1.5–1.8C, 0.5–1.8C, 0.3C, 0.5C, and 1.8C; the discharge to 0%–10% SOC includes, but is not limited to: 0%–5% SOC, 5%–10% SOC, 0% SOC, and 10% SOC.

[0035] In some embodiments of the present invention, steps S3, S4, S5, and S6 are performed at 45°C to 65°C, including but not limited to: 45°C to 60°C, 45°C to 55°C, 45°C to 50°C, 50°C to 65°C, 50°C to 60°C, 50°C to 55°C, and 50°C.

[0036] In some embodiments of the present invention, in step S7, the current is 0.1C to 1.5C, including but not limited to: 0.1C to 1.0C, 0.1C to 0.5C, 1.0C to 1.5C, 0.5C to 1.5C, 0.1C, 0.5C, and 1.5C.

[0037] In some embodiments of the present invention, in step S7, the charge is brought to 70% to 90% SOC, including but not limited to: 70% to 80% SOC, 80% to 90% SOC, 70% SOC, 80% SOC, and 90% SOC.

[0038] In some embodiments of the present invention, step S7 is performed at 70°C to 90°C, including but not limited to: 70°C to 80°C, 80°C to 90°C, 70°C, 80°C, and 90°C.

[0039] In some embodiments of the present invention, in step S7, the resting period after charging for 5 to 20 minutes includes, but is not limited to, 5 to 15 minutes, 5 to 10 minutes, 10 to 20 minutes, 10 to 15 minutes, and 10 minutes. The purpose of resting is to allow the battery to stabilize.

[0040] In some embodiments of the present invention, the outer surface of the active material is further provided with a coating layer.

[0041] In some embodiments of the present invention, the lithium replenishing agent is blended with the positive electrode active material. Because the surface of the positive electrode active material has a coating layer, the lithium in the lithium replenishing agent will be preferentially consumed during formation.

[0042] In some embodiments of the present invention, the thickness of the coating layer is 0.03 μm to 1 μm, preferably 0.05 μm to 0.1 μm. A thicker coating layer allows lithium to be preferentially extracted from the lithium replenishing agent during formation for lithium-ion consumption in the SEI, thereby increasing the reversible specific capacity of the positive electrode active material and improving battery performance.

[0043] In some embodiments of the present invention, the coating material may be selected from one or more of metal oxides, phosphates, silicates, solid electrolytes, etc., but is not limited thereto.

[0044] In some embodiments of the present invention, the current in step S4 and the thickness of the coating layer satisfy the following relationship:

[0045]

[0046] Where c represents the current in step S4, expressed in C; and d represents the thickness of the coating layer, expressed in μm.

[0047] In this invention, the coating thickness and the current in S4 need to satisfy a certain relationship, which can further improve the high-temperature cycling performance. This is because: the S4 charging stage is the stage when the positive electrode active material begins to delithiate. By adjusting the current in the S4 stage and the coating thickness of the positive electrode active material to satisfy the above relationship, the lithium in the lithium replenishment agent is preferentially removed during formation and used for the lithium ion consumption of SEI. The reversible specific capacity of the positive electrode active material is increased, thus improving the battery performance.

[0048] In some embodiments of the present invention, the lithium replenishing agent has a delithiation plateau ≥ 3V. Preferably, the lithium replenishing agent is selected from at least one of lithium-rich lithium iron ore and lithium-rich lithium nickel ore. The reason is that the present invention selects lithium-rich compounds as lithium replenishing agents, such as LFO and LNO. LFO / LNO materials have a significant delithiation plateau above 3.0V and high specific capacity. When matched with the formation steps and parameters of the present invention, delithiation is more complete, solving the gas generation problem while improving high-temperature cycling performance. Conversely, other lithium replenishing agents, such as Li3S, have a delithiation plateau of 2.5V. When using the formation steps of the present invention, delithiation is incomplete, resulting in a significant decrease in cycling performance.

[0049] In some embodiments of the present invention, the positive electrode active material of the lithium-ion battery is selected from at least one of lithium cobalt oxide, lithium-rich manganese-based materials, ternary materials, lithium manganese oxide, and lithium iron phosphate. Preferably, the positive electrode active material of the lithium-ion battery is lithium cobalt oxide.

[0050] In some embodiments of the present invention, the negative electrode active material of the lithium-ion battery is selected from at least one of graphite, silicon-carbon, and silicon-oxygen. Preferably, the negative electrode active material of the lithium-ion battery is silicon-carbon. More preferably, the negative electrode active material of the lithium-ion battery is 5% silicon-carbon.

[0051] In some preferred embodiments of the present invention, the lithium-ion battery adopts a lithium cobalt oxide-silicon carbon system in order to improve the battery energy density.

[0052] The lithium-ion battery formation method according to embodiments of the present invention has at least the following beneficial effects:

[0053] The formation process of the positive electrode lithium-ion battery provided by this invention specifically employs a formation process of three charges, one discharge, and then a fourth charge, with the third charge current > the first charge current > the second charge current. This combination improves the delithiation efficiency of the lithium-replenishing material during the formation stage and releases oxygen from the lithium-replenishing agent during this stage, maximizing oxygen desorption and gas generation. This improves the battery's high-temperature cycling and high-temperature storage gas generation issues, enhancing its high-temperature cycling performance. Furthermore, by controlling the pressure, current, temperature, and SOC during the formation charge and discharge process, the delithiation efficiency is controlled, ensuring complete delithiation of the lithium-replenishing agent on the positive electrode side at the delithiation plateau. The formation process steps of this invention are interconnected and mutually influential, collectively improving the delithiation and gas generation phenomenon of the lithium-replenishing material, and enhancing high-temperature storage and cycling performance.

[0054] In addition, compared with the prior art, the present invention uses low current charging, which makes the delithiation effect of the lithium replenishment agent better, and generates as much deoxygenation gas as possible during the formation stage, thereby improving the problem of gas generation in the later cycle and storage of the battery. Detailed Implementation

[0055] The following will describe the concept and technical effects of the present invention clearly and completely with reference to embodiments, so as to fully understand the purpose, features and effects of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are all within the scope of protection of the present invention.

[0056] Example

[0057] In this invention, unless otherwise specified, all equipment and raw materials are available from the market or commonly used in the industry. Unless otherwise specified, the methods in the following embodiments are conventional methods in the art.

[0058] In a specific embodiment of the present invention, the structure of the lithium-ion battery cell is prepared by the following method:

[0059] The positive electrode is a lithium-ion electrode, and the negative electrode is a silicon-carbon electrode. The separator is a JL 7μm oil-based separator. A bare cell is obtained using a fully automated winding method. The bare cell is then sealed with an aluminum-plastic film of a specific size. A certain amount of electrolyte is injected into the dried, semi-encapsulated cell, and the encapsulation is completed. Further processes such as settling, formation, shaping, and capacity testing are then performed to complete the fabrication of the lithium-ion pouch battery.

[0060] Example 1

[0061] This embodiment provides a method for the formation of a lithium-ion battery. The positive electrode material of the lithium-ion battery includes the active material lithium cobalt oxide and the lithium replenishing agent LFO. LFO is mixed with lithium cobalt oxide. The outer surface of the lithium cobalt oxide is provided with a coating layer with a thickness of 0.06 μm.

[0062] The formation method of lithium-ion batteries includes the following steps:

[0063] (1) Place the lithium-ion battery cell that has been filled with liquid and pre-sealed into the formation cabinet, adjust the temperature inside the cabinet, and apply a pressure of 1.2 MPa to the surface of the battery cell to start the segmented charging of the battery cell.

[0064] (2) The first stage involves hot pressing the battery at 80°C for 10 minutes.

[0065] (3) In the second stage, the formation cabinet is cooled to 50°C and charged to 40% SOC with a constant current and constant voltage of 0.05C. The cut-off current is 0.02C.

[0066] (4) In the third stage, the battery cell is charged at a constant current of 0.02C to 80% SOC;

[0067] (5) In the fourth stage, the battery cell is charged at a constant current of 0.5C to the predetermined voltage of 105% SOC, the cut-off current is 0.02C, and then left to stand for 10 minutes.

[0068] (6) In the fifth stage, the cell is discharged at a constant current of 0.5C until the voltage reaches 0% SOC;

[0069] (7) In the sixth stage, the formation cabinet is heated to 80°C, and the battery is charged at 0.5C constant current and constant voltage to 80% SOC, and then left to rest for 10 minutes.

[0070] Example 2

[0071] This embodiment provides a method for the formation of a lithium-ion battery, which is carried out with reference to Embodiment 1, except that: step (3) is charged to 35% SOC.

[0072] Example 3

[0073] This embodiment provides a method for the formation of a lithium-ion battery, which is carried out in accordance with the method in Embodiment 1, except that: in step (6), the battery is discharged to 10% SOC.

[0074] Example 4

[0075] This embodiment provides a method for the formation of a lithium-ion battery, which is carried out in accordance with Embodiment 1, except that: step (4) is to charge to 70% SOC.

[0076] Example 5

[0077] This embodiment provides a method for the formation of a lithium-ion battery, which is carried out with reference to Embodiment 1, except that: step (4) is to charge to 60% SOC.

[0078] Example 6

[0079] This embodiment provides a method for the formation of a lithium-ion battery, which is carried out with reference to Embodiment 1, except that: step (3) is charged to 30% SOC.

[0080] Example 7

[0081] This embodiment provides a method for the formation of a lithium-ion battery, which is carried out in accordance with Embodiment 1, except that: step (5) is to charge to 110% SOC.

[0082] Example 8

[0083] This embodiment provides a method for forming a lithium-ion battery, which is carried out with reference to Embodiment 1, except that the current in step (3) is 0.1C.

[0084] Example 9

[0085] This embodiment provides a method for forming a lithium-ion battery, which is carried out with reference to Embodiment 1, except that the current in step (6) is 1.8C.

[0086] Example 10

[0087] This embodiment provides a method for the formation of a lithium-ion battery, which is carried out with reference to Embodiment 1, except that the temperature of step (7) is 70°C.

[0088] Example 11

[0089] This embodiment provides a method for forming a lithium-ion battery, which is carried out with reference to Embodiment 1, except that the current in step (7) is 1.5C.

[0090] Example 12

[0091] This embodiment provides a lithium-ion battery formation method, which is carried out in accordance with Embodiment 1, except that the lithium replenishing agent is replaced with LNO.

[0092] Example 13

[0093] This embodiment provides a method for forming a lithium-ion battery, which is carried out with reference to Embodiment 1, except that the current in step (4) is 0.045C and the coating thickness is 0.1μm.

[0094] Comparative Example 1

[0095] This comparative example provides a method for forming a lithium-ion battery, which is carried out with reference to Example 1, except that the pressure in step (1) is 1.0 MPa.

[0096] Comparative Example 2

[0097] This comparative example provides a method for forming a lithium-ion battery, which is carried out with reference to Example 1, except that step (7) is omitted.

[0098] Comparative Example 3

[0099] This comparative example provides a method for forming a lithium-ion battery, which is carried out with reference to Example 1, except that steps (6) and (7) are omitted.

[0100] Comparative Example 4

[0101] This comparative example provides a method for the formation of a lithium-ion battery, which is carried out with reference to Example 1, except that the temperature of step (2) is 45°C.

[0102] Comparative Example 5

[0103] This comparative example provides a method for forming a lithium-ion battery, which is carried out with reference to Example 1, except that: step (3) is charged to 20% SOC.

[0104] Comparative Example 6

[0105] This comparative example provides a method for forming a lithium-ion battery, which is carried out with reference to Example 1, except that the current in step (3) is 0.15C.

[0106] Comparative Example 7

[0107] This comparative example provides a method for forming a lithium-ion battery, which is carried out with reference to Example 1, except that: step (4) is to charge to 50% SOC.

[0108] Comparative Example 8

[0109] This comparative example provides a method for forming a lithium-ion battery, which is carried out in accordance with Example 1, except that the current in step (4) is 0.05C, which does not satisfy the following relationship:

[0110]

[0111] Where c represents the current in step S4, expressed in C; and d represents the thickness of the coating layer, expressed in μm.

[0112] Comparative Example 9

[0113] This comparative example provides a method for forming a lithium-ion battery, which is carried out with reference to Example 1, except that the temperature of step (7) is 60°C.

[0114] Comparative Example 10

[0115] This comparative example provides a method for forming a lithium-ion battery, which is carried out with reference to Example 1, except that the current in step (7) is 2C.

[0116] Comparative Example 11

[0117] This comparative example provides a method for forming a lithium-ion battery, which is carried out with reference to Example 1, except that: in step (6), the battery is discharged to 12%.

[0118] Comparative Example 12

[0119] This comparative example provides a method for the formation of a lithium-ion battery, which is carried out with reference to Example 1, except that the lithium replenishing agent is Li2S.

[0120] Comparative Example 13

[0121] This comparative example provides a method for forming a lithium-ion battery, which is carried out with reference to Example 1, except that the current in step (5) is 1.3C.

[0122] Comparative Example 14

[0123] This comparative example provides a method for forming a lithium-ion battery, which is carried out with reference to Example 1, except that step (4) is omitted.

[0124] Comparative Example 15

[0125] This comparative example provides a method for the formation of a lithium-ion battery, which is carried out with reference to Example 1, except that: step (7) is omitted and steps (4) to (6) are repeated 4 times.

[0126] Comparative Example 16

[0127] This comparative example provides a method for forming a lithium-ion battery, which is carried out with reference to Example 1, except that the thickness of the coating layer is 0.05 μm, which does not satisfy the relational formula.

[0128] Comparative Example 17

[0129] This comparative example provides a method for forming a lithium-ion battery, which is carried out with reference to Example 13, except that the thickness of the coating layer is 0.06 μm, which does not satisfy the relational formula.

[0130] Test case

[0131] Formation gas production test: The gas production of the battery is measured by the difference in the volume of water drained when the battery is submerged in water, ΔV = V2 - V1.

[0132] High-temperature storage test: After capacity grading, the battery was charged to 4.48V at room temperature using a constant current and constant voltage of 0.5C (cutoff current is 0.02C), and the initial discharge capacity of the battery was measured. Then, after storing at 85℃ for 6 hours, the battery was discharged to 3.0V at 0.5C, and the retention capacity and recovery capacity of the battery were measured.

[0133] Cyclic test: At room temperature (25±2℃) or high temperature (45℃±2℃), charge the battery after capacity testing to 4.48V using a constant current and constant voltage of 0.5C (cutoff current is 0.01C), and then discharge it to 3.0V using a constant current of 0.5C.

[0134] The test results are shown in Table 1 below.

[0135] Table 1

[0136]

[0137]

[0138] The test results from Examples 1-13 show that: The optimized formation process using the technical solution of this invention ensures complete delithiation of the lithium supplement LFO during the formation stage, which is beneficial for gas generation during the formation process and improves the battery's high-temperature cycle performance and high-temperature storage performance. However, when the formation pressure, charging current, SOC, and temperature exceed the specified range, the delithiation effect of the lithium supplement material is poor. During performance testing, the lithium supplement material releases oxygen, which reacts with the electrolyte, causing gas generation in the battery and affecting storage and cycle performance. The formation process steps of this invention are interconnected and mutually influential. Steps exceeding the scope of this solution or lacking a particular step significantly impact gas generation or high-temperature cycling performance.

[0139] Specifically:

[0140] As can be seen from Example 1 and Comparative Example 1, the pressure range throughout the entire formation process needs to be above 1.1 MPa. If it is below 1.1 MPa, or if some steps are not above 1.1 MPa, especially during the three charging processes, the gas generated during formation will not be able to be discharged into the gas bag in time, affecting the formation interface and deteriorating the high-temperature cycling performance.

[0141] As can be seen from Examples 1 and 8, and Comparative Examples 6 / 8 / 13, the three charging currents must satisfy the condition that the third charging current > the first charging current > the second charging current, and the three charging currents must satisfy the condition that the first charging current is 0.03C to 0.1C, the second charging current is 0.01C to 0.045C, and the third charging current is 0.1C to 1.2C. When the charging current is higher, the lithium removal effect becomes worse, which also affects the lithium removal efficiency during subsequent discharge and the fourth charging, as well as the residual alkali reaction on the surface of the lithium replenishing agent.

[0142] As can be seen from Examples 1, 10, 11 and Comparative Examples 2 / 3 / 9 / 10, the fourth charge after discharge is performed to ensure that the residual alkali on the surface of the lithium replenishing agent and the lithium replenishing agent delithiation reaction are more complete. If there is no fourth charge, the temperature or charging current is not within the range, which will affect the delithiation effect of the material and the reaction of the residual alkali will be insufficient.

[0143] As can be seen from Example 1 and Comparative Example 13, the third charge uses a larger current, but it must be lower than 1.2C. Otherwise, the polarization will be large, the SEI film density will be low, and it will affect the subsequent discharge and the delithiation efficiency in the fourth charge.

[0144] As can be seen from Examples 1, 10, 11 and Comparative Example 9 / 10, the temperature and current of the fourth charge affect the residual alkali on the surface of the lithium replenishing agent and the delithiation effect. When the current or temperature of the fourth charge is not within the range, the thermal expansion rate of the thermal thickness and the high-temperature cycling performance at 85°C deteriorate significantly.

[0145] As can be seen from Example 1 and Comparative Examples 2 / 3 / 14, the formation pressure and charging / discharging steps are interconnected and coordinated. Removing any step in the formation process of this scheme will significantly worsen the formation gas production and high-temperature cycling.

[0146] Examples 1 / 12 and Comparative Example 12 show that the lithium-rich compound LFO / LNO material has a significant delithiation plateau above 3.0V and high specific capacity. When matched with the above-mentioned formation process, delithiation is more complete, which can solve the gas generation problem and improve high-temperature cycling performance. The delithiation plateau of Li3S is around 2.5V. When using the formation process of this scheme, delithiation and oxygen release by the lithium replenishment agent are incomplete, resulting in a significant decrease in cycle performance.

[0147] As can be seen from Example 1 and Comparative Example 15, without the fourth charging step of this scheme, the gas production and high-temperature storage performance will decrease if the S4-S6 charging and discharging steps are continuously cycled. Moreover, due to the multiple charging and discharging, the cycle performance will decrease significantly. Comparative Example 15 has a long formation time and complicated steps. Repeated charging and discharging cannot completely solve the problems of gas production and high-temperature cycle.

[0148] As shown in Examples 1 / 13 and Comparative Examples 8 / 16 / 17, when the coating thickness satisfies the relationship, the high-temperature cycling performance is improved. This is because the S4 charging stage is the stage where lithium cobalt oxide begins to delithigate. By adjusting the current in the S4 stage and the coating thickness of the positive electrode active material to satisfy the above relationship, lithium in the lithium replenishment agent is preferentially extracted during formation and used for lithium ion consumption in the SEI. This improves the reversible specific capacity of the positive electrode active material and enhances battery performance.

[0149] In summary, Examples 1-13 and Comparative Examples 1-17, which use LCO & LFO combined with silicon-carbon composite materials, were compared and analyzed. Table 1 shows that the optimized formation process using the technical solution of this invention ensures complete delithiation of the lithium supplement LFO during the formation stage, which is beneficial for gas generation during the formation process and can improve the battery's high-temperature cycle performance and high-temperature storage performance. When the formation pressure, charging current, SOC, and temperature exceed the specified range, the delithiation effect of the lithium supplement material is poor. During performance testing, the lithium supplement material releases oxygen, which reacts with the electrolyte, causing gas generation in the battery and affecting storage and high-temperature cycle performance.

[0150] The above description provides a detailed account of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Within the scope of knowledge possessed by those skilled in the art, various changes can be made without departing from the spirit of the present invention. Furthermore, unless otherwise specified, the embodiments of the present invention and the features thereof can be combined with each other.

Claims

1. A method of forming a lithium ion battery, characterized by, The positive electrode material of the lithium-ion battery includes an active material and a lithium replenishing agent, and the formation method includes the following steps: S1. Under a pressure of 1.1 MPa to 1.6 MPa, the lithium-ion battery is injected with liquid and then formed. S2. The lithium-ion battery is hot-pressed at 75℃~90℃; S3. Charge at a constant current of 0.03C~0.1C until 30%~40% SOC; S4. Charge at a constant current of 0.01C~0.045C to 60%~80% SOC; S5. Charge at a constant current of 0.1C~1.2C to 100%~120% SOC; S6. Perform constant current discharge to 0%~10% SOC; S7. Charge at a constant current and constant voltage of 0.1C~1.5C to 70%~90% SOC. Wherein, the current in step S5 is greater than the current in step S3, which is greater than the current in step S4; Step S7 is performed at 70℃~90℃; The outer surface of the active material is further provided with a coating layer, the thickness of which is 0.03μm~1μm.

2. The formation method according to claim 1, characterized in that, In step S2, the hot pressing time is 5 min to 20 min.

3. The formation method according to claim 1, characterized in that, In step S5, the charging cutoff current is 0.01C~0.03C.

4. The formation method according to claim 1, characterized in that, In step S5, the charging process involves allowing the device to stand for 5 to 20 minutes.

5. The formation method according to claim 1, characterized in that, In step S6, a constant current discharge is performed with a current of 0.3C to 1.8C.

6. The formation method according to claim 1, characterized in that, Steps S3, S4, S5, and S6 are performed at 45℃~65℃.

7. The formation method according to claim 1, characterized in that, In step S7, the charging is followed by a resting period of 5 to 20 minutes.

8. The formation method according to claim 1, characterized in that, The current in step S4 and the thickness of the coating layer satisfy the following relationship: Where c represents the current in step S4, expressed in C; and d represents the thickness of the coating layer, expressed in μm.

9. The formation method according to claim 1, characterized in that, The delithiation plateau of the lithium replenishing agent is ≥3V.

10. The formation method according to claim 1, characterized in that, The lithium supplement is selected from at least one of lithium iron ferrite rich in lithium and lithium nickel ferrite rich in lithium.

11. The formation method according to claim 1, characterized in that, The positive electrode active material of the lithium-ion battery is selected from at least one of lithium cobalt oxide, lithium-rich manganese-based materials, ternary materials, lithium manganese oxide, and lithium iron phosphate.

12. The formation method according to claim 1, characterized in that, The negative electrode active material of the lithium-ion battery is selected from at least one of graphite, silicon-carbon, and silicon-oxygen.

Citation Information

Patent Citations

  • Positive electrode lithium supplement agent, lithium ion battery and positive electrode pre-lithiation formation method thereof

    CN115954453A

  • Formation method of total battery containing positive electrode lithium supplement agent, lithium ion battery and application

    CN116706285A