A method for preparing a thin film semiconductor chip and a structure for preparing a thin film semiconductor chip

By using composite metal substrate structure and corrosive liquid etching technology in the preparation of thin film semiconductor chips, the problem of chip damage caused by temporary bonding is solved, thin film and high yield are achieved, and the requirements for chip processing and thin film are met.

CN117913017BActive Publication Date: 2024-10-22DR TECH CO LTD YIXING JIANGSU
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410081501.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-19
Publication Date
2024-10-22
Estimated Expiration
2044-01-19

AI Technical Summary

Technical Problem

In the existing technology, thin film semiconductor chips are prone to secondary damage during the temporary bonding and debonding process, resulting in abnormal chip quality and loss of yield. Moreover, the thickness of the metal substrate is difficult to control, and cannot meet the requirements of chip processing and thin film production at the same time. Require.

Method used

A composite metal substrate structure is used, including a thin film metal layer, a cutoff layer and a second temporary substrate. The sacrificial layer and cutoff layer are corroded by the corrosive liquid, the semiconductor chip epitaxial wafer is peeled off, and the second temporary substrate and cutoff are removed after chip processing. layer to achieve thin film.

Benefits of technology

It improves the yield rate of thin film semiconductor chips, meets the support requirements for chip processing, and achieves thin film processing. The process is simple and easy to implement, and secondary damage in the bonding process is avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117913017B_ABST
    Figure CN117913017B_ABST
Patent Text Reader

Abstract

The present application discloses a method for preparing a thin-film semiconductor chip and a corresponding preparation structure. The method comprises: epitaxially growing a semiconductor chip epitaxial wafer on a first temporary substrate; preparing a composite metal substrate on the semiconductor chip epitaxial wafer; corroding a sacrificial layer with a first etching liquid to peel off the semiconductor chip epitaxial wafer from the first temporary substrate; using the composite metal substrate as a support, performing subsequent chip processing on the semiconductor chip epitaxial wafer; and removing the second temporary substrate to obtain a thin-film semiconductor chip. According to the thin-film semiconductor chip preparation method and the corresponding preparation structure of the present application, a composite metal substrate is provided, and the composite metal substrate comprises a thin-film metal layer, a cut-off layer and a second temporary substrate. Therefore, during the chip processing, the composite metal substrate has sufficient thickness and supporting capacity. After the chip processing is completed, the second temporary substrate can be removed to meet the requirements of chip thin filmization; the process is simple and easy to implement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of semiconductor technology, and specifically relates to a thin film semiconductor chip preparation technology. Background Art

[0002] With the development of semiconductor technology, high power-to-weight ratio, thin film, and flexible semiconductor chips have received more and more attention and have become a field that urgently needs to be focused on and a direction of technological development. Thin film semiconductor chips, such as thin film photodetector chips, LED chips, solar cell chips, etc., can be realized in micron or nanometer sizes. Due to their small thickness, weak mechanical strength of the material, and easy warping, chip processing usually needs to be carried out on a hard substrate with a certain strength.

[0003] For this reason, during the semiconductor chip preparation process, it is necessary to temporarily bond the semiconductor chip epitaxial wafer to a hard support substrate, such as a silicon wafer and a sapphire wafer, and then carry out the subsequent chip production process. After completing all processing techniques, the bonding layer and the hard substrate are removed. However, the thin film chip is connected to the support substrate by temporary bonding, and then the chip is produced. Because it is a temporary bonding support substrate structure, there are many restrictions on the chip process, such as high temperature resistance, corrosion resistance, etc.; in addition, the thin film chip will be accompanied by secondary damage to the thin film chip during the temporary bonding and debonding process, resulting in irreversible material defects in the thin film chip, resulting in abnormal quality parameters of the thin film chip and loss of yield.

[0004] In the prior art, metal substrates are also used as thin film support substrates, but the thickness of the metal substrate is not easy to control. If it is too thin, it will not play a supporting role and will be unfavorable for subsequent chip manufacturing; if it is too thick, it will not meet the requirements of chip thin film. Summary of the invention

[0005] In view of the above-mentioned defects of the prior art, one of the objectives of the present application is to provide a thin-film semiconductor chip preparation process and structure that can simultaneously meet the chip processing requirements and the thin film requirements.

[0006] Another object of the present application is to avoid damage to the chip caused by a temporary bonding process.

[0007] In one aspect, the present application provides a method for preparing a thin film semiconductor chip, comprising:

[0008] epitaxially growing a semiconductor chip epitaxial wafer on a first temporary substrate, the semiconductor chip epitaxial wafer comprising a sacrificial layer adjacent to the temporary substrate;

[0009] Preparing a composite metal substrate on a side of the semiconductor chip epitaxial wafer opposite to the first temporary substrate, the composite metal substrate comprising a thin film metal layer, a stop layer and a second temporary substrate in order from one side of the semiconductor chip epitaxial wafer;

[0010] The sacrificial layer is corroded by a first corrosive solution to peel off the semiconductor chip epitaxial wafer from the first temporary substrate;

[0011] Using the composite metal substrate as a support, performing subsequent chip processing on a side of the semiconductor chip epitaxial wafer opposite to the composite metal substrate; and

[0012] The second temporary substrate and the cut-off layer are removed to obtain a thin film semiconductor chip.

[0013] According to one embodiment of the present application, preparing a composite metal substrate on a side of a semiconductor chip epitaxial wafer opposite to a first temporary substrate includes:

[0014] A thin film metal layer, a cut-off layer and a temporary metal substrate layer are sequentially deposited on a semiconductor chip epitaxial wafer using an evaporation process or a liquid phase deposition process.

[0015] According to one embodiment of the present application, removing the second temporary substrate and the stop layer includes:

[0016] The stop layer is etched by the second etching solution to peel the thin film semiconductor chip from the second temporary substrate.

[0017] According to one embodiment of the present application, the thin film semiconductor chip manufacturing method further includes: before etching the stop layer with a second etching solution, vertically dividing the semiconductor chip to the upper surface of the stop layer or the upper surface of the second temporary substrate.

[0018] According to one embodiment of the present application, removing the second temporary substrate and the stop layer includes:

[0019] The second temporary substrate is removed by grinding, and then the stop layer is etched by a second etching solution.

[0020] According to one embodiment of the present application, the thickness of the thin film metal layer is 10-100 um.

[0021] According to an embodiment of the present application, the cutoff layer is a metal layer, and the second temporary substrate is a metal substrate.

[0022] According to one embodiment of the present application, the thin film semiconductor chip is a light emitting diode device, a photovoltaic cell device or a photodetector.

[0023] Another aspect of the present application provides a thin film semiconductor chip preparation structure, which sequentially comprises:

[0024] A semiconductor chip epitaxial wafer on a first temporary substrate, wherein a sacrificial layer is provided between the semiconductor chip epitaxial wafer and the temporary substrate, wherein the sacrificial layer is subsequently used to peel off the semiconductor chip and the first temporary substrate; and

[0025] A composite metal substrate on a semiconductor chip epitaxial wafer, wherein the composite metal substrate comprises a thin film metal layer, a cutoff layer and a second temporary substrate in sequence from one side of the semiconductor chip epitaxial wafer, wherein the cutoff layer is subsequently used to peel off the semiconductor chip and the second temporary substrate.

[0026] According to one embodiment of the present application, the thickness of the thin film metal layer is 10-100 um.

[0027] According to the thin-film semiconductor chip preparation method and the corresponding preparation structure of the present application, a composite metal substrate is set up, and the composite metal substrate includes a thin-film metal layer, a cut-off layer and a second temporary substrate. Therefore, during the chip processing, the composite metal substrate has sufficient thickness and supporting capacity to meet the support requirements of chip processing; on the other hand, after the chip processing is completed, the second temporary substrate and the cut-off layer are removed to meet the requirements of chip thin film; therefore, the thin-film semiconductor chip preparation method and the corresponding preparation structure of the present application can simultaneously meet the chip processing requirements and the requirements of thin film, and the process is simple and easy to implement.

[0028] In addition, the thin-film semiconductor chip preparation method and corresponding preparation structure of the present application avoid the secondary damage to the thin-film chip caused by the temporary bonding and debonding process of connecting the semiconductor epitaxial wafer and the supporting substrate using a bonding process, thereby improving the yield rate of the thin-film semiconductor chip. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 is a flow chart of a method for preparing a thin film semiconductor chip according to an embodiment of the present application;

[0030] Figure 2 Yes Complete Figure 1 A schematic cross-sectional view of the thin film semiconductor chip preparation structure after step S2;

[0031] Figure 3 Yes Complete Figure 1 A schematic cross-sectional view of the thin film semiconductor chip preparation structure after step S4;

[0032] Figure 4 Yes Complete Figure 1 A schematic cross-sectional view of the thin film semiconductor chip preparation structure after step S5;

[0033] Figure 5 is a schematic diagram showing a fabrication structure of a thin film semiconductor chip according to an exemplary embodiment of the present application;

[0034] Figure 6 It is prepared Figure 5 Schematic diagram of the structure of a thin-film semiconductor chip. DETAILED DESCRIPTION

[0035] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the exemplary embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the accompanying drawings, components with the same or similar functions are indicated by the same or similar reference numerals. In addition, some components that are not directly related to the concept of the present invention may be omitted from the illustration. The description of the drawings and specific embodiments is only for a better understanding of the present invention, and the present invention is not limited to the embodiments illustrated in the drawings and described in the specification.

[0036] The technical terms or scientific terms used in the present invention should be the common meanings understood by people with ordinary skills in the field to which the present invention belongs. The use of "including" or "comprising" and similar words in the present invention indicates an open meaning, and does not exclude other elements, components, parts or items except for the elements, parts, parts or items clearly listed. "Connect" or "connected" and similar words are not limited to physical or mechanical connections, but may include electrical connections, whether direct or indirect. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly. "First", "second" and the like are used to distinguish different components and do not indicate a specific order.

[0037] See also Figure 1 -4. A method for preparing a thin film semiconductor chip according to an embodiment of the present application comprises the following steps:

[0038] Step S1: epitaxially grow a semiconductor chip epitaxial wafer on a first temporary substrate 200, wherein the semiconductor chip epitaxial wafer includes a semiconductor functional layer 204 and a sacrificial layer 202 adjacent to the first temporary substrate 200; wherein the sacrificial layer is subsequently used to peel off the semiconductor chip and the first temporary substrate 200. The first temporary substrate 200 may be a GaAs substrate, a silicon substrate, etc. The semiconductor chip may be a light-emitting diode device, a photovoltaic cell device, or a photodetector, etc. Accordingly, the semiconductor functional layer 204 may include a light-emitting diode functional layer, a photovoltaic cell functional layer, or a photodetector functional layer, etc. In some embodiments, the semiconductor chip epitaxial wafer may also include a buffer layer, an ohmic contact layer, and other structures as needed, which are omitted from illustration.

[0039] Next, in step S2, a composite metal substrate is prepared on the semiconductor chip epitaxial wafer, and the composite metal substrate sequentially includes a thin film metal layer 102, a cut-off layer 101 and a second temporary substrate 100; wherein the cut-off layer 101 is subsequently used to peel off the semiconductor chip and the second temporary substrate 100. Here, the thickness of the thin film metal layer 102 may be 10-100um, the thickness of the cut-off layer 101 may be 10-50um, and the thickness of the second temporary substrate 100 may be 150-450um. The cut-off layer 101 may be selected as a metal material or other materials, and the second temporary substrate 100 may be selected as a metal material. According to some embodiments of the present application, preparing a composite metal substrate on a semiconductor chip epitaxial wafer includes: sequentially depositing a thin film metal layer, a cut-off layer and a temporary metal substrate layer on the semiconductor chip epitaxial wafer by an evaporation process or a liquid phase deposition process.

[0040] After completing steps S1-S2, the thin film semiconductor chip preparation structure is as follows Figure 2 shown.

[0041] Next, in step S3, the sacrificial layer 202 is cleaned by etching with a first etching solution, and the semiconductor chip epitaxial wafer is peeled off from the first temporary substrate 200; here, the first etching solution can be selected to have a selective etching solution for the sacrificial layer 202 and the semiconductor chip epitaxial wafer, that is, the first etching solution can corrode the sacrificial layer but not the semiconductor chip epitaxial wafer. Alternatively, other processes can be used to remove the sacrificial layer 202 and the first temporary substrate 200 to obtain a semiconductor chip epitaxial wafer containing only a composite metal substrate.

[0042] Next, in step S4, the semiconductor chip preparation structure peeled off from the first temporary substrate 200 is flipped over, and the composite metal substrate is used as a support, and subsequent chip processing is performed on the side of the semiconductor chip epitaxial wafer opposite to the composite metal substrate, so as to prepare various required structures on the semiconductor epitaxial wafer according to the specific type of semiconductor chip. For example, an electrode 206, an anti-reflection film 205, etc. are prepared on the semiconductor functional layer 204, such as Figure 3 shown.

[0043] Next, in step S5, the second temporary substrate 100 is removed to obtain a thin film semiconductor chip. Specifically, in some embodiments, removing the second temporary substrate 100 includes: cleaning the stop layer 101 by etching with a second etching solution, and peeling the thin film semiconductor chip from the second temporary substrate 100. Here, the second etching solution can be selected to have a selective etching solution for the stop layer 101 and the flexible metal layer 102, that is, the second etching solution can corrode the stop layer 101, but does not corrode the flexible metal layer 102.

[0044] According to this embodiment, optionally, before the stop layer 101 is etched by the second etching liquid, the semiconductor chip layer is pre-vertically divided until the upper surface of the stop layer 101 or the upper surface of the second temporary substrate 100. For example, the boundary area between the single chips in the semiconductor chip layer can be etched by a photolithography process, and the chip part above the upper surface of the stop layer 101 or the upper surface of the second temporary substrate 100 is pre-separated into separate chip units. After that, the stop layer 101 is cleaned by etching with the second etching liquid, and the thin film semiconductor chip is peeled off from the second temporary substrate 100. The advantage of this is that the etching liquid can corrode the stop layer within the range of the entire semiconductor chip layer, rather than only corroding from the side, which is conducive to uniformly and efficiently corroding the stop layer, so that the thickness of the semiconductor chip is uniform; and after the stop layer 101 is cleaned by etching with the second etching liquid, the chip is formed into a separate single chip, and there is no need to perform chip separation.

[0045] In another embodiment, grinding combined with etching and cleaning can be used to remove the second temporary substrate 100 and the cut-off layer 101 to obtain a thin film semiconductor chip, that is, the second temporary substrate 100 is removed by grinding, and then the cut-off layer 101 is corroded by the second etching solution. The grinding process itself has the characteristic of uneven thickness of the grinding plane, and the thickness fluctuates within a certain error range. In this embodiment, the cut-off layer 101 is first ground to the cut-off layer, and the cut-off layer plane has an uneven thickness. Then, the thin cut-off layer is cleaned with a solution, and a thin film semiconductor chip with consistent specifications can be obtained. Compared with directly grinding to the flexible metal layer, the process of grinding combined with etching and cleaning can avoid the uneven thickness of the flexible substrate caused by directly grinding to the flexible metal layer; compared with the solution of etching and cleaning alone, the work of processing the reactants after etching and cleaning alone can be avoided. In addition, grinding combined with etching and cleaning is used to remove the second temporary substrate 100 and the cut-off layer 101, and the semiconductor chip layer can be divided before or after removing the second temporary substrate 100, which is more flexible in process.

[0046] After step S5, the obtained thin film semiconductor chip structure is as follows Figure 4 shown.

[0047] As described above, the present application sets up a composite metal substrate, which includes a thin film metal layer, a cut-off layer, and a second temporary substrate. Therefore, during the chip processing, the composite metal substrate has sufficient thickness and support capacity to meet the support requirements of chip processing; on the other hand, after the chip processing is completed, the second temporary substrate is removed to meet the requirements of chip thin filmization. Therefore, the thin film semiconductor chip preparation method and the corresponding preparation structure of the present application can simultaneously meet the chip processing requirements and the requirements of thin filmization.

[0048] In addition, the method for preparing a thin-film semiconductor chip and the corresponding preparation structure of the present application use processes such as evaporation coating, liquid-phase deposition, grinding, and / or etching solution cleaning to prepare a thin-film semiconductor chip, which has high process compatibility, simple processes, and is easy to implement throughout the entire process of chip production. It avoids the secondary damage of the thin-film chip during the temporary bonding and debonding processes caused by using the bonding process to connect the semiconductor epitaxial wafer and the support substrate, and improves the yield rate of the thin-film semiconductor chip.

[0049] The following will illustrate the preparation process of the thin-film semiconductor chip of the present invention with specific examples.

[0050] See Figure 5 -6. In a specific embodiment, the preparation process of the thin-film semiconductor chip of the present invention is as follows:

[0051] First, prepare a flip-chip semiconductor chip, which specifically includes:

[0052] 1. Using gallium arsenide as a temporary substrate, grow a GaAs buffer layer, a first sacrificial layer / etching barrier layer for peeling, an epitaxial functional layer 104, and an ohmic contact layer 103 on the GaAs substrate by metalorganic chemical vapor deposition (MOCVD) or molecular beam epitaxy (MBE).

[0053] The GaAs substrate is an N-type conductive substrate. The sacrificial layer of the peeling substrate is selected from AlAs or AlxGaAs materials with a thickness of 10 - 50 nm, and the component of Al is 0.4 < x ≤ 1. Alternatively, the etching barrier layer can be selected as GaInP. The ohmic contact layer 103 can be selected from any one metal material or any combination of two or more metal materials among Pd, Au, Ag, Ni, Ti, Zn, Al, Cu, and Fe.

[0054] Furthermore, the epitaxial functional layer can be selected from one of the following:

[0055] 1.1 The epitaxial functional layer can be selected as an electro-optical conversion layer to form a light-emitting diode device structure. Select an N-type semiconductor, multiple quantum wells, and P-type semiconductor structure fabricated by a thin-film semiconductor preparation process. High-concentration electrons and holes are respectively injected into the quantum wells from the N-type semiconductor region and the P-type semiconductor region for recombination to generate photons, realizing electro-optical conversion. Taking a red light-emitting diode as an example, an N-AlInP layer, multiple AlGaInP quantum wells, and a P-AlInP layer can be selected as the epitaxial functional layer.

[0056] 1.2 The epitaxial functional layer can be selected as a photoelectric conversion layer to form a photovoltaic cell device structure. The N-type semiconductor and P-type semiconductor structures made by the thin-film semiconductor preparation process are selected. The working principle of the photovoltaic cell is as follows: (1) The electrons in the semiconductor absorb photons from an external light source (sun, laser, various fluorescent lights), and the photons excite the electrons to generate electron-hole pairs. These unbalanced carriers have a sufficient lifespan and will not recombine and disappear before separation; (2) The generated unbalanced carriers complete the separation of electron-hole pairs under the action of the built-in electric field. The electrons are concentrated on the N-type semiconductor side and the holes are concentrated on the P-type semiconductor side, resulting in the accumulation of opposite charges on both sides of the PN junction, thereby generating a photoinduced electromotive force; (3) The PN junction is connected with a wire to form a current and supply power to the load through an external circuit to obtain effective power output.

[0057] Gallium arsenide is a direct transition material. It can absorb light in the wavelength range of 300-900nm. A material with a thickness of 5-10μm can absorb up to 95% of sunlight, and can achieve a high photoelectric conversion efficiency. The above-mentioned photovoltaic device single-junction photovoltaic device can select N-type GaAs\P-type GaAs. In order to further improve the photoelectric conversion efficiency, multi-junction photovoltaic cells are set up, and the semiconductor energy band is regulated by doping and other methods, so that different cells can achieve absorption of different bands, further improving the utilization rate of light; a typical multi-junction cell can be a GaInP / GaAs / InGaAs triple-junction cell, which has the characteristics of high conversion efficiency, excellent radiation resistance, and stable performance.

[0058] 1.3 The epitaxial functional layer can be selected as an infrared detection layer composed of a photoelectric conversion layer. The basic principle of semiconductor detection is similar to that of photovoltaic cells. The detection photons enter the PN junction and generate electron-hole pairs. The electron-hole pairs drift under the action of the external electric field and output signals. Specifically, it is manifested as a change in the number of corresponding carriers (i.e., electron-holes) of the detector. Taking infrared detection as an example, for III-V materials, the InP / InGaAs material system can be selected as an infrared detector, which has the characteristics of high detection rate, high uniformity, and high stability.

[0059] 2. Growing a supporting substrate on the ohmic contact layer

[0060] The support substrate is a composite metal substrate, which includes at least a flexible metal layer 102, a cutoff layer 101, and a temporary metal substrate layer 100. The metal substrate layer 100 mainly serves as a temporary support, which helps to realize the peeling of the epitaxial layer and the temporary GaAs substrate in the subsequent steps and the growth of the subsequent structural layer. The cutoff layer 101 is finally removed by cleaning with an etching solution to separate the temporary metal substrate layer 100 and the flexible metal layer 102. The flexible metal layer 102 is finally used as part of the semiconductor chip, as a chip electrode and to maintain the flexibility of the entire chip. Its thickness can be set to 10-100um as needed.

[0061] Specifically, the composite metal substrate is prepared by evaporation. Compared with bonding, the evaporation process is simple, and the same evaporation equipment can be used. Only the evaporation source needs to be replaced to deposit multiple layers of metal on the composite metal substrate. As an alternative, the composite metal substrate can also be prepared by liquid phase deposition.

[0062] 3. Stripping and removal of temporary GaAs substrate

[0063] The first sacrificial layer can be chemically stripped. The principle is to set a sacrificial layer between two thin films, and use the high selectivity of the etching liquid to the sacrificial layer and the two films, that is, the etching rate of the etching liquid to the sacrificial layer is much higher than that of the two films, so that the corrosion of the etching liquid to the two films can be ignored. The sacrificial layer is removed by the etching liquid to separate the two films. The stripping sacrificial layer is selected from a material whose etching rate in an acidic or oxidizing solution is much higher than that of GaAs, such as HF, to strip and remove the gallium arsenide substrate. That is, by immersing in an HF solution, the AlAs sacrificial layer is corroded away, so that the gallium arsenide substrate falls off, and an epitaxial film with a composite metal substrate is obtained.

[0064] In other embodiments of the present invention, the corrosion barrier layer is used to corrode the gallium arsenide substrate using a mixture of phosphoric acid and hydrogen peroxide to remove the gallium arsenide. Thereafter, the corrosion barrier layer GaInP is removed by using a mixture of nitric acid and hydrochloric acid to achieve temporary GaAs substrate peeling and obtain an epitaxial layer film with a composite metal substrate.

[0065] 4. Prepare an electrode 106 on the side of the GaAs substrate where the epitaxial film is peeled off

[0066] Specifically, the electrode 106 is prepared by photolithography, metal evaporation, and resist stripping.

[0067] 5. Prepare an anti-reflection film 105 around the electrode 106

[0068] Specifically, the anti-reflection film 105 can be manufactured by photolithography, evaporation of TiO2 / Al2O3 double anti-reflection film, and debonding.

[0069] The structure of the semiconductor chip prepared is as follows Figure 5 shown.

[0070] 6. Cutting epitaxial layer and part of composite metal substrate

[0071] The electrode 106 and the anti-reflection film 105 are covered with photoresist; that is, the effective area of ​​the chip is covered with photoresist by photolithography, and the cutting area is free of photoresist, and the epitaxial layer and part of the composite metal substrate are etched along the cutting area in a direction perpendicular to the chip. Specifically, the epitaxial layer and the flexible metal layer can be selectively etched; optionally, the epitaxial layer, the flexible metal layer 102, and the cut-off layer 101 can be selectively etched. Specifically, dry etching or wet etching can be selected.

[0072] 7. Remove the stop layer 101 and the temporary metal substrate layer 100 to obtain a thin-film semiconductor chip.

[0073] The temporary metal substrate 100 on the back of the chip is ground, specifically polished, to be thinned to a pre-set cut-off layer 101, and then the surface is cleaned by a wet chemical method using an etching solution to clean the cut-off layer 101, thereby obtaining a super-thin single-chip particle, such as Figure 6 shown.

[0074] The above embodiments are merely illustrative of the principles and structures of the present invention, and are not intended to limit the present invention. It should be understood by those skilled in the art that any changes and improvements made to the present invention without departing from the overall concept of the present invention are within the scope of the present invention. The scope of protection of the present invention shall be subject to the scope defined by the claims of this application.

Claims

1. A method for preparing a thin film semiconductor chip, comprising: epitaxially growing a semiconductor chip epitaxial wafer on a first temporary substrate, the semiconductor chip epitaxial wafer comprising a sacrificial layer adjacent to the temporary substrate; Preparing a composite metal substrate on a side of the semiconductor chip epitaxial wafer opposite to the first temporary substrate, the composite metal substrate comprising a thin film metal layer, a stop layer and a second temporary substrate in order from one side of the semiconductor chip epitaxial wafer; The sacrificial layer is corroded by a first corrosive solution to peel off the semiconductor chip epitaxial wafer from the first temporary substrate; Using the composite metal substrate as a support, subsequent chip processing is performed on the side of the semiconductor chip epitaxial wafer opposite to the composite metal substrate; as well as removing the second temporary substrate and the cut-off layer to obtain a thin film semiconductor chip; Wherein, the cut-off layer is a metal layer, and the second temporary substrate is a metal substrate.

2. The method for manufacturing a thin film semiconductor chip according to claim 1, wherein: Preparing a composite metal substrate on a side of the semiconductor chip epitaxial wafer opposite to the first temporary substrate includes: A thin film metal layer, a cut-off layer and a temporary metal substrate layer are sequentially deposited on a semiconductor chip epitaxial wafer using an evaporation process or a liquid phase deposition process.

3. The method for manufacturing a thin film semiconductor chip according to claim 1, wherein: Removing the second temporary substrate and the stop layer comprises: The stop layer is etched by the second etching solution to peel the thin film semiconductor chip from the second temporary substrate.

4. The method for manufacturing a thin film semiconductor chip according to claim 3, further comprising: Before the stop layer is etched by the second etching solution, the semiconductor chip layer is vertically divided until the upper surface of the stop layer or the upper surface of the second temporary substrate.

5. The method for manufacturing a thin film semiconductor chip according to claim 1, wherein: Removing the second temporary substrate and the stop layer comprises: The second temporary substrate is removed by grinding, and then the stop layer is etched by a second etching solution.

6. The method for manufacturing a thin film semiconductor chip according to claim 1, wherein: The thickness of the thin film metal layer is 10-100 μm.

7. The method for manufacturing a thin film semiconductor chip according to claim 1, wherein: The thin film semiconductor chip is a light emitting diode device, a photovoltaic cell device or a photodetector.

8. A thin film semiconductor chip preparation structure, comprising: A semiconductor chip epitaxial wafer on a first temporary substrate, wherein a sacrificial layer is provided between the semiconductor chip epitaxial wafer and the temporary substrate, wherein the sacrificial layer is subsequently used to peel off the semiconductor chip and the first temporary substrate; and A composite metal substrate on a semiconductor chip epitaxial wafer, wherein the composite metal substrate comprises a thin film metal layer, a cut-off layer and a second temporary substrate in sequence from one side of the semiconductor chip epitaxial wafer, wherein the cut-off layer is subsequently used to peel off the semiconductor chip and the second temporary substrate; The cut-off layer is a metal layer, and the second temporary substrate is a metal substrate.

9. The thin film semiconductor chip preparation structure according to claim 8, wherein: The thickness of the thin film metal layer is 10-100 μm.