A high-gloss universal water-based nuclear titanium dioxide slurry and its preparation method

Through the high-gloss universal water-based core titanium dioxide formula and dispersion technology, the problems of traditional resin-free titanium dioxide dispersion effect and insufficient storage time are solved, the stable dispersion and high versatility of titanium dioxide are achieved, and the gloss and gloss of the coating are improved. Value for money.

CN117924972BActive Publication Date: 2024-10-18FOSHAN JIANFA RUITONG TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410255924.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-06
Publication Date
2024-10-18
Estimated Expiration
2044-03-06

AI Technical Summary

Technical Problem

Traditional resin-free titanium dioxide slurry has deficiencies in dispersion effect and storage time, which causes titanium dioxide particles to easily agglomerate, reducing the storage time and use effect of the coating.

Method used

It adopts a high-gloss universal water-based core titanium dioxide formula, including deionized water, co-solvent, defoaming agent, wetting agent, dispersant A and modified coating resin B. Through high-speed dispersion and grinding technology, the uniformity of titanium dioxide is ensured. Dispersion and particle size control, using specific media balls and coating resin B to enhance dispersion and versatility.

Benefits of technology

It achieves stable dispersion of titanium dioxide, improves the versatility and gloss of the coating, extends the storage time, and improves the pigment concentration and cost performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention provides a high-gloss universal water-based core titanium dioxide slurry, wherein the contents of the components are as follows, in parts by weight: 30 parts by weight of deionized water, 1-5 parts by weight of a cosolvent, 0.3-0.5 parts by weight of a defoamer, 0.3-0.5 parts by weight of a wetting agent, 1-2 parts by weight of a dispersant A, 1-5 parts by weight of a coating resin B, and 70 parts by weight of core titanium dioxide. Preferably, the cosolvent is one or more of ethanol, propylene glycol, ethylene glycol butyl ether, and diethylene glycol monobutyl ether; and the defoamer is one or more of BYK022, BYK028, TEGO901W, TEGO902W, NOPTAM-398, NOPTAM-1311, and SN-6024. The present invention activates the powder surface by dispersant A to solve the problem of low surface activity of the powder; medium balls of specific specifications are mixed in a specific proportion to promote the homogenous dispersion of nuclear titanium dioxide; modified coating additives are used to solve the problems of versatility and gloss of nuclear titanium dioxide slurry; in addition, the water-based nuclear titanium dioxide slurry is a resin-free system, has a higher effective pigment concentration, and has a better cost-effectiveness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of titanium dioxide slurry, and in particular to a high-gloss universal water-based core titanium dioxide slurry and a preparation method thereof. Background Art

[0002] As one of the main components of white or light-colored coatings, the production of titanium dioxide has always attracted widespread attention. The resin-free titanium dioxide made by using ultra-dispersion technology and adding surfactants to water as the medium is becoming more and more widely used. Compared with the resin system, the resin-free titanium dioxide has more advantages. First, it is more versatile. Due to the limitations of resin performance, the use of resin-based titanium dioxide is subject to certain limitations, and sometimes it cannot be used due to compatibility. The resin-free system is more widely used and suitable for most coating systems. Secondly, the resin-free titanium dioxide usually has a higher concentration and better cost-effectiveness. In addition, the resin-free titanium dioxide is more suitable for grinding technology and can produce products with higher concentration and finer fineness.

[0003] The performance of resin-free titanium dioxide slurry mainly depends on the performance and content of titanium dioxide used. The dispersion of titanium dioxide is the key to the production of titanium dioxide slurry. Each titanium dioxide has different hydrophilic and lipophilic properties. Traditional wetting dispersants have weak dispersion effects on titanium dioxide. The hydrophilic groups in the dispersant molecules have insufficient affinity for the surface of titanium dioxide with lower polarity and are easily detached, causing the titanium dioxide particles to re-agglomerate and making the titanium dioxide dispersion system unstable. After the titanium dioxide is dispersed, due to its finer particles and larger specific surface area, it will slowly settle during long-term storage and is difficult to disperse again, reducing the shelf life and use effect of the titanium dioxide slurry.

[0004] In summary, it is of great significance to develop a universal water-based nuclear titanium dioxide slurry that does not contain resin, has better dispersion effect, longer storage time and a wide range of applications. Summary of the invention

[0005] The purpose of the present invention is to provide a high-gloss universal water-based nuclear titanium dioxide slurry and a preparation method thereof to solve the problems in the above-mentioned background technology.

[0006] To achieve the above object, the present invention provides the following technical solutions: In a first aspect, the present invention provides a high-gloss universal water-based nuclear titanium dioxide slurry, wherein the content of each component is as follows in parts by weight:

[0007] 30 parts by weight of deionized water, 1-5 parts by weight of cosolvent, 0.3-0.5 parts by weight of defoamer, 0.3-0.5 parts by weight of wetting agent, 1-2 parts by weight of dispersant A, 1-5 parts by weight of coating resin B and 70 parts by weight of core titanium dioxide.

[0008] Preferably, the cosolvent is one or more of ethanol, propylene glycol, ethylene glycol butyl ether, and diethylene glycol monobutyl ether; the defoamer is one or more of BYK022, BYK028, TEGO901W, TEGO902W, NOPTAM-398, NOPTAM-1311, and SN-6024.

[0009] Preferably, the wetting agent is one or more of BYK-346, BYK-345, TEGO270, TEGO4100, SURFYNOL465, and SURFYNOL104E; and the dispersant A is one or more of BYK190, BYK2055, NOPCALL-5180, DISPERS-755 W, SN-1710, and SN-1729.

[0010] Preferably, the coating resin B is one or more of THYON PH729, THYON SRT3069, THYON SR675, AD666, and AD8058; and the core titanium dioxide is one or more of RTR201, RTR202, and RTR203.

[0011] The second aspect of the present invention provides a method for preparing the high-gloss universal water-based nuclear titanium dioxide slurry according to the first aspect of the present invention, comprising the following steps:

[0012] S1, preparation of nuclear titanium dioxide fine raw material slurry:

[0013] Add deionized water, cosolvent, dispersant A, defoamer and wetting agent into a stirring kettle in sequence and mix evenly. Add nuclear titanium dioxide and disperse at high speed for 20-30 minutes. Grind with a horizontal mill and adjust the particle size and proportion of the grinding medium balls.

[0014] S2, preparation of finished slurry:

[0015] Add modified coating resin B to the fine raw material slurry of nuclear titanium dioxide, and send the slurry obtained by grinding into a stirring kettle. Adjust the speed to 500-600 rpm, and add thickener to adjust to 10000-20000mPa.s

[0016] Preferably, the rotation speed of the high-speed dispersion in S1 is 800-1200 rpm.

[0017] Preferably, the particle size and proportion of the grinding medium balls are adjusted in S1 so that the particle size of the nuclear titanium dioxide slurry is -2um≥90%.

[0018] Preferably, the particle size of the final finished slurry in S2 is -2um≥90%.

[0019] Preferably, the horizontal mill contains three kinds of medium balls, whose diameters are 5 mm, 3 mm and 1.5 mm respectively, and the three kinds of medium balls are mixed in a weight ratio of (1-3): (1-2): (1-2).

[0020] Preferably, the three dielectric balls are one of 3.5 mm, 1.5 mm or 0.8 mm.

[0021] The present invention has at least the following beneficial effects:

[0022] (1) The present invention provides a high-gloss universal water-based nuclear titanium dioxide slurry and a preparation method thereof. The powder surface is activated by dispersant A to solve the problem of low surface activity of the powder; dielectric balls of specific specifications are mixed in a specific proportion to promote the homogenization and dispersion of nuclear titanium dioxide; and modified coating additives are used to solve the problems of versatility and gloss of the nuclear titanium dioxide slurry.

[0023] (2) The present invention provides a high-gloss universal water-based core titanium dioxide slurry and a preparation method thereof. The water-based core titanium dioxide slurry is a resin-free system with a higher effective pigment concentration and better cost-effectiveness.

[0024] (3) The present invention provides a high-gloss universal water-based nuclear titanium dioxide slurry and a preparation method thereof. The slurry prepared using nuclear titanium dioxide has the characteristics of narrow particle size distribution, uniform distribution and small particle size;

[0025] (4) The present invention provides a high-gloss universal water-based core titanium dioxide slurry and a preparation method thereof. The amphiphilic groups on the modified coating resin B react with the core titanium dioxide to produce an association effect, further improving the dispersibility of the particles in the coating system. The slurry is compatible with most coating systems, has stronger versatility, and has a higher coating gloss. DETAILED DESCRIPTION

[0026] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] The present invention provides a high-gloss universal water-based nuclear titanium dioxide slurry, and the content of each component is as follows in parts by weight:

[0028] 30 parts by weight of deionized water, 1-5 parts by weight of cosolvent, 0.3-0.5 parts by weight of defoamer, 0.3-0.5 parts by weight of wetting agent, 1-2 parts by weight of dispersant A, 1-5 parts by weight of coating resin B and 70 parts by weight of core titanium dioxide.

[0029] Among them, the cosolvent is one or more of ethanol, propylene glycol, ethylene glycol butyl ether, and diethylene glycol monobutyl ether; the defoaming agent is one or more of BYK022, BYK028, TEGO901W, TEGO902W, NOPTAM-398, NOPTAM-1311, and SN-6024.

[0030] Among them, the wetting agent is one or more of BYK-346, BYK-345, TEGO270, TEGO4100, SURFYNOL465, SURFYNOL104E; the dispersant A is one or more of BYK190, BYK2055, NOPCALL-5180, DISPERS-755W, SN-1710, SN-1729.

[0031] The coating resin B is one or more of THYON PH729, THYON SRT3069, THYON SR675, AD666, and AD8058; and the core titanium dioxide is one or more of RTR201, RTR202, and RTR203.

[0032] The preparation method of the above high-gloss universal water-based nuclear titanium dioxide slurry comprises the following steps:

[0033] S1, preparation of nuclear titanium dioxide fine raw material slurry:

[0034] Add deionized water, cosolvent, dispersant A, defoamer and wetting agent into a stirring kettle in sequence and mix evenly. Add nuclear titanium dioxide and disperse at high speed for 20-30 minutes. Grind with a horizontal mill and adjust the particle size and proportion of the grinding medium balls.

[0035] S2, preparation of finished slurry:

[0036] The modified coating resin B is added to the fine raw material slurry of nuclear titanium dioxide, and the slurry obtained by grinding is sent to a stirring kettle, the speed is adjusted to 500-600 rpm, and a thickener is added to adjust the pressure to 10000-20000 mPa.s.

[0037] Among them, the speed of high-speed dispersion in S1 is 800-1200 rpm.

[0038] Among them, the particle size and matching ratio of the grinding medium balls are adjusted in S1 so that the particle size of the nuclear titanium dioxide slurry is -2um≥90%.

[0039] Among them, the final finished slurry particle size in S2 is -2um≥90%.

[0040] There are three kinds of medium balls in the horizontal mill, with diameters of 5 mm, 3 mm, 1.5 mm or 3.5 mm, 1.5 mm, 0.8 mm, respectively. The three kinds of medium balls are mixed in a weight ratio of (1-3): (1-2): (1-2).

[0041] Based on the above technical solution, the present invention provides the following embodiments:

[0042] Example 1

[0043] (1) Add 30 kg of deionized water into a stirring kettle, add a cosolvent, a defoamer, a wetting agent, and then add 1 kg of dispersant A and 70 kg of nuclear titanium dioxide, and disperse at high speed for 30 minutes; then grind with a horizontal mill, there are 3 kinds of medium balls in the mill, the diameters of which are 5 mm, 3 mm, and 1.5 mm, respectively, and the 3 kinds of medium balls are mixed in a weight ratio of 3:1:1. The grinding speed is 600 rpm, the grinding temperature is controlled to be less than 70°C, and the slurry fineness -2um ≥ 90%.

[0044] (2) After grinding, add 1 kg of modified coating resin B, add 0.5 kg of thickener to the slurry, adjust the viscosity to 10000-20000 mpa.s, and control the fineness of the finished slurry to -2 um ≥ 90%.

[0045] Example 2

[0046] (1) Add 30 kg of deionized water into a stirring kettle, add a cosolvent, a defoamer, a wetting agent, and then add 1.5 kg of dispersant A and 70 kg of nuclear titanium dioxide, and disperse at high speed for 30 minutes; then grind with a horizontal mill, there are 3 kinds of medium balls in the mill, the diameters of which are 5 mm, 3 mm, and 1.5 mm, respectively, and the 3 kinds of medium balls are mixed in a weight ratio of 3:2:2. The grinding speed is 600 rpm, the grinding temperature is controlled to be less than 70°C, and the slurry fineness -2um ≥ 98%.

[0047] (2) After grinding, add 1.5 kg of modified coating resin B, add 0.5 kg of thickener to the slurry, adjust the viscosity to 10000-20000 mpa.s, and control the fineness of the finished slurry to -2 um ≥ 95%.

[0048] Example 3

[0049] (1) Add 30 kg of deionized water into a stirring kettle, add a cosolvent, a defoamer, a wetting agent, and then add 2 kg of dispersant A and 70 kg of nuclear titanium dioxide, and disperse at high speed for 30 minutes; then grind with a horizontal mill, there are 3 kinds of medium balls in the mill, the diameters of which are 5 mm, 3 mm, and 1.5 mm, respectively, and the 3 kinds of medium balls are mixed in a weight ratio of 1:1:1. The grinding speed is 600 rpm, the grinding temperature is controlled to be less than 70°C, and the slurry fineness -2um ≥ 98%.

[0050] (2) After grinding, add 2 kg of modified coating resin B, add 0.5 kg of thickener to the slurry, adjust the viscosity to 10000-20000 mpa.s, and control the fineness of the finished slurry to -2 um ≥ 98%.

[0051] Example 4

[0052] (1) Add 30 kg of deionized water into a stirring kettle, add a cosolvent, a defoamer, a wetting agent, and then add 2 kg of dispersant A and 70 kg of nuclear titanium dioxide, and disperse at high speed for 30 minutes; then grind with a horizontal mill, there are 3 kinds of medium balls in the mill, the diameters of which are 5 mm, 3 mm, and 1.5 mm, respectively, and the 3 kinds of medium balls are mixed in a weight ratio of 1:2:2, the grinding speed is 800 rpm, the grinding temperature is controlled to be less than 70°C, and the slurry fineness -2um ≥ 98%.

[0053] (2) After grinding, add 2 kg of modified coating resin B, add 0.5 kg of thickener to the slurry, adjust the viscosity to 10000-20000 mpa.s, and control the fineness of the finished slurry to -2 um ≥ 98%.

[0054] In the above Examples 1-4, the cosolvent is ethanol, the defoamer is BYK022, the wetting agent is BYK-346, the dispersant A is BYK190, and the coating resin B is THYON PH729.

[0055] A series of relevant performance tests were carried out on the products obtained in the above Examples 1-4, and the results are shown in the following table:

[0056]

[0057] In the technical solution of the present invention:

[0058] 1. Since the core titanium dioxide is made of a variety of inorganic powders interlaced, embedded and coated, the surface of the particles is very complex, with both positive and negative charge sites. The various active groups of positive and negative charges on the dispersant A are adsorbed on the core titanium dioxide crushed into fine particles and anchored, which greatly enhances the interaction between the core titanium dioxide and the dispersant.

[0059] 2. The amine, ammonium or quaternary ammonium group in dispersant A can form hydrogen bonds with a large number of hydroxyl groups generated on the surface of the core titanium dioxide particles during the grinding process, thereby producing an anchoring effect.

[0060] 3. The surface of nuclear titanium dioxide has polar or polarizable groups, and dispersant A also has polar or polarizable groups, so anchoring can also occur. This interaction is usually relatively weak, but the combined charge force and hydrogen bond force will strengthen this mutual effect.

[0061] 4. The coating resin B is a composite water-based acrylic resin with a special structure, and the solvated chain segments in the dispersant A extend in the coating resin B or the solvent, forming a barrier layer of solvated polymer segments of a certain thickness to prevent the aggregation and agglomeration between powder particles, making the core titanium dioxide particles smaller, thereby improving the gloss, improving the leveling, and enhancing the tinting strength and hiding power.

[0062] The above shows and describes the basic principles, main features and advantages of the present invention. It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and that the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention.

[0063] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A high-gloss universal water-based nuclear titanium dioxide slurry, It is characterized in that The contents of each component in parts by weight are as follows: 30 parts by weight of deionized water, 1-5 parts by weight of cosolvent, 0.3-0.5 parts by weight of defoamer, 0.3-0.5 parts by weight of wetting agent, 1-2 parts by weight of dispersant A, 1-5 parts by weight of coating resin B and 70 parts by weight of core titanium dioxide, and a certain amount of thickener is added to adjust to 10000-20000 mPa.s; The cosolvent is one or more of ethanol, propylene glycol, ethylene glycol butyl ether, and diethylene glycol monobutyl ether; the defoamer is one or more of BYK022, BYK028, TEGO901W, TEGO902W, NOPTAM-398, NOPTAM-1311, and SN-6024; The wetting agent is one or more of BYK-346, BYK-345, TEGO270, TEGO4100, SURFYNOL465, and SURFYNOL104E; the dispersant A is one or more of BYK190, BYK2055, NOPCALL-5180, DISPERS-755 W, SN-1710, and SN-1729; The coating resin B is one or more of THYON PH729, THYON SRT3069, THYON SR675, AD666, and AD8058; the core titanium dioxide is one or more of RTR201, RTR202, and RTR203.

2. A method for preparing a high-gloss universal water-based nuclear titanium dioxide slurry as claimed in claim 1, It is characterized in that The following steps are involved: S1, preparation of nuclear titanium dioxide fine raw material slurry: Add deionized water, cosolvent, dispersant A, defoamer and wetting agent into a stirring kettle in sequence and mix evenly. Add nuclear titanium dioxide and disperse at high speed for 20-30 minutes. Grind with a horizontal mill and adjust the particle size and proportion of the grinding medium balls. S2, preparation of finished slurry: The modified coating resin B is added to the fine raw material slurry of nuclear titanium dioxide, and the slurry obtained by grinding is sent to a stirring kettle, the speed is adjusted to 500-600 rpm, and a thickener is added to adjust the pressure to 10000-20000 mPa.s.

3. The method for preparing a high-gloss universal water-based nuclear titanium dioxide slurry according to claim 2, It is characterized in that The speed of the high-speed dispersion in S1 is 800-1200 rpm.

4. The method for preparing a high-gloss universal water-based nuclear titanium dioxide slurry according to claim 2, It is characterized in that In the S1, the particle size and the proportion of the grinding medium balls are adjusted so that the particle size of the nuclear titanium dioxide slurry is -2um≥90%.

5. The method for preparing a high-gloss universal water-based nuclear titanium dioxide slurry according to claim 2, It is characterized in that The particle size of the final finished slurry in S2 is -2um≥90%.

6. The method for preparing a high-gloss universal water-based nuclear titanium dioxide slurry according to claim 2, It is characterized in that The horizontal mill contains three kinds of medium balls, with diameters of 5 mm, 3 mm and 1.5 mm respectively. The three kinds of medium balls are mixed in a weight ratio of (1-3): (1-2): (1-2).

Citation Information

Patent Citations

  • Aqueous woodenware paint titanium white slurry and its preparation method

    CN103614005A

  • Modified titanium dioxide powder with coated polyacrylic acid

    CN105860592A