A supported catalyst, its preparation method and application

By using pure-phase calcium oxide as a support and mixing it with noble metal colloids under an inert atmosphere to prepare a catalyst, the problem of calcium oxide easily generating impurities was solved, and high selectivity was achieved in the selective hydrogenation of styrene oxide to 1-phenylethanol.

CN117920205BActive Publication Date: 2026-11-17THE NAT CENT FOR NANOSCI & TECH NCNST OF CHINA
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410088483.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-22
Publication Date
2026-11-17
Estimated Expiration
2044-01-22

AI Technical Summary

Technical Problem

Existing supported catalyst carriers, such as calcium oxide, readily react with water and carbon dioxide in the air to generate impurities, leading to a decline in catalyst performance and making it difficult to effectively improve the selectivity of 1-phenylethanol.

Method used

Pure-phase calcium oxide was used as a support, and a supported catalyst was prepared by mixing it with noble metal colloids and organic solvents under an inert atmosphere to avoid the reaction of water and carbon dioxide. The size of the noble metal particles was controlled at 1-5 nm.

Benefits of technology

It significantly improves the selectivity of selective hydrogenation of styrene oxide to 1-phenylethanol, increasing it from 0.3% in the prior art to over 41.2%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117920205B_ABST
    Figure CN117920205B_ABST
Patent Text Reader

Abstract

This invention provides a supported catalyst, its preparation method, and its application. The supported catalyst includes a support and an active component, wherein the active component includes a noble metal, and the support is calcium oxide, which does not contain calcium carbonate or calcium hydroxide impurities. The supported catalyst of this invention uses pure-phase calcium oxide as the support and a noble metal as the active component. It can be applied to the selective hydrogenation of styrene oxide and significantly improves the selectivity of the hydrogenation product 1-phenylethanol. It is an excellent catalyst for controlling the ring-opening site of styrene oxide to generate 1-phenylethanol.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of precious metal catalyst technology, and relates to a supported catalyst, its preparation method and application. Background Technology

[0002] The selective hydrogenation of styrene to phenethyl alcohol is an important alcohol production pathway, with products of different hydrogenation sites being 1-phenylethanol and 2-phenylethanol. 2-phenylethanol is more readily obtained due to the greater stability of carbocations or radicals attached to the benzene ring. 1-Phenylene alcohol has higher economic value and is more difficult to generate; therefore, finding catalysts to improve the selectivity of 1-phenylethanol is crucial.

[0003] CN 1111228A discloses a method for preparing β-phenylethanol by catalytic hydrogenation of styrene oxide. The inert organic solvent used in the preparation process is water. Under alkaline conditions, skeletal nickel is used as a catalyst, and the catalytic hydrogenation to prepare β-phenylethanol is carried out at a reaction temperature of 25–50 °C and a pressure of 1.0–5.0 MPa. CN 1546444A discloses a catalyst for the hydrogenation of styrene oxide to prepare β-phenylethanol, its preparation, and its application. The catalyst is prepared by loading Pd onto NaY, MCM41, β-molecular sieve, metal oxides γ-Al2O3, TiO2, and MgO using an equal-volume impregnation method, wherein the Pd content is 0.1 wt%–0.15 wt%. Both of these prior art methods disclose the ring-opening reaction of styrene oxide hydrogenation, with 2-phenylethanol as the main product and a selectivity of over 98%. However, none of them mention 1-phenylethanol in the product list.

[0004] Traditional supported catalysts typically use carbon supports, alumina, and magnesium oxide as supports. Calcium oxide is rarely used as a catalyst support, primarily because it readily transforms in air to form calcium carbonate (reacting with carbon dioxide) and calcium hydroxide (reacting with water). Another reason is that calcium oxide is difficult to support metals. Traditional metal-supported methods involve impregnation, where an aqueous solution of a metal salt is heated with the support and then calcined, causing the metal salt to decompose into metal oxides, which are then reduced by hydrogen to obtain the supported metal catalyst. However, calcium oxide readily reacts with water and swells during this process, significantly altering its structure. Furthermore, the calcination process involves contact with carbon dioxide, generating numerous impurity phases, which is detrimental to producing catalysts supported by pure calcium oxide crystals and hinders the expression of the advantages and characteristics of calcium oxide as a support.

[0005] Based on the above research, there is a need to provide a supported catalyst, which uses calcium oxide as a support and can be applied to the selective hydrogenation of styrene oxide. Summary of the Invention

[0006] The purpose of this invention is to provide a supported catalyst, its preparation method, and its application, particularly a supported catalyst for the selective hydrogenation of styrene to 1-phenylethanol, its preparation method, and its application. The supported catalyst uses pure-phase calcium oxide as a support and noble metal as the active component. It can selectively hydrogenate styrene and significantly improve the selectivity of the hydrogenation product 1-phenylethanol. It is an excellent catalyst for controlling the ring-opening site of styrene oxidation to generate 1-phenylethanol.

[0007] To achieve this objective, the present invention employs the following technical solution:

[0008] In a first aspect, the present invention provides a supported catalyst comprising a support and an active component, wherein the active component comprises a noble metal, the support is calcium oxide, and the calcium oxide does not contain calcium carbonate and calcium hydroxide impurities.

[0009] Since the acid and basic sites of the catalyst are very important for the catalytic reaction, calcium oxide, as a basic support, plays an important role in improving the selectivity of selective hydrogenation of styrene oxide. This invention uses pure-phase calcium oxide as a noble metal support to improve the selectivity of selective hydrogenation of styrene oxide to the hydrogenation product 1-phenylethanol.

[0010] Preferably, the precious metal includes any one or a combination of at least two of platinum, ruthenium, iridium, rhodium, or palladium.

[0011] Preferably, the particle size of the precious metal is 1-5nm, which means that the minimum particle size of the precious metal is above 1nm, such as 1nm, 1.5nm or 2nm, and the maximum particle size is below 5nm, such as 5nm, 4.5nm or 4nm, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable, preferably 2-4nm.

[0012] Preferably, the content of noble metal in the supported catalyst is 0.01-10 wt%, for example, it can be 0.05 wt%, 1 wt%, 3 wt%, 5 wt%, 7 wt%, 9 wt% or 10 wt%, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0013] Thirdly, the present invention provides a method for preparing a supported catalyst as described in the first aspect, the method comprising the following steps:

[0014] (1) Calcium oxide is calcined to obtain calcined calcium oxide;

[0015] (2) Under an inert atmosphere, the colloid containing precious metals, the organic solvent and the calcined calcium oxide described in step (1) are mixed, separated into solid and liquid and dried to obtain the supported catalyst;

[0016] Alternatively, under an inert atmosphere, the noble metal source, organic solvent, and the calcined calcium oxide described in step (1) are mixed and dried, and then treated under a reducing atmosphere to obtain the supported catalyst.

[0017] This invention enables the preparation of the supported catalyst using two methods. One method involves adsorption and loading of calcium oxide with a colloid containing noble metals, avoiding the disadvantages of introducing salt and water in the impregnation method, thereby preventing the introduction of impurity phases into the calcium oxide. The other method involves directly mixing, evaporating, and reducing the noble metal source, organic solvent, and calcium oxide. Both methods require calcination of the calcium oxide first to decompose the original calcium carbonate and calcium hydroxide in the support, thereby improving the purity of the support raw materials.

[0018] Preferably, the organic solvent in step (2) includes an ultra-dry organic solvent, preferably ultra-dry acetonitrile.

[0019] This invention uses ultra-dry acetonitrile as a supporting solvent to prepare the catalyst under inert gas protection, avoiding the reaction of water in the air and solution with calcium oxide to form calcium hydroxide; at the same time, acetonitrile as a solvent can dissolve noble metal salts, replacing the traditional method of using water as a solvent, and avoiding the reaction of calcium oxide with water to form calcium hydroxide.

[0020] Preferably, the water content in the ultra-dry organic solvent is ≤100ppm, for example, it can be 100ppm, 90ppm, 80ppm, 70ppm, 60ppm, 50ppm, 40ppm or 30ppm, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0021] Preferably, in step (2), when mixing the precious metal-containing colloid, the organic solvent, and the calcined calcium oxide described in step (1), under an inert atmosphere, the organic solvent and the calcined calcium oxide described in step (1) are first stirred and dispersed to obtain a dispersion. Then, the precious metal-containing colloid is dropped into the dispersion and stirred. The ratio of the volume (mL) of the organic solvent to the mass (g) of the calcined calcium oxide described in step (1) is 10-500, for example, it can be 50, 100, 200, 300, 400, or 500. The stirring time for dropping the precious metal-containing colloid into the dispersion is greater than 0.5h, for example, it can be 0.8h, 1h, 2h, or 3h, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0022] Preferably, the method for preparing the noble metal-containing colloid in step (2) includes:

[0023] The noble metal source and ethylene glycol are mixed, the pH is adjusted, and then the mixture is heated in an inert gas atmosphere. After cooling, the colloid containing the noble metal is obtained.

[0024] Preferably, the pH is adjusted to 9-13, for example, 10, 11, 12 or 13, but not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0025] Preferably, the heating temperature is 120-180℃, for example, it can be 130℃, 150℃, 170℃ or 180℃, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0026] In this invention, sodium hydroxide is added to adjust the pH, and then the solution is heated in an inert gas until it turns brown or other dark colors, after which heating continues for a period of time.

[0027] When mixing the precious metal source, organic solvent and the calcined calcium oxide described in step (1) in step (2), the precious metal source and organic solvent are first mixed to obtain a mixture, and then the calcined calcium oxide described in step (1) is mixed with the mixture.

[0028] Preferably, the temperature of the treatment in the reducing atmosphere in step (2) is 0-200℃, for example, 50℃, 100℃, 150℃ or 200℃, and the time is ≥1min, for example, 1min, 3min, 5min, 8min, 10min, 15min, 20min, 25min or 30min, but not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0029] Preferably, the reducing atmosphere in step (2) includes hydrogen.

[0030] Preferably, the noble metal source includes any one or a combination of at least two of chloroplatinic acid, potassium chloroplatinate, platinum nitrate, ruthenium trichloride, ruthenium nitrate, rhodium trichloride, rhodium nitrate, iridium trichloride, iridium nitrate, or palladium chloride.

[0031] Preferably, the calcination temperature in step (1) is 700-1200℃, for example, 800℃, 1000℃, or 1200℃, and the time is ≥1h, for example, 2h, 4h, 6h, or 8h, but not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0032] As a preferred embodiment of the preparation method of the present invention, the preparation method includes the following steps:

[0033] (1) Calcium oxide is calcined at 700-1200℃ for more than 1 hour.

[0034] (2) Mix the precious metal source and ethylene glycol, then adjust the pH to 9-13, and heat it in an inert gas to 120-180℃. After cooling, a colloid containing precious metal is obtained.

[0035] Under an inert atmosphere, ultra-dry acetonitrile and the calcined calcium oxide described in step (1) are first stirred and dispersed to obtain a dispersion. Then, the colloid containing noble metal is dropped into the dispersion and stirred until the supernatant is transparent and colorless. Then, ultra-dry acetonitrile is centrifuged and washed, and finally, freeze-dried to obtain the supported catalyst.

[0036] Alternatively, the noble metal source is mixed with ultra-dry acetonitrile to obtain a mixture. Then, under an inert atmosphere, the calcined calcium oxide from step (1) is mixed with the mixture and dried. Then, under a reducing atmosphere, it is treated at a temperature of 0-200°C for more than 1 minute. Finally, it is washed and dried with ultra-dry acetonitrile to obtain the supported catalyst.

[0037] Thirdly, the present invention provides an application of the supported catalyst as described in the first aspect, the application including selective hydrogenation reduction of styrene.

[0038] Preferably, the organic solvent used in the application includes saturated liquid alkanes, the reaction temperature is 40-200°C, for example, 50°C, 100°C, 150°C or 200°C, and the pressure is greater than 0.1 MPa, for example, 0.3 MPa, 0.5 MPa, 0.9 MPa or 1 MPa, but not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0039] Preferably, the saturated liquid alkanes include C5-C12 straight-chain alkanes and / or cycloalkanes, such as pentane, hexane, heptane, octane, nonane, undecane, dodecane, cyclopentane, cyclohexane, methylcyclohexane, or dimethylcyclohexane.

[0040] Compared with the prior art, the present invention has the following beneficial effects:

[0041] This invention uses pure-phase calcium oxide as a support for noble metals. The catalyst supported on pure calcium oxide is applied to the selective hydrogenation of styrene oxide. The selectivity of 1-phenylethanol, the selective hydrogenation product of styrene oxide, is greatly improved, and the selectivity of 1-phenylethanol is increased from 0.3% in the reference catalyst (Pt / TiO2) to more than 41.2%. Attached Figure Description

[0042] Figure 1 The XRD pattern of commercially available calcium oxide that has not undergone calcination, as shown in Example 1 of this invention;

[0043] Figure 2 The XRD pattern of calcium oxide after calcination in step (1) of Example 1 of this invention;

[0044] Figure 3 The XRD pattern of the supported catalyst 0.5Pt / CaO-P-ultra-dry acetonitrile described in Example 1 of this invention;

[0045] Figure 4 This is a transmission electron microscope (TEM) image of the supported catalyst described in Example 1 of this invention on a 10 nm scale.

[0046] Figure 5 This is a transmission electron microscope (TEM) image of the supported catalyst described in Example 1 of this invention on a 5 nm scale.

[0047] Figure 6 The image shows the XRD pattern of the 0.5Pt / CaO supported catalyst described in Comparative Example 1 of this invention.

[0048] Figure 7 The XRD pattern of the supported catalyst 0.5Pt / CaO-acetone described in Example 7 of this invention;

[0049] Figure 8 The XRD pattern of the supported catalyst 0.5Pt / CaO-cyclohexanone described in Example 8 of this invention;

[0050] Figure 9 The XRD pattern of the supported catalyst 0.5Pt / CaO-ethanol described in Example 9 of this invention;

[0051] Figure 10 The XRD pattern of the supported catalyst 0.05Ru / CaO-P-ultra-dry acetonitrile described in Example 2 of this invention;

[0052] Figure 11 The image shows the XRD pattern of the supported catalyst 6Ru / CaO-P-impregnation method described in Example 3 of this invention.

[0053] Figure 12 The XRD pattern of the supported catalyst 2Rh / CaO-P-ultra-dry acetonitrile described in Example 4 of this invention;

[0054] Figure 13 The XRD pattern of the supported catalyst 3Ir / CaO-P-ultra-dry acetonitrile described in Example 5 of this invention;

[0055] Figure 14 The image shows the XRD pattern of the supported catalyst 9Pd / CaO-P-ultra-dry acetonitrile described in Example 6 of this invention. Detailed Implementation

[0056] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be considered as specific limitations thereof; in the ultra-dry acetonitrile used in the following embodiments, the water content is 100 ppm.

[0057] Example 1

[0058] This embodiment provides a supported catalyst, which includes a support and an active component. The active component is Pt, and the support is calcium oxide. The calcium oxide does not contain calcium carbonate or calcium hydroxide impurities. In the supported catalyst, the Pt content is 0.5 wt%, and the size of the Pt particles is in the range of 1-3 nm.

[0059] The preparation method of the supported catalyst includes the following steps:

[0060] (1) Under an argon atmosphere, 10g of commercial calcium oxide (CaO) was calcined at 1000℃ for 3h to obtain calcined calcium oxide.

[0061] (2) Dissolve 1.0 g H2PtCl6·6H2O in 200 mL of ethylene glycol, then add 75 mL of NaOH / EG (ethylene glycol) solution, stir magnetically for 20 min, adjust the pH to 11, and then heat to 130 °C under argon protection. After the solution turns blackish-brown, keep it for 0.5 h and cool naturally to obtain a Pt colloidal solution with a mass fraction of 0.12 wt%.

[0062] (3) Under an argon atmosphere, 1.0 g of the calcined calcium oxide obtained in step (1) was placed in 50 mL of ultra-dry acetonitrile, and 4.2 g of the Pt colloidal solution obtained in step (2) was added dropwise. After the Pt was fully loaded, the supernatant was removed by centrifugation, washed with ultra-dry acetonitrile, and freeze-dried to obtain the supported catalyst, which is denoted as 0.5Pt / CaO-P-ultra-dry acetonitrile.

[0063] The XRD pattern of commercially available calcium oxide that has not undergone calcination in this embodiment is shown below. Figure 1 As shown, the results indicate that the calcium oxide contains not only diffraction peaks but also impurity phases of calcium hydroxide and calcium carbonate. The XRD pattern of the calcined calcium oxide from step (1) is shown below. Figure 2 As shown, the XRD pattern of the supported catalyst 0.5Pt / CaO-P-ultra-dry acetonitrile is as follows. Figure 3 As shown, the results indicate that only calcium oxide diffraction peaks are present; the transmission electron microscope image of the supported catalyst under a 10 nm scale is shown below. Figure 4 As shown, the transmission electron microscope (TEM) image at a 5 nm scale is as follows. Figure 5 As shown, by Figure 5It can be seen that d = 0.278 nm corresponds to the (111) crystal plane of CaO and d = 0.226 nm corresponds to the (111) crystal plane of Pt.

[0064] Example 2

[0065] This embodiment provides a supported catalyst, which includes a support and an active component. The active component is Ru, and the support is calcium oxide. The calcium oxide does not contain calcium carbonate or calcium hydroxide impurities. In the supported catalyst, the Ru content is 0.05 wt%, and the Ru particle size is in the range of 1-3 nm.

[0066] The preparation method of the supported catalyst includes the following steps:

[0067] (1) Under an argon atmosphere, 10g of commercial calcium oxide (CaO) was calcined at 850℃ for 5h to obtain calcined calcium oxide.

[0068] (2) Dissolve 1.0g RuCl3·3H2O in 200mL of ethylene glycol, then add 60mL of NaOH / EG (ethylene glycol) solution, stir magnetically for 20min, adjust pH to 10, and then heat to 180℃ under argon protection. After the solution turns blackish-brown, keep it for 0.5h and cool naturally to obtain a Ru colloidal solution with a mass fraction of 0.13wt%.

[0069] (3) Under an argon atmosphere, 1.0 g of the calcined calcium oxide obtained in step (1) was placed in 30 mL of ultra-dry acetonitrile, and 0.4 g of the Ru colloidal solution obtained in step (2) was added dropwise. After the Ru was fully loaded, the supernatant was removed by centrifugation, washed with ultra-dry acetonitrile, and freeze-dried to obtain the supported catalyst, which is denoted as 0.05Ru / CaO-P-ultra-dry acetonitrile.

[0070] The XRD pattern of the supported catalyst 0.05Ru / CaO-P-ultra-dry acetonitrile described in this embodiment is as follows: Figure 10 As shown.

[0071] Example 3

[0072] This embodiment provides a supported catalyst, which includes a support and an active component. The active component is Ru, and the support is calcium oxide. The calcium oxide does not contain calcium carbonate and calcium hydroxide impurities. In the supported catalyst, the Ru content is 6 wt%, and the Ru particle size is in the range of 1-3 nm.

[0073] The preparation method of the supported catalyst includes the following steps:

[0074] (1) Under an argon atmosphere, 10g of commercial calcium oxide (CaO) was calcined at 1200℃ for 1.5h to obtain calcined calcium oxide;

[0075] (2) Under magnetic stirring, 1.0 g RuCl3·3H2O was dissolved in 300 mL of ultra-dry acetonitrile to obtain a Ru solution with a mass fraction of 0.16 wt%.

[0076] (3) Under an argon atmosphere, 37.5g of Ru solution was placed in a three-necked flask, and 1.0g of the calcined calcium oxide from step (1) was placed in the three-necked flask. The temperature was then raised to 80°C and evaporated to dryness under magnetic stirring. Then, the atmosphere was switched to hydrogen and Ru was reduced to black-gray at 80°C. The solution was kept for 20 minutes. Finally, the solution was washed with ultra-dry acetonitrile, the supernatant was removed by centrifugation, and the solution was freeze-dried to obtain the supported catalyst, which was denoted as 6Ru / CaO-P-impregnation method.

[0077] The XRD pattern of the supported catalyst 6Ru / CaO-P-impregnation method described in this embodiment is as follows: Figure 11 As shown.

[0078] Example 4

[0079] This embodiment provides a supported catalyst, which includes a support and an active component. The active component is Rh, and the support is calcium oxide. The calcium oxide does not contain calcium carbonate or calcium hydroxide impurities. In the supported catalyst, the content of Rh is 2 wt%, and the size of the Rh particles is in the range of 1-3 nm.

[0080] The preparation method of the supported catalyst includes the following steps:

[0081] (1) Under an argon atmosphere, 10g of commercial calcium oxide (CaO) was calcined at 1000℃ for 3h to obtain calcined calcium oxide.

[0082] (2) Dissolve 1.0 g RhCl3·3H2O in 200 mL of ethylene glycol, then add 70 mL of NaOH / EG solution, stir magnetically for 20 min, then heat the mixture to 130 °C under argon protection, and keep it for 0.5 h after the solution turns blackish brown. Finally, cool it naturally to room temperature under argon protection to obtain a Rh colloidal solution with a mass fraction of 0.13 wt%.

[0083] (3) Under argon protection, 1.0 g of calcined calcium oxide from step (1) was placed in 200 mL of ultra-dry acetonitrile, and 15.4 g of Rh colloidal solution was added dropwise. After Rh loading was complete, the supernatant was removed by centrifugation, washed with ultra-dry acetonitrile, and freeze-dried to obtain the supported catalyst, denoted as 2Rh / CaO-P-ultra-dry acetonitrile.

[0084] The XRD pattern of the supported catalyst 2Rh / CaO-P-ultra-dry acetonitrile described in this embodiment is as follows: Figure 12 As shown.

[0085] Example 5

[0086] This embodiment provides a supported catalyst, which includes a support and an active component. The active component is Ir, and the support is calcium oxide. The calcium oxide does not contain calcium carbonate or calcium hydroxide impurities. In the supported catalyst, the content of Ir is 3 wt%, and the size of the Ir particles is in the range of 1-3 nm.

[0087] The preparation method of the supported catalyst includes the following steps:

[0088] (1) Under an argon atmosphere, 10g of commercial calcium oxide (CaO) was calcined at 1000℃ for 3h to obtain calcined calcium oxide.

[0089] (2) Dissolve 1.0g IrCl3·3H2O in 200mL of ethylene glycol, then add 65mL of NaOH / EG solution, stir magnetically for 20min, then heat the mixture to 130℃ under argon protection, and keep it for 0.5h after the solution turns black brown. Finally, cool naturally to room temperature under argon protection to obtain an Ir colloidal solution with a mass fraction of 0.18wt%.

[0090] (3) Place 1.0g of calcined calcium oxide from step (1) into 100mL of ultra-dry acetonitrile, add 16.5g of Ir colloidal solution dropwise, and after Ir is fully loaded, centrifuge to remove the supernatant, wash with ultra-dry acetonitrile, freeze dry to obtain the supported catalyst, denoted as 3Ir / CaO-P-ultra-dry acetonitrile.

[0091] The XRD pattern of the supported catalyst 3Ir / CaO-P-ultra-dry acetonitrile described in this embodiment is as follows: Figure 13 As shown.

[0092] Example 6

[0093] This embodiment provides a supported catalyst, which includes a support and an active component. The active component is Pd, and the support is calcium oxide. The calcium oxide does not contain calcium carbonate or calcium hydroxide impurities. In the supported catalyst, the Pd content is 9 wt%, and the size of the Pd particles is in the range of 1-3 nm.

[0094] The preparation method of the supported catalyst includes the following steps:

[0095] (1) Under an argon atmosphere, 10g of commercial calcium oxide (CaO) was calcined at 1000℃ for 3h to obtain calcined calcium oxide.

[0096] (2) Under magnetic stirring, 1.0 g of PdCl2 was dissolved in 1200 mL of ultra-dry acetonitrile to obtain a Pd solution with a mass fraction of 0.064 wt%.

[0097] (2) Under an argon atmosphere, 140.6 g of Pd colloidal solution was placed in a three-necked flask, and 1.0 g of calcined calcium oxide from step (1) was placed in the three-necked flask. The temperature was then raised to 80°C and evaporated to dryness under magnetic stirring. Then, the atmosphere was switched to hydrogen and Pd was reduced to blackish-gray at 160°C. The reaction was maintained for 20 min. Finally, the solid was washed with acetonitrile, the supernatant was removed by centrifugation, and the solid was freeze-dried to obtain the supported catalyst, denoted as 9Pd / CaO-P-ultra-dry acetonitrile.

[0098] The XRD pattern of the supported catalyst 9Pd / CaO-P-ultra-dry acetonitrile described in this embodiment is as follows: Figure 14 As shown, by Figure 10-14 The results show that there are no impurity phase peaks such as calcium hydroxide.

[0099] Example 7

[0100] This embodiment provides a supported catalyst. Except for the method of preparation, in which acetone is replaced by an equal volume of ultra-dry acetonitrile to adapt the resulting supported catalyst (denoted as 0.5Pt / CaO-T-acetone), the rest of the supported catalyst is the same as in Example 1.

[0101] In this embodiment, the acetone used is a super-dehydrating solvent with a water content of 8 ppm.

[0102] The XRD pattern of the supported catalyst 0.5Pt / CaO-acetone obtained in this embodiment is shown in the figure below. Figure 7 As shown.

[0103] Example 8

[0104] This embodiment provides a supported catalyst. Except for the method of preparation, in which cyclohexanone is replaced by an equal volume of ultra-dry acetonitrile to adapt the resulting supported catalyst (denoted as 0.5Pt / CaO-cyclohexanone), the rest of the supported catalyst is the same as in Example 1.

[0105] In this embodiment, cyclohexanone is dehydrated using calcium oxide before use, and the water content of the cyclohexanone used is 1420 ppm.

[0106] The XRD pattern of the supported catalyst 0.5Pt / CaO-cyclohexanone obtained in this embodiment is shown below. Figure 8As shown.

[0107] Example 9

[0108] This embodiment provides a supported catalyst. Except for the method of preparation, in which ethanol is replaced by an equal volume of ultra-dry acetonitrile to change the adaptability of the resulting supported catalyst (denoted as 0.5Pt / CaO-ethanol), the supported catalyst is the same as in Example 1.

[0109] In this embodiment, the ethanol is dehydrated with calcium oxide before use, and the water content of the ethanol used is 50 ppm.

[0110] The XRD pattern of the supported catalyst 0.5Pt / CaO-ethanol obtained in this embodiment is shown in the figure below. Figure 9 As shown, by Figure 7-9 The results show that all samples contain calcium hydroxide as an impurity phase. When ethanol is used as a solvent, almost all calcium oxide is converted into calcium hydroxide. This is because ketones and alcohols are prone to condensation reactions. However, hydrocarbon solvents are not miscible with Pt colloids and are therefore not suitable as benign solvents.

[0111] Comparative Example 1

[0112] This comparative example provides a supported catalyst, which is the same as in Example 1 except that step (1) is not performed in its preparation method to make the obtained supported catalyst (denoted as 0.5Pt / CaO) adaptable.

[0113] The XRD pattern of the 0.5Pt / CaO supported catalyst obtained in this comparative example is shown below. Figure 6 As shown, the results reveal impurity crystalline phases containing calcium hydroxide and calcium carbonate.

[0114] Comparative Example 2

[0115] This comparative example provides a supported catalyst, which is the same as in Example 1 except that the calcium oxide in step (1) is replaced with MgO by mass in its preparation method, so that the resulting supported catalyst (denoted as 0.5Pt / MgO) is adapted to change.

[0116] Comparative Example 3

[0117] This comparative example provides a supported catalyst, which is the same as in Example 1 except that the calcium oxide in step (1) is replaced with TiO2 by mass in its preparation method, so that the resulting supported catalyst (denoted as 0.5Pt / TiO2) is adapted to change.

[0118] Comparative Example 4

[0119] This comparative example provides a supported catalyst, which is the same as in Example 1 except that in its preparation method, the calcium oxide in step (1) is replaced by ZnO by mass, so that the resulting supported catalyst (denoted as 0.5Pt / ZnO) is adapted to change.

[0120] Comparative Example 5

[0121] This comparative example provides a supported catalyst, which is the same as in Example 1 except that the calcium oxide in step (1) is replaced with Al2O3 by mass in its preparation method, so that the resulting supported catalyst (denoted as 0.5Pt / Al2O3) is adapted to change.

[0122] Application Example 1

[0123] This application example provides a method for the catalytic oxidation of styrene hydrogenation using a supported catalyst, wherein the supported catalyst is the 0.5Pt / CaO-P supported catalyst described in Example 1, and the method includes the following steps:

[0124] (1) Catalyst pretreatment: Weigh 0.3247g of the supported catalyst described in Example 1 and place it in the reaction liner. Then add 30mL of cyclohexane as the reaction solvent. Place the liner in a magnetic high-pressure reactor and charge and release H2 5 times to remove the air in the high-pressure reactor. Then charge 2MPa H2 at 500rpm, set the temperature to 90℃, and the treatment time is 30min.

[0125] (2) Catalytic oxidation of styrene hydrogenation: After the autoclave is cooled to room temperature, about 0.1000 g of styrene oxide is added to the above system. The liner is placed in the magnetic high-pressure reactor. H2 is charged and discharged 5 times to remove the air in the autoclave. Then, 2 MPa H2 is charged at 500 rpm. The temperature is set to 90°C and the reaction time is 8 h.

[0126] (3) Results analysis: After the reaction vessel was cooled to room temperature, 0.1550 g of biphenyl was added to the above system and stirred until completely dissolved. The supernatant was filtered and the product was analyzed by gas chromatography.

[0127] Application Example 2

[0128] This application example provides a method for the catalytic oxidation of styrene hydrogenation using a supported catalyst. The method is the same as that in Application Example 1, except that octane is used as the reaction solvent in step (1).

[0129] Application Example 3

[0130] This application example provides a method for the catalytic oxidation of styrene hydrogenation using a supported catalyst. The method is the same as that in Application Example 1, except that methylcyclohexane is used as the reaction solvent in step (1).

[0131] Application Example 4

[0132] This application example provides a method for catalytic oxidation of styrene hydrogenation using a supported catalyst. Except that the supported catalyst is the 0.05Ru / CaO-P-ultra-dry acetonitrile supported catalyst described in Example 2, and the amount of supported catalyst added in step (1) is 3.2470 g, the rest are the same as in Application Example 1.

[0133] Application Example 5

[0134] This application example provides a method for catalytic oxidation of styrene hydrogenation using a supported catalyst. The supported catalyst is the 6Ru / CaO-P-impregnation method of the supported catalyst described in Example 3. Except for the amount of the supported catalyst added in step (1) being 0.0271g, all other steps are the same as in Application Example 1.

[0135] Application Example 6

[0136] This application example provides a method for catalytic oxidation of styrene hydrogenation using a supported catalyst. The supported catalyst is the 2Rh / CaO-P-ultra-dry acetonitrile supported catalyst described in Example 4. Except for the amount of supported catalyst added in step (1) being 0.0813 g, the rest is the same as in Application Example 1.

[0137] Application Example 7

[0138] This application example provides a method for catalytic oxidation of styrene hydrogenation using a supported catalyst. The supported catalyst is the 3Ir / CaO-P-ultra-dry acetonitrile supported catalyst described in Example 5. Except for the amount of supported catalyst added in step (1) being 0.0541 g, the rest is the same as in Application Example 1.

[0139] Application Example 8

[0140] This application example provides a method for catalytic oxidation of styrene hydrogenation using a supported catalyst. The supported catalyst is the 9Pd / CaO-P-ultra-dry acetonitrile supported catalyst described in Example 6. Except for the amount of supported catalyst added in step (1) being 0.0181g, the rest is the same as in Application Example 1.

[0141] Application Example 9

[0142] This application example provides a method for catalytic oxidation and hydrogenation of styrene using a supported catalyst. The supported catalyst is the same as that in Application Example 1, except that it is the supported catalyst described in Example 7.

[0143] Application Example 10

[0144] This application example provides a method for catalytic oxidation and hydrogenation of styrene using a supported catalyst. The supported catalyst is the same as that in Application Example 1, except that it is the supported catalyst described in Example 8.

[0145] Application Example 11

[0146] This application example provides a method for catalytic oxidation and hydrogenation of styrene using a supported catalyst. The supported catalyst is the same as that in Application Example 1, except that it is the supported catalyst described in Example 9.

[0147] Comparative Application Example 1

[0148] This application example provides a method for catalytic oxidation and hydrogenation of styrene using a supported catalyst. The supported catalyst is the same as that in Application Example 1, except that it is the same as the supported catalyst described in Comparative Example 1.

[0149] Comparative Application Example 2

[0150] This application example provides a method for catalytic oxidation and hydrogenation of styrene using a supported catalyst. The supported catalyst is the same as that in Application Example 1, except that it is the 0.5Pt / MgO supported catalyst described in Comparative Example 2.

[0151] Comparative Application Example 3

[0152] This application example provides a method for catalytic oxidation and hydrogenation of styrene using a supported catalyst. The supported catalyst is the same as that in Application Example 1, except that it is the 0.5Pt / TiO2 supported catalyst described in Comparative Example 3.

[0153] Comparative Application Example 4

[0154] This application example provides a method for catalytic oxidation and hydrogenation of styrene using a supported catalyst. The supported catalyst is the same as that in Application Example 1, except that it is the 0.5Pt / ZnO supported catalyst described in Comparative Example 4.

[0155] Comparative Application Example 5

[0156] This application example provides a method for catalytic oxidation and hydrogenation of styrene using a supported catalyst. The supported catalyst is the same as that in Application Example 1, except that it is the 0.5Pt / Al2O3 supported catalyst described in Comparative Example 5.

[0157] The product analysis results of the above application examples and comparative application examples are shown in Table 1:

[0158] Table 1

[0159]

[0160] As can be seen from Table 1:

[0161] As can be seen from Application Example 1 and Comparative Application Example 1, the supported catalyst of the present invention exhibits higher selectivity for 1-phenylethanol in the catalytic hydrogenation of styrene, increasing from 15.5% in Comparative Application Example 1 to 41.2%, which is related to the presence of Ca(OH)2 and CaCO3 impurities in the calcium oxide in Comparative Application Example 1. As can be seen from Application Example 1 and Comparative Application Examples 2-5, the use of common supports such as MgO, TiO2, ZnO, and Al2O3 results in lower selectivity for the 1-phenylethanol product of styrene hydrogenation. (The last sentence appears to be incomplete and possibly refers to a different application example.) As shown in 4-8, when ruthenium, rhodium, iridium, and palladium were used as active centers to study the hydrogenation performance of styrene oxide, the selectivity of 1-phenylethanol was reduced to a certain extent compared with that of purified calcium oxide supported on platinum. As shown in Application Examples 1 and 9-11, even though other solvents have less water content than ultra-dry acetonitrile, they still cannot achieve the technical effect of ultra-dry acetonitrile. This is because the hydroxyl groups and carbonyl groups in acetone, cyclohexanone, and ethanol are prone to condensation reactions to generate water. Therefore, the above three solvents will cause calcium oxide to react with water to generate calcium hydroxide impurity phase.

[0162] In summary, this invention provides a supported catalyst, its preparation method, and its application. The supported catalyst uses pure-phase calcium oxide as a support and noble metal as the active component. It can be applied to the selective hydrogenation of styrene oxide and significantly improves the selectivity of the hydrogenation product 1-phenylethanol. It is an excellent catalyst for regulating the ring-opening site of styrene oxide to generate 1-phenylethanol.

[0163] The above description is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention fall within the protection and disclosure scope of the present invention.

Claims

1. A supported catalyst for the selective hydrogenation of styrene to 1-phenylethanol, characterized in that, The supported catalyst includes a support and an active component. The active component includes a noble metal, wherein the noble metal is platinum, and the support is calcium oxide, wherein the calcium oxide does not contain calcium carbonate or calcium hydroxide impurities. The supported catalyst is prepared by the following method, which includes the following steps: (1) Calcium oxide is calcined to obtain calcined calcium oxide; (2) Under an inert atmosphere, the colloid containing precious metals, the organic solvent and the calcined calcium oxide described in step (1) are mixed, separated into solid and liquid and dried to obtain the supported catalyst; Alternatively, under an inert atmosphere, the noble metal source, organic solvent and the calcined calcium oxide described in step (1) are mixed and dried, and then treated under a reducing atmosphere to obtain the supported catalyst; The organic solvent in step (2) is ultra-dry acetonitrile.

2. The supported catalyst according to claim 1, characterized in that, The particle size of the precious metal is 1-5 nm.

3. The supported catalyst according to claim 2, characterized in that, The particle size of the precious metal is 2-4 nm.

4. The supported catalyst according to claim 1, characterized in that, The supported catalyst contains 0.01-10 wt% precious metals.

5. A method for preparing a supported catalyst as described in any one of claims 1-4, characterized in that, The preparation method includes the following steps: (1) Calcium oxide is calcined to obtain calcined calcium oxide; (2) Under an inert atmosphere, the colloid containing precious metals, the organic solvent and the calcined calcium oxide described in step (1) are mixed, separated into solid and liquid and dried to obtain the supported catalyst; Alternatively, under an inert atmosphere, the noble metal source, organic solvent and the calcined calcium oxide described in step (1) are mixed and dried, and then treated under a reducing atmosphere to obtain the supported catalyst; The organic solvent in step (2) is ultra-dry acetonitrile.

6. The preparation method according to claim 5, characterized in that, The water content in the ultra-dry acetonitrile is ≤100 ppm.

7. The preparation method according to claim 5, characterized in that, In step (2), when mixing the precious metal-containing colloid, organic solvent, and the calcined calcium oxide described in step (1), the organic solvent and the calcined calcium oxide described in step (1) are first stirred and dispersed under an inert atmosphere to obtain a dispersion. Then, the precious metal-containing colloid is dropped into the dispersion and stirred.

8. The preparation method according to claim 5, characterized in that, The method for preparing the noble metal-containing colloid in step (2) includes: The noble metal source and ethylene glycol are mixed, the pH is adjusted, and then the mixture is heated in an inert gas atmosphere. After cooling, the colloid containing the noble metal is obtained.

9. The preparation method according to claim 8, characterized in that, Adjust the pH to 9-13.

10. The preparation method according to claim 8, characterized in that, The heating temperature is 120-180℃.

11. The preparation method according to claim 5, characterized in that, When mixing the precious metal source, organic solvent and the calcined calcium oxide described in step (1) in step (2), the precious metal source and organic solvent are first mixed to obtain a mixture, and then the calcined calcium oxide described in step (1) is mixed with the mixture.

12. The preparation method according to claim 5, characterized in that, The temperature for treatment in the reducing atmosphere described in step (2) is 80-200℃, and the time is ≥1min.

13. The preparation method according to claim 5, characterized in that, The reducing atmosphere in step (2) includes hydrogen.

14. The preparation method according to claim 5, characterized in that, The precious metal source includes any one or a combination of at least two of chloroplatinic acid, potassium chloroplatinate, or platinum nitrate.

15. The preparation method according to claim 5, characterized in that, The calcination temperature in step (1) is 700-1200℃, and the time is ≥1h.

16. The preparation method according to claim 5, characterized in that, The preparation method includes the following steps: (1) Calcium oxide is calcined at 700-1200℃ for more than 1 hour to obtain calcined calcium oxide; (2) Mix the precious metal source and ethylene glycol, then adjust the pH to 9-13, and heat it to 120-180℃ in an inert gas. After cooling, a colloid containing precious metal is obtained. Under an inert atmosphere, ultra-dry acetonitrile and the calcined calcium oxide described in step (1) are first stirred and dispersed to obtain a dispersion. Then, the colloid containing noble metal is dropped into the dispersion and stirred until the supernatant is transparent and colorless. Then, ultra-dry acetonitrile is centrifuged and washed, and finally, freeze-dried to obtain the supported catalyst. Alternatively, under an inert atmosphere, the noble metal source is mixed with ultra-dry acetonitrile to obtain a mixture. The calcined calcium oxide from step (1) is then mixed with the mixture and evaporated to dryness. The mixture is then treated at a temperature of 80-200°C for more than 1 minute under a reducing atmosphere. Finally, it is washed and dried with ultra-dry acetonitrile to obtain the supported catalyst.

17. An application of the supported catalyst as described in any one of claims 1-4, characterized in that, The applications include the selective hydrogenation of styrene to 1-phenylethanol via catalytic oxidation.

18. The application according to claim 17, characterized in that, The organic solvent used in the application includes saturated liquid alkanes, the reaction temperature is 40-200℃, and the reaction pressure is greater than 0.1MPa.

19. The application according to claim 18, characterized in that, The saturated liquid alkanes include C5-C12 straight-chain alkanes and / or cycloalkanes.

Citation Information

Patent Citations

  • Catalytic hydrogenation preparation of bata-phenethyl alcohol from phenylethylene oxide

    CN1111228A

  • Catalyst for hydrogenation of styrene oxide to beta-phenethyl alcohol, preparation and use thereof

    CN1546444A

  • Catalyst for anoxic dehydrogenation of methanol, and application thereof

    CN105170145A

  • Load type nano precious metal catalyst and preparation method and application thereof

    CN105457629A

  • Application of supported noble metal catalyst in reaction for preparing 2-phenethyl alcohol through styrene oxide hydrogenation

    CN116640044A