A method for preparing microwave foamed silicone rubber foam and composite material thereof

Through the microwave foaming method, the silicone rubber substrate and water are cross-linked in the microwave reaction, which solves the problems of complex preparation process and uneven pore size distribution of existing silicone rubber foam materials, achieving environmentally friendly, low-cost and efficient preparation with excellent The mechanical properties and small pore size of silicone rubber foam materials.

CN117903485BActive Publication Date: 2024-10-22UNIV OF SCI & TECH OF CHINA
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410072779.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-18
Publication Date
2024-10-22
Estimated Expiration
2044-01-18

AI Technical Summary

Technical Problem

The existing silicone rubber foam materials have complex preparation processes, high costs, large environmental pollution, and uneven pore size distribution, which limits the further development of the materials.

Method used

Using the microwave foaming method, the silicone rubber base material, cross-linking agent and functional nanomaterials are mixed with water, and a rapid and uniform thermal reaction is achieved through microwave reaction to prepare porous silicone rubber foam materials with uniform pore sizes.

Benefits of technology

It achieves process simplification, environmental protection, and low-cost preparation of silicone rubber foam materials. It has excellent mechanical properties and can quickly and controllably prepare small-pore silicone rubber foam materials, which is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117903485B_ABST
    Figure CN117903485B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a microwave-foamed silicone rubber foam and a composite material thereof, and belongs to the technical field of functional polymer composite material preparation. A silicone rubber substrate, a vinyl silicone rubber substrate, a crosslinking agent, polyhydrogen silane, a functional nanomaterial and water are fully mixed, and a crosslinking reaction occurs under microwave conditions to obtain a porous silicone rubber material. The entire material preparation process is simple, green and environmentally friendly, time-saving and efficient, overcoming the disadvantages of the current porous silicone rubber preparation field of cumbersome steps and the use of other harmful pore-forming agents, and is suitable for large-scale industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a green, simple and controllable microwave foaming method for preparing a porous silicone rubber foam material, belonging to the technical field of silicone rubber materials. Background Art

[0002] Silicone rubber foam material is a polymer elastic material with a loose porous structure prepared by silicone rubber material through foaming technology. It is widely used in mechanics, optics, electricity and other fields. Silicone rubber foam material itself has the physical and chemical properties of silicone rubber such as high and low temperature resistance, oil resistance, good biocompatibility, and has the advantages of low density, good elasticity and good air permeability of porous materials. It is a polymer material widely used in society. At present, the existing silicone rubber foaming process mainly revolves around solid solution foaming, microsphere filling foaming, supercritical gas foaming, irradiation vulcanization high temperature foaming, etc. Its preparation process has high requirements, many reaction steps, uneven pore size distribution, and large environmental pollution. The disadvantages limit the further development of silicone rubber foam materials. At present, it is of great significance to develop a green, fast, controllable, and uniformly distributed pore size silicone rubber foam preparation technology and its composite materials.

[0003] Microwave heating technology has the characteristics of uniform spatial radiation and significant thermal effect. It can quickly and evenly generate heat energy inside the reactants, and is expected to achieve rapid and uniform spatial thermal reaction, promote the preparation process to break through the limitations of traditional processing, and prepare new materials. In addition, water has a good wave absorption effect under microwave conditions and can respond quickly to generate heat energy. It is an environmentally friendly, healthy, and low-cost foaming template. The required post-processing method is simple and easy to implement, and porous silicone rubber foam materials can be prepared quickly and conveniently. The preparation of rubber foam material composites mainly revolves around the two-step interface modification functional composite materials, which have high process requirements and cumbersome steps. Therefore, it is of great significance to develop a convenient, fast, simple, controllable, low-cost, and repeatable one-step process to prepare porous silicone rubber material composites. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing silicone rubber foam and its composite materials with simple process, mild reaction conditions, and environmental protection and greenness, so as to overcome the shortcomings of the current silicone rubber foam material production process, high technical difficulty, high cost, and the use of foaming agents that are harmful to the environment. The microwave reaction method of the invention and the presence of water can effectively reduce the curing time of the silicone rubber foam, and prepare silicone rubber foam materials with smaller pore sizes. Not only does the preparation method have the economic benefits of energy saving, emission reduction, low carbon and environmental protection, but the prepared elastomeric material also has excellent mechanical properties.

[0005] To achieve the above object, the present invention adopts the following technical scheme: a method for preparing microwave foamed silicone rubber foam and its composite material, the preparation method comprising the following steps:

[0006] (1) mixing a silicone rubber substrate, a vinyl silicone rubber substrate, a crosslinking agent, polyhydrogen silane, and a functional nanomaterial to obtain a mixture A; the mass ratio of the vinyl silicone rubber substrate, polyhydrogen silane, and the functional nanomaterial used in step (1) is: 100 parts of the vinyl silicone rubber substrate, 1-20 parts of the polyhydrogen silane, and 0-20 parts of the functional nanomaterial;

[0007] (2) Mixture A and water are stirred in a mixer to obtain mixture B; the mass ratio of water used in step (2) to mixture A is 1-500:1;

[0008] (3) placing the mixture B in step (2) into a microwave reactor for microwave curing and foaming to obtain a silicone rubber foam material C;

[0009] (4) Drying the silicone rubber foam material C in step (3) to obtain microwave-foamed silicone rubber foam and its composite material D.

[0010] Preferably, the functional nanomaterial described in step (1) is one or more of graphene, carbon nanotubes, silver powder, graphene oxide, titanium oxide, zinc oxide, silicon dioxide, ferrous oxide, vanadium pentoxide, molybdenum disulfide, boron nitride, carbon nitride, copper iodide, calcium carbonate, barium carbonate, barium titanate, barium sulfate, polyvinylidene fluoride, cellulose, styrene-butadiene rubber, and montmorillonite.

[0011] Preferably, the weight proportions of the vinyl silicone rubber substrate, polyhydrogen silane and functional nanomaterial in step (1) are: 100 parts of vinyl silicone rubber substrate, 10 parts of polyhydrogen silane and 10 parts of functional nanomaterial.

[0012] Preferably, the mixing in step (1) is uniform, the stirring speed is 100-3000 rpm, and the time is 0.1-360 minutes.

[0013] Preferably, the mass ratio of the water used in step (2) to the mixture A is 200:1.

[0014] Preferably, in step (2), the stirring speed of the stirrer is 100-3000 rpm, and the stirring time is 0.1-360 minutes.

[0015] Preferably, in step (3), the microwave curing frequency is 1-100 GHz, and the curing time is 0.1-60 minutes.

[0016] Preferably, the drying method in step (4) is drying in an oven at a temperature of 40-100° C. for 1-24 hours, or vacuum freeze drying for 1-24 hours.

[0017] Preferably, the preparation method comprises the following steps:

[0018] (1) mixing a vinyl silicone rubber substrate, polyhydrogen silane, and boron nitride in the following weight proportions: 100 parts of the vinyl silicone rubber substrate, 10 parts of the polyhydrogen silane, and 10 parts of the boron nitride for 30 minutes to obtain a mixture A;

[0019] (2) stirring the obtained mixture A and 200 parts of water in a blender at 1000 rpm for 120 minutes to obtain a mixture B;

[0020] (3) Pour the mixture B into a mold, put it into a microwave reactor, and perform microwave curing and foaming at a microwave frequency of 2.45 GHz for 2 minutes to obtain a silicone rubber foam material C;

[0021] (4) Dry the silicone rubber foam material C in an oven at 60° C. for 12 hours to obtain microwave foamed silicone rubber foam and its composite material D.

[0022] Preferably, the preparation method comprises the following steps:

[0023] (1) mixing a vinyl silicone rubber substrate, polyhydrogen silane, and graphene in the following weight proportions: 100 parts of the vinyl silicone rubber substrate, 10 parts of the polyhydrogen silane, and 10 parts of the graphene for 30 minutes to obtain a mixture A;

[0024] (2) stirring the obtained mixture A and 200 parts of water in a blender at 1000 rpm for 120 minutes to obtain a mixture B;

[0025] (3) Pour the mixture B into a mold, put it into a microwave reactor, and perform microwave curing and foaming at a microwave frequency of 5 GHz for 0.5 minutes to obtain a silicone rubber foam material C;

[0026] (4) Dry the silicone rubber foam material C in an oven at 60° C. for 12 hours to obtain microwave foamed silicone rubber foam and its composite material D.

[0027] In step (3), mixture B can be poured into a mold or three-dimensionally printed.

[0028] Beneficial effects:

[0029] 1. The present invention uses water as the foaming template, which is green, environmentally friendly, low-priced, and has extremely high resource advantages and cost advantages.

[0030] 2. The preparation process of the silicone rubber foam material proposed in the present invention is simple, the conditions are mild and controllable, the production cost is low, the repeatability is high, and it is easy to industrialize production.

[0031] 3. The silicone rubber foam material synthesized by the present invention has a three-dimensional porous structure and controllable pore size.

[0032] 4. The present invention can rapidly prepare various silicone rubber foam material composites in one step.

[0033] 5. The present invention discloses a method for preparing a microwave foamed silicone rubber foam material. The silicone rubber substrate, vinyl silicone rubber substrate, crosslinking agent polyhydrogen silane, functional nanomaterials and water are fully mixed, and a crosslinking reaction occurs under microwave conditions to obtain a porous silicone rubber material. The entire material preparation process is simple, green and environmentally friendly, time-saving and efficient, overcoming the disadvantages of the current porous silicone rubber preparation field of cumbersome steps and the use of other harmful pore-forming agents, and is suitable for large-scale industrial production.

[0034] 6. As can be seen from Table 1, the curing time required for step 3 of Examples 1-4 and the pore size of the prepared silicone rubber foam material are significantly better than those of the comparative example, indicating that the microwave reaction method and the presence of water can effectively reduce the curing time of the silicone rubber foam and prepare a silicone rubber foam material with a smaller pore size. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is a scanning electron microscope image of the microwave-foamed silicone rubber foam material prepared in Example 3.

[0036] Figure 2 This is the infrared spectrum of the microwave foamed silicone rubber foam material prepared in Example 3.

[0037] Figure 3 This is a diagram of the mechanical properties of the microwave-foamed silicone rubber foam material prepared in Example 3. DETAILED DESCRIPTION

[0038] The embodiments of the present invention are described in further detail below:

[0039] A method for preparing a microwave foamed silicone rubber foam material and a composite thereof. After a silicone rubber matrix material, a crosslinking agent, a functional nanomaterial and water are mixed and microwave-treated, a sample having a honeycomb porous silicone rubber structure can be formed. The porous material preparation process is simple, the process is fast and efficient, the foaming template is environmentally friendly, the source is wide, and green production can be achieved, and it is applied to the low-carbon and environmentally friendly preparation of silicone rubber foam materials.

[0040] The specific steps include:

[0041] 1. The silicone rubber substrate, vinyl silicone rubber substrate, crosslinking agent polyhydrogen silane, and functional nanomaterials are uniformly mixed in a blender at a speed of 100-3000 rpm for 0.1-360 minutes to obtain a mixture A;

[0042] 2. Stirring the obtained mixture A and 1-500 parts of water in a blender at a speed of 100-3000 rpm for 0.1-360 minutes to obtain a mixture B;

[0043] 3. Pour the mixture B into a mold or three-dimensionally print it into a microwave reactor, and perform microwave curing and foaming for 0.1-30 minutes at a microwave frequency of 1-10 GHz to obtain a silicone rubber foam material C;

[0044] 4. Dry the silicone rubber foam material C in an oven at 40-100° C. for 1-24 hours, or freeze-dry it in a vacuum for 1-24 hours to obtain D.

[0045] Example 1

[0046] 1. The vinyl silicone rubber substrate, polyhydrogen silane and graphene were uniformly mixed in a blender at a speed of 1000 rpm for 30 minutes in the following weight proportions: 100 parts of the vinyl silicone rubber substrate, 10 parts of the polyhydrogen silane and 10 parts of the graphene, to obtain a mixture A;

[0047] 2. Mixture A and 200 parts of water were stirred in a blender at 1000 rpm for 120 minutes to obtain mixture B;

[0048] 3. Pour the mixture B into a mold, put it into a microwave reactor, and perform microwave curing and foaming for 2 minutes at a microwave frequency of 2.45 GHz to obtain a silicone rubber foam material C;

[0049] 4. Dry the silicone rubber foam material C in an oven at 60°C for 10 hours to obtain microwave foamed silicone rubber foam and its composite material D.

[0050] Example 2

[0051] 1. The vinyl silicone rubber substrate, polyhydrogen silane and graphene were uniformly mixed in a blender at a speed of 1000 rpm for 30 minutes in the following weight proportions: 100 parts of the vinyl silicone rubber substrate, 10 parts of the polyhydrogen silane and 0 parts of the graphene, to obtain a mixture A;

[0052] 2. Mixture A and 200 parts of water were stirred in a blender at 1000 rpm for 120 minutes to obtain mixture B;

[0053] 3. Pour the mixture B into a mold, put it into a microwave reactor, and perform microwave curing and foaming for 2 minutes at a microwave frequency of 2.45 GHz to obtain a silicone rubber foam material C;

[0054] 4. Dry the silicone rubber foam material C in an oven at 60°C for 12 hours to obtain a microwave-foamed silicone rubber foam material D.

[0055] Summary: Compared with Example 1, this Example 2 does not add graphene, which has no effect on the curing time required for step 3 and the pore size of the silicone rubber foam material prepared in step 4, indicating that doping with functional nanomaterials has no effect on the preparation of silicone rubber foam materials.

[0056] Example 3

[0057] 1. The vinyl silicone rubber substrate, polyhydrogen silane and boron nitride were uniformly mixed in a mixer at a speed of 1000 rpm for 30 minutes in the following mass proportions: 100 parts of vinyl silicone rubber substrate, 10 parts of polyhydrogen silane and 10 parts of boron nitride to obtain a mixture A;

[0058] 2. Mixture A and 200 parts of water were stirred in a blender at 1000 rpm for 120 minutes to obtain mixture B;

[0059] 3. Pour the mixture B into a mold, put it into a microwave reactor, and perform microwave curing and foaming for 2 minutes at a microwave frequency of 2.45 GHz to obtain a silicone rubber foam material C;

[0060] 4. Dry the silicone rubber foam material C in an oven at 60°C for 12 hours to obtain a microwave-foamed silicone rubber foam material D.

[0061] By the attached Figure 1 It can be seen from the scanning electron microscope image that the silicone rubber foam material prepared in Example 3 has a three-dimensional honeycomb morphology structure with uniform pore size and a relatively small pore size (5-10 μm), and the functional nanomaterial boron nitride is uniformly loaded on the surface.

[0062] By the attached Figure 2 It can be seen from the Fourier infrared spectrum that the sample of Example 3 has a wavelength of 1060-1012 cm -1 and 791cm -1 The peaks at 2160 cm-1 are attributed to Si-O and Si-C bonds, proving that the main structure of silicone rubber foam is a molecular network structure containing Si-O and Si-C. -1 There is no Si-H peak, which proves that the silicone rubber substrate and the cross-linking agent are completely cured.

[0063] By the attached Figure 3It can be seen from the mechanical properties diagram that the silicone rubber foam material of Example 3 has a wide deformation range (0-90%), and at a deformation of 90%, the stress is 105N, and has good flexibility.

[0064] Summary: Compared with Example 1, in Example 3, the graphene in step 1 is replaced by boron nitride, which has no obvious effect on the curing time required for step 3 and the pore size of the silicone rubber foam material prepared in step 4, but only changes the doped functional material of the silicone rubber foam material obtained in step 4, which is expected to achieve functional changes in the silicone rubber foam material, indicating that doping with functional nanomaterials has no effect on the preparation process of the silicone rubber foam material, but only affects the type of functional material loaded.

[0065] Example 4

[0066] 1. The vinyl silicone rubber substrate, polyhydrogen silane and graphene were uniformly mixed in a blender at a speed of 1000 rpm for 30 minutes in the following weight proportions: 100 parts of the vinyl silicone rubber substrate, 10 parts of the polyhydrogen silane and 10 parts of the graphene, to obtain a mixture A;

[0067] 2. Mixture A and 200 parts of water were stirred in a blender at 1000 rpm for 120 minutes to obtain mixture B;

[0068] 3. Pour the mixture B into a mold, put it into a microwave reactor, and perform microwave curing and foaming for 0.5 minutes at a microwave frequency of 5 GHz to obtain a silicone rubber foam material C;

[0069] 4. Dry the silicone rubber foam material C in an oven at 60°C for 12 hours to obtain a microwave-foamed silicone rubber foam material D.

[0070] Summary: Compared with Example 1, in Example 4, the microwave frequency of 2.45 GHz in Step 3 of Example 1 is replaced by a microwave frequency of 5 GHz, which will shorten the curing time required for Step 3 from 2 minutes to 0.5 minutes, and the pore size of the silicone rubber foam material obtained in Step 4 is increased from 5 microns to 4 microns.

[0071] Example 5

[0072] 1. The vinyl silicone rubber substrate, polyhydrogen silane and graphene were uniformly mixed in a blender at a speed of 1000 rpm for 30 minutes in the following weight proportions: 100 parts of the vinyl silicone rubber substrate, 10 parts of the polyhydrogen silane and 10 parts of the graphene, to obtain a mixture A;

[0073] 2. Mixture A and 50 parts of water were stirred in a blender at 1000 rpm for 120 minutes to obtain mixture B;

[0074] 3. Pour the mixture B into a mold, put it into a microwave reactor, and perform microwave curing and foaming for 50 minutes at a microwave frequency of 2.45 GHz to obtain a silicone rubber foam material C;

[0075] 4. Dry the silicone rubber foam material C in an oven at 60°C for 12 hours to obtain a microwave-foamed silicone rubber foam material D.

[0076] Summary: In Example 5, compared with Example 1, 200 parts of water in Step 2 of Example 1 are replaced by 50 parts of water, which will increase the curing time required for Step 3 to 50 minutes, and the pore size of the silicone rubber foam material obtained in Step 4 increases from 5 microns to 200 microns.

[0077] In order to compare and illustrate the advantages of the above five embodiments, comparative examples are listed below, in which the raw materials selected are partially the same, partially different, or a few raw materials are missing, and the preparation methods selected are partially the same, partially different, or a few methods are missing.

[0078] Comparative Example 1

[0079] 1. The vinyl silicone rubber substrate, polyhydrogen silane and graphene were uniformly mixed in a blender at a speed of 1000 rpm for 30 minutes in the following weight proportions: 100 parts of the vinyl silicone rubber substrate, 10 parts of the polyhydrogen silane and 10 parts of the graphene, to obtain a mixture A;

[0080] 2. Mixture A and 0 parts of water were stirred in a blender at 1000 rpm for 120 minutes to obtain mixture B;

[0081] 3. Pour the mixture B into a mold, put it into a microwave reactor, and perform microwave curing and foaming for 90 minutes at a microwave frequency of 2.45 GHz to obtain a silicone rubber foam material C;

[0082] 4. Dry the silicone rubber foam material C in an oven at 60°C for 12 hours to obtain D.

[0083] Summary: Compared with Example 1, this Comparative Example 1 replaces 200 parts of water in Step 2 of Example 1 with 0 parts of water, which will cause the curing time required for Step 3 to increase from 2 minutes to 90 minutes, and the silicone rubber foam material obtained in Step 4 does not show porous structural characteristics, but presents a solid internal structure, indicating that the water in Step 2 not only helps to shorten the curing time of Step 3, but also serves as the source of the porous structure.

[0084] Comparative Example 2

[0085] 1. The vinyl silicone rubber substrate, polyhydrogen silane and graphene were uniformly mixed in a blender at a speed of 1000 rpm for 30 minutes in the following weight proportions: 100 parts of the vinyl silicone rubber substrate, 10 parts of the polyhydrogen silane and 10 parts of the graphene, to obtain a mixture A;

[0086] 2. Mixture A and 200 parts of water were stirred in a blender at 1000 rpm for 120 minutes to obtain mixture B;

[0087] 3. Pour the mixture B into the mold, and set the oven at 60°C for high temperature curing and foaming for 60 minutes to obtain the silicone rubber foam material C;

[0088] 4. Dry the silicone rubber foam material C in an oven at 60°C for 12 hours to obtain D.

[0089] Summary: Compared with Example 1, in Comparative Example 2, replacing the microwave reactor in step 3 of Example 1 with an oven will increase the curing time required for step 3 from 2 minutes to 60 minutes, and the pore size of the silicone rubber foam material obtained in step 4 increases from 5 microns to 20 microns. This indicates that the microwave reaction in step 3 helps to shorten the curing time of step 3 and can prepare silicone rubber foam materials with smaller pore sizes.

[0090] Comparative Example 3

[0091] 1. The vinyl silicone rubber substrate, polyhydrogen silane and graphene were uniformly mixed in a blender at a speed of 1000 rpm for 30 minutes in the following weight proportions: 100 parts of the vinyl silicone rubber substrate, 10 parts of the polyhydrogen silane and 10 parts of the graphene, to obtain a mixture A;

[0092] 2. Mixture A and 200 parts of sugar cubes were stirred in a blender at 1000 rpm for 120 minutes to obtain mixture B;

[0093] 3. Pour the mixture B into a mold, put it into a microwave reactor, and perform microwave curing and foaming for 90 minutes at a microwave frequency of 2.45 GHz to obtain a silicone rubber foam material C;

[0094] 4. Dry the silicone rubber foam material C in an oven at 60°C for 12 hours to obtain D.

[0095] Summary: Compared with Example 1, in Comparative Example 3, replacing the water in Step 2 of Example 1 with sugar cubes will increase the curing time required for Step 3 from 2 minutes to 90 minutes, and the pore size of the silicone rubber foam material obtained in Step 4 increases from 5 microns to 100 microns, indicating that the water in Step 2 is beneficial to the preparation of silicone rubber foam materials with small pores and to shortening the preparation time.

[0096] Comparative Example 4

[0097] 1. The vinyl silicone rubber substrate, polyhydrogen silane and graphene were uniformly mixed in a blender at a speed of 1000 rpm for 30 minutes in the following weight proportions: 100 parts of the vinyl silicone rubber substrate, 10 parts of the polyhydrogen silane and 10 parts of the graphene, to obtain a mixture A;

[0098] 2. Mixture A and 200 parts of sugar cubes were stirred in a blender at 1000 rpm for 120 minutes to obtain mixture B;

[0099] 3. Pour the mixture B into the mold, and set the oven at 60°C for high temperature curing and foaming for 60 minutes to obtain the silicone rubber foam material C;

[0100] 4. Dry the silicone rubber foam material C in an oven at 60°C for 12 hours to obtain D.

[0101] Summary: Compared with Example 1, in Comparative Example 4, the water in step 2 of Example 1 is replaced with sugar cubes, and the microwave reactor in step 3 is replaced with an oven, which will cause the curing time required for step 3 to increase from 2 minutes to 60 minutes, and the pore size of the silicone rubber foam material obtained in step 4 to increase from 5 microns to 100 microns, indicating that the water in step 2 is beneficial to small size, and the microwave reaction in step 3 helps to shorten the required curing time.

[0102] Comparative Example 5

[0103] 1. The vinyl silicone rubber substrate, polyhydrogen silane and graphene were uniformly mixed in a blender at a speed of 1000 rpm for 30 minutes in the following weight proportions: 100 parts of the vinyl silicone rubber substrate, 10 parts of the polyhydrogen silane and 10 parts of the graphene, to obtain a mixture A;

[0104] 2. The obtained mixture A and 200 parts of NaCl particles were stirred in a mixer at 1000 rpm for 120 minutes to obtain a mixture B;

[0105] 3. Pour the mixture B into the mold, and set the oven at 60°C for high temperature curing and foaming for 60 minutes to obtain the silicone rubber foam material C;

[0106] 4. Dry the silicone rubber foam material C in an oven at 60°C for 12 hours to obtain D.

[0107] Summary: Compared with Example 1, this Comparative Example 5 replaces the water in Step 2 of Example 1 with salt, and replaces the microwave reactor in Step 3 with an oven, which will cause the curing time required for Step 3 to increase from 2 minutes to 60 minutes, and the pore size of the silicone rubber foam material obtained in Step 4 to increase from 5 microns to 200 microns, indicating that the water in Step 2 is beneficial to the preparation of small-size pores of silicone rubber foam materials, and the microwave reaction in Step 3 helps to shorten the required curing time.

[0108] Table 1

[0109] Evaluation Project Silicone rubber foam material pore size Step 3 Curing Time Required Composite material types Example 1 5 microns 2 minutes Graphene Example 2 5 microns 2 minutes none Example 3 5 microns 2 minutes Boron Nitride Example 4 4 microns 0.5 minutes Graphene Example 5 100 microns 50 minutes Graphene Comparative Example 1 No holes 90 minutes Graphene Comparative Example 2 20 microns 60 minutes Graphene Comparative Example 3 100 microns 90 minutes Graphene Comparative Example 4 100 microns 60 minutes Graphene Comparative Example 5 200 microns 60 minutes Graphene

[0110] It can be seen from Table 1 that the curing time required for step 3 of Examples 1-4 and the pore size of the prepared silicone rubber foam material are significantly better than those of the comparative example, indicating that the microwave reaction method and the presence of water can effectively reduce the curing time of the silicone rubber foam and prepare a silicone rubber foam material with a smaller pore size.

[0111] The specific implementation methods described above provide a detailed description of the technical solutions and beneficial effects of the present invention. It should be understood that the above is only the most preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, supplements and equivalent substitutions made within the scope of the principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing microwave foamed silicone rubber foam, characterized in that: The preparation method comprises the following steps: (1) A vinyl silicone rubber substrate, polyhydrogen silane, and graphene were uniformly mixed in a blender at a speed of 1000 rpm for 30 minutes in the following weight ratios: 100 parts of the vinyl silicone rubber substrate, 10 parts of the polyhydrogen silane, and 10 parts of the graphene, to obtain a mixture A; (2) stirring the obtained mixture A and 200 parts of water in a blender at 1000 rpm for 120 minutes to obtain a mixture B; (3) Pour the mixture B into a mold, put it into a microwave reactor, and perform microwave curing and foaming at a microwave frequency of 5 GHz for 0.5 minutes to obtain a silicone rubber foam material C; (4) Dry the silicone rubber foam material C in an oven at 60°C for 12 hours to obtain microwave-foamed silicone rubber foam D.

Citation Information

Patent Citations

  • Small pore diameter silicone rubber sponge and preparation method thereof

    CN104530712A

  • Method for preparing porous polymer block by water template method and prepared porous polymer

    CN116396526A

  • Method for the preparation of foamed and cured silicone rubber body

    US5041466A