Modified lithium manganese iron phosphate positive electrode material and preparation method thereof, positive electrode sheet and battery
By introducing superlattice structures of titanium aluminum lithium and carbon into lithium manganese iron phosphate positive electrode material, the poor magnification and circulation performance of lithium manganese iron phosphate materials in lithium ion batteries are solved, and high lithium ion diffusion coefficient and Electronic conductivity improves the low-temperature performance of the battery.
Patent Information
- Application Number
- CN202410105625.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-25
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-01-25
AI Technical Summary
Lithium manganese iron phosphate materials show poor rate performance and poor cycle performance in lithium-ion battery applications, mainly due to their poor conductivity and ion conductivity, and manganese ions are prone to disproportionation reactions.
Modified lithium manganese phosphate positive electrode material, which includes a core of lithium manganese phosphate and a cladding layer. The core of lithium manganese phosphate has a superlattice structure formed by lithium manganese phosphate and aluminum titanium phosphate. In the cladding layer, Containing lithium titanium phosphate and carbon, it is prepared by mixing with polyvinylidene fluoride solution and calcining to form a material with high lithium ion diffusion coefficient and electron conductivity.
It improves the battery's low-temperature charging and discharging capabilities, ensures that the low-temperature charging does not eliminate lithium, and improves the constant current ratio of the low-temperature charging, significantly improving the material's conductivity and cycling performance.
Smart Images

Figure CN117936742B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of batteries, and in particular to a modified lithium manganese iron phosphate positive electrode material and a preparation method thereof, a positive electrode sheet and a battery. Background Art
[0002] With the application of lithium-ion batteries, commercial products have higher and higher requirements for the cost performance of lithium-ion batteries, which is mainly reflected in the increasingly fierce competition among battery manufacturers for the cost per watt-hour of batteries. In recent years, the market share of lithium iron phosphate has surpassed that of ternary batteries. On the one hand, it is because lithium iron phosphate is safer, and on the other hand, it is because the price of lithium iron phosphate is lower. With the development of material technology, lithium iron manganese phosphate has received more and more attention from the industry. Compared with lithium iron phosphate, lithium iron manganese phosphate has a similar gram capacity, but the voltage of lithium iron phosphate is higher than that of lithium iron phosphate, so the theoretical cost of lithium iron phosphate battery is lower than that of lithium iron phosphate, so the research on lithium iron phosphate by materials, batteries and vehicle manufacturers has gradually deepened.
[0003] Lithium manganese iron phosphate introduces manganese on the basis of lithium iron phosphate, so its electrical conductivity and ion conductivity are worse than those of lithium iron phosphate. In battery applications, it manifests as poor rate performance. In addition, manganese ions are prone to disproportionation reactions, resulting in poor material cycle performance.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] The purpose of the present application is to provide a modified lithium manganese iron phosphate positive electrode material and a preparation method thereof, a positive electrode sheet and a battery, so as to solve or improve the above-mentioned technical problems.
[0006] This application can be implemented as follows:
[0007] In the first aspect, the present application provides a modified lithium iron manganese phosphate positive electrode material, which includes a lithium iron manganese phosphate core and a coating layer coated on the outside of the lithium iron manganese phosphate core, the lithium iron manganese phosphate core has a superlattice structure formed by lithium iron manganese phosphate and lithium titanium aluminum phosphate; the coating in the coating layer includes lithium titanium aluminum phosphate and carbon.
[0008] In a second aspect, the present application provides a method for preparing a modified lithium iron manganese phosphate positive electrode material as described in the aforementioned embodiment, comprising the following steps: mixing a lithium iron manganese phosphate material having a superlattice structure formed by lithium iron manganese phosphate and lithium titanium aluminum phosphate with a polyvinylidene fluoride solution dispersed with lithium titanium aluminum phosphate to obtain a mixed solution; and calcining the mixed solution.
[0009] In an optional embodiment, the preparation of the lithium manganese iron phosphate material comprises: solid-phase mixing manganese iron oxide, aluminum titanium oxide, a lithium source and a phosphorus source, followed by solid-phase sintering.
[0010] In an alternative embodiment, the chemical formula of the manganese iron oxide is (Mn x Fe 1-x ) m O n , where 0<x<1, 1:1≤m:n≤1:2, 0 <n≤4;
[0011] Or, the chemical formula of aluminum titanium oxide is Al x Ti 2-x O k , where 0<x<2, k=4-0.5x;
[0012] Or, the lithium source includes at least one of lithium hydroxide and lithium carbonate;
[0013] Alternatively, the phosphorus source includes at least one of lithium dihydrogen phosphate and ammonium dihydrogen phosphate.
[0014] In an alternative embodiment, the molar weight of the manganese iron oxide is greater than the molar weight of the aluminum titanium oxide;
[0015] Alternatively, the average particle size of the manganese iron oxide is larger than the average particle size of the aluminum titanium oxide.
[0016] In an optional embodiment, the temperature of the solid phase sintering is 350-900° C., and the time of the solid phase sintering does not exceed 24 hours.
[0017] In an optional embodiment, the solvent in the polyvinylidene fluoride solution is N-methylpyrrolidone, and the weight percentage of polyvinylidene fluoride in the polyvinylidene fluoride solution does not exceed 20%;
[0018] Alternatively, the mass percentage of lithium aluminum titanium phosphate dispersed in the polyvinylidene fluoride solution does not exceed 10%.
[0019] In an optional embodiment, the weight of lithium aluminum titanium phosphate dispersed in the polyvinylidene fluoride solution is less than 20% of the weight of the lithium iron manganese phosphate material;
[0020] Alternatively, the average particle size of lithium aluminum titanium phosphate dispersed in the polyvinylidene fluoride solution is smaller than the average particle size of lithium iron manganese phosphate material.
[0021] In an optional embodiment, the calcination temperature is 300-800° C., and the calcination time does not exceed 24 hours.
[0022] In a third aspect, the present application provides a positive electrode sheet, wherein the slurry for preparing the positive electrode sheet contains the modified lithium manganese iron phosphate positive electrode material of the aforementioned embodiment.
[0023] In an optional embodiment, the slurry further contains at least one of a layered polyacid lithium positive electrode material, a spinel-type lithium manganese oxide positive electrode material, a layered manganese-rich lithium-based positive electrode material, an olivine-type lithium iron phosphate positive electrode material, and an olivine-type lithium manganese phosphate positive electrode material.
[0024] In a fourth aspect, the present application provides a battery comprising the positive electrode sheet of the aforementioned embodiment.
[0025] The beneficial effects of this application include:
[0026] The present application creatively proposes a modified lithium iron manganese phosphate positive electrode material, which includes a lithium iron manganese phosphate core and a coating layer coated on the outside of the lithium iron manganese phosphate core, the lithium iron manganese phosphate core has a superlattice structure formed by lithium iron manganese phosphate (LMFP) and lithium aluminum titanium phosphate (LATP); the coating in the coating layer includes lithium aluminum titanium phosphate and carbon.
[0027] In the above superlattice structure, lithium iron manganese phosphate and lithium titanium aluminum phosphate are chemically reacted to make the crystals grow uniformly into one. The coating layer is located outside the core, and in the coating layer, there is both a carbon layer and lithium titanium aluminum phosphate.
[0028] The modified lithium manganese iron phosphate positive electrode material having the above-mentioned specific structure has higher lithium ion diffusion coefficient and electronic conductivity.
[0029] A battery containing a positive electrode sheet further prepared from the modified lithium manganese iron phosphate positive electrode material has excellent low-temperature rate charging and discharging capabilities, and has the advantages of no lithium precipitation during low-temperature charging and a high constant current ratio during low-temperature charging. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0031] Figure 1 This is a schematic diagram of the general structure of the lithium manganese iron phosphate material with a superlattice structure prepared in Example 1 of the present invention;
[0032] Figure 2 This is a schematic diagram of the general structure of the modified lithium iron manganese phosphate material prepared in Example 1 of the present invention;
[0033] Figure 3 This is the XRD pattern of the modified lithium iron manganese phosphate material prepared in Example 1 of the present invention;
[0034] Figure 4This is the electron diffraction pattern of the modified lithium manganese iron phosphate material prepared in Example 1 of the present invention;
[0035] Figure 5 This is a TEM image of the modified lithium manganese iron phosphate material prepared in Example 1 of the present invention.
[0036] Icons: 10-lithium iron manganese phosphate material with superlattice structure; 11-first lithium titanium aluminum phosphate; 12-lithium iron manganese phosphate; 20-coating layer; 21-carbon; 22-second lithium titanium aluminum phosphate; 30-modified lithium iron manganese phosphate positive electrode material. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0038] The modified lithium manganese iron phosphate positive electrode material and its preparation method, positive electrode sheet and battery provided in this application are described in detail below.
[0039] The present application proposes a modified lithium iron manganese phosphate positive electrode material, which includes a lithium iron manganese phosphate core and a coating layer coated on the outside of the lithium iron manganese phosphate core, the lithium iron manganese phosphate core has a superlattice structure formed by lithium iron manganese phosphate (LMFP) and lithium aluminum titanium phosphate (LATP); the coating in the coating layer includes lithium aluminum titanium phosphate and carbon.
[0040] In the above superlattice structure, lithium iron manganese phosphate and lithium titanium aluminum phosphate are chemically reacted to make the crystals grow uniformly into one. The coating layer is located outside the core, that is, all the coating structures located outside the core are collectively referred to as the coating layer. In the present application, lithium titanium aluminum phosphate and carbon form the coating layer together. In other words, in the coating layer, there is both a carbon layer and lithium titanium aluminum phosphate.
[0041] As mentioned above, the modified lithium manganese iron phosphate positive electrode material with the above-mentioned specific structure provided in the present application has a higher lithium ion diffusion coefficient and electronic conductivity.
[0042] Correspondingly, the present application also provides a method for preparing the above-mentioned modified lithium iron manganese phosphate positive electrode material, comprising the following steps: mixing a lithium iron manganese phosphate material having a superlattice structure formed by lithium iron manganese phosphate and lithium titanium aluminum phosphate with a polyvinylidene fluoride solution dispersed with lithium titanium aluminum phosphate to obtain a mixed solution; and calcining the mixed solution.
[0043] For reference, the preparation of lithium manganese iron phosphate material includes: solid-phase mixing of manganese iron oxide, aluminum titanium oxide, lithium source and phosphorus source, followed by solid-phase sintering.
[0044] The chemical formula of the above manganese-iron oxide is (Mn x Fe 1-x ) m O n , where 0 < x < 1, 1:1 ≤ m:n ≤ 1:2, 0 < n ≤ 4. The manganese-iron oxide is obtained by solid-phase sintering of a manganese source and an iron source, where at least one of the manganese source and the iron source is an oxide. Exemplarily, the manganese source can be at least one of manganese tetroxide, manganese sesquioxide, manganese monoxide, manganese dioxide, manganese hydroxy oxide MnO(OH), hydrated manganese dioxide MnO(OH)2, manganese hydroxide Mn(OH)2, manganese sulfate, manganese carbonate, manganese oxalate, and manganese acetate. The iron source can be at least one of iron tetroxide, iron sesquioxide, ferrous oxide, basic iron oxide FeO(OH), iron hydroxide, ferrous hydroxide, ferrous sulfate, ferric sulfate, iron carbonate, iron oxalate, ferrous oxalate, iron acetate, and iron citrate.
[0045] The sintering temperature of the iron source and the manganese source can be 300 - 1200 °C, such as 300 °C, 500 °C, 800 °C, 1000 °C, or 1200 °C, etc. If the sintering temperature is too low, the reaction will not occur; if the sintering temperature is too high, it will cause energy waste.
[0046] The chemical formula of the above aluminum-titanium oxide is Al x Ti 2-x O k , where 0 < x < 2, k = 4 - 0.5x. The aluminum-titanium oxide is obtained by solid-phase sintering of an aluminum source and a titanium source, where at least one of the aluminum source and the titanium source is an oxide. Exemplarily, the aluminum source can include at least one of Al2O3, Al2O3·3H2O, Al2(CO3)3, AlOOH, Al(OH)3, Al2(SO4)3, and Al(NO3)3. The titanium source can include at least one of TiO2, H2TiO3, TiO, Ti3O5, Ti2O3, TiOSO4, TiO(OH)2, Ti2(SO4)3, TiSO4, H4TiO4, and Ti(NO3)4.
[0047] The sintering temperature of the aluminum source and the titanium source can be 900 - 1400 °C, such as 900 °C, 1000 °C, 1100 °C, 1200 °C, 1300 °C, or 1400 °C, etc. Similarly, if the sintering temperature is too low, the reaction will not occur; if the sintering temperature is too high, it will cause energy waste.
[0048] It should be noted that the manganese-iron oxide and aluminum-titanium oxide in this application can be prepared by oneself or directly purchased from the market.
[0049] The lithium source may include, by way of example but not limitation, at least one of lithium hydroxide and lithium carbonate. The phosphorus source may include, by way of example but not limitation, at least one of lithium dihydrogen phosphate and ammonium dihydrogen phosphate. Among them, lithium dihydrogen phosphate may be used as both a phosphorus source and a lithium source.
[0050] In the present application, the usage of ferromanganese oxide, aluminum-titanium oxide, lithium source and phosphorus source is in the following relationship: molar weight of Li in lithium source = molar weight of P in phosphorus source = molar weight of ferromanganese oxide + molar weight of aluminum-titanium oxide.
[0051] The molar weight of manganese iron oxide is greater than that of aluminum titanium oxide, and the average particle size of manganese iron oxide is greater than that of aluminum titanium oxide, so as to obtain a superlattice structure with lithium manganese iron phosphate as the main body.
[0052] In some embodiments, the average particle size of the manganese iron oxide may be 1 to 100 μm, and the average particle size of the aluminum titanium oxide may be 0.1 to 10 μm. Small-particle materials react more fully, but it is difficult to synthesize small-particle materials, which has very high requirements for sand mills and damages equipment. Large-particle materials are not easy to react fully, and the final material performance is poor.
[0053] For reference, the solid phase sintering temperature of manganese iron oxide, aluminum titanium oxide, lithium source and phosphorus source can be 350-900°C, such as 350°C, 500°C, 600°C, 700°C, 800°C or 900°C. The solid phase sintering time does not exceed 24h, such as 24h, 20h, 16h, 12h, 8h, 4h, etc. Too low sintering temperature will result in no reaction; too high sintering temperature and too long sintering time will not only cause energy waste, but also cause volatilization loss of lithium.
[0054] Furthermore, the lithium manganese iron phosphate material having the above superlattice structure is coated.
[0055] In the present application, the coating solution is a polyvinylidene fluoride solution dispersed with lithium aluminum titanium phosphate (LATP), wherein polyvinylidene fluoride (PVDF) can decompose during calcination to form a carbon coating layer, and lithium aluminum titanium phosphate is also coated on the outside of the lithium iron manganese phosphate material during the calcination process.
[0056] Exemplarily, the solvent in the polyvinylidene fluoride solution is N-methylpyrrolidone (NMP), and the weight percentage of polyvinylidene fluoride in the polyvinylidene fluoride solution does not exceed 20%, for example, it can be 20%, 15%, 10%, 8% or 5%, etc. The mass percentage of lithium aluminum titanium phosphate dispersed in the polyvinylidene fluoride solution does not exceed 10%, for example, it can be 10%, 8%, 6%, 4% or 2%, etc.
[0057] The weight of lithium aluminum titanium phosphate dispersed in the polyvinylidene fluoride solution is less than 20% of the weight of the lithium iron manganese phosphate material. The average particle size of the lithium aluminum titanium phosphate dispersed in the polyvinylidene fluoride solution is smaller than the average particle size of the lithium iron manganese phosphate material.
[0058] In some embodiments, the average particle size of the lithium aluminum titanium phosphate dispersed in the polyvinylidene fluoride solution can be 0.1 to 10 μm, and the average particle size of the lithium iron manganese phosphate material can be 1 to 100 μm. The average particle size of the lithium iron manganese phosphate material with good performance that is normally commercially available is 1 to 10 μm. Materials with too small particle sizes make it difficult to disperse and coat the lithium battery ingredients, and materials with too large particle sizes ultimately result in poor battery rate performance.
[0059] Through the above coating conditions, the conductivity of the modified lithium manganese iron phosphate positive electrode material can be improved while avoiding adverse effects on the capacity of the modified lithium manganese iron phosphate positive electrode material.
[0060] In the present application, the calcination temperature may be 300-800°C, such as 300°C, 400°C, 500°C, 600°C, 700°C or 800°C, etc., or any other value within the range of 300-800°C. The calcination time may not exceed 24h, such as 24h, 20h, 16h, 12h, 8h, 4h, etc. Too low a calcination temperature will result in no reaction; too high a calcination temperature and too long a calcination time will result in a waste of energy.
[0061] As mentioned above, the preparation method of the modified lithium iron manganese phosphate positive electrode material provided in the present application is simple, easy to operate, and has low cost, and can obtain a modified lithium iron manganese phosphate positive electrode material with better performance.
[0062] In addition, the present application also provides a positive electrode sheet, and the slurry for preparing the positive electrode sheet contains the above-mentioned modified lithium manganese iron phosphate positive electrode material.
[0063] For reference, the slurry for preparing the positive electrode sheet may also contain at least one of a layered polyacid lithium positive electrode material, a spinel lithium manganese oxide positive electrode material, a layered manganese-rich lithium-based positive electrode material, an olivine lithium iron phosphate positive electrode material, and an olivine lithium manganese phosphate positive electrode material.
[0064] The relationship between the amounts of various positive electrode materials used in the slurry is not limited here, and the total amount of positive electrode materials can refer to the conventional settings in the art.
[0065] Furthermore, the present application also provides a battery, which contains the above-mentioned positive electrode sheet.
[0066] The battery has excellent low-temperature rate charging and discharging capabilities. In addition, it has the advantages of no lithium precipitation during low-temperature charging and high constant current ratio during low-temperature charging.
[0067] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0068] Example 1
[0069] This embodiment provides a modified lithium manganese iron phosphate positive electrode material 30, and the preparation method thereof includes:
[0070] S1: Manganese iron oxide (Mn 0.9 Fe 0.6 )2O4) and aluminum titanium oxide (Al 0.3 Ti 1.7 O 3.85 ) and lithium dihydrogen phosphate solid phase mixed to obtain a first mixture.
[0071] The molar weight of aluminum titanium oxide is 10% of the molar weight of manganese iron oxide, and the molar weight of lithium dihydrogen phosphate is 110% of the molar weight of manganese iron oxide. 50 The average particle size of aluminum titanium oxide is larger than that of aluminum titanium oxide. 50 The average particle size D 50 1μm.
[0072] S2: The first mixture is solid-phase sintered at 900° C. for 12 h to obtain a lithium iron manganese phosphate material 10 having a superlattice structure formed by the lithium iron manganese phosphate 12 and the first lithium titanium aluminum phosphate 11 (SEM image as shown in FIG. Figure 1 shown).
[0073] S3: Add PVDF powder into NMP solution, set the solid content to 10%, and then stir to fully dissolve PVDF in NMP to obtain PVDF-NMP solution. Then stir the lithium manganese iron phosphate material obtained in S2 with the PVDF-NMP solution dispersed with the second lithium titanium aluminum phosphate 22 to obtain a mixed solution.
[0074] The average particle size D of the second lithium aluminum titanium phosphate 22 in the PVDF-NMP solution is 50 The average particle size D of the lithium manganese iron phosphate material 10 having a superlattice structure is smaller than that of the lithium manganese iron phosphate material 10. 50 The average particle size D 50 The mass percentage of the second lithium titanium aluminum phosphate 22 in the PVDF-NMP solution is 5%, and the weight of the second lithium titanium aluminum phosphate 22 in the PVDF-NMP solution is 10% of the weight of the lithium manganese iron phosphate material 10 having a superlattice structure.
[0075] S4: The mixed solution obtained in S3 was calcined at 800°C for 12 hours to obtain a modified lithium manganese iron phosphate positive electrode material 30 (SEM image as shown in FIG. Figure 2 shown).
[0076] The modified lithium iron manganese phosphate positive electrode material 30 includes a lithium iron manganese phosphate core (that is, a lithium iron manganese phosphate material 10 with a superlattice structure) and a coating layer 20 coated on the outside of the lithium iron manganese phosphate core. The lithium iron manganese phosphate core has a superlattice structure formed by lithium iron manganese phosphate 12 (LMFP) and a first lithium aluminum titanium phosphate 11 (LATP); the coating in the coating layer 20 includes a second lithium aluminum titanium phosphate 22 and carbon 21.
[0077] The X-ray diffraction (XRD) pattern of the lithium manganese iron phosphate material 10 with a superlattice structure prepared in this embodiment is characterized, and the results are as follows: Figure 3 As shown by Figure 3 It can be seen that based on the XRD spectrum of lithium manganese iron phosphate LMFP, the characteristic peaks I012 and I113 of LATP appear at around 15° and 24.5° respectively. The electron diffraction analysis of the above lithium manganese iron phosphate material is continued, and the results are as follows Figure 4 As shown by Figure 4 It can be seen that the white diamond area has a different crystal structure from other areas. Figure 3 and Figure 4 , it can be determined that the lithium manganese iron phosphate material has a superlattice structure.
[0078] The modified lithium manganese iron phosphate positive electrode material 30 prepared in this embodiment was subjected to TEM test, and the results are as follows: Figure 5 As shown by Figure 5 It can be seen that outside the superlattice structure body (the black area on the upper right), there is a coating carbon layer (the area indicated by the arrow) and another material coating (the box area), and the coating is LATP.
[0079] Example 2
[0080] S1: Manganese iron oxide (Mn 0.8 Fe 0.1 )2O4) is mixed with aluminum titanium oxide ((Al2Ti)O5) as well as lithium carbonate and diammonium dihydrogen phosphate in a solid phase to obtain a first mixture.
[0081] The molar weight of aluminum titanium oxide is 5% of the molar weight of manganese iron oxide, the molar weight of lithium carbonate Li2CO3 is 52.5% of the molar weight of manganese iron oxide, and the molar weight of ammonium dihydrogen phosphate is 105% of the molar weight of manganese iron oxide. The average particle size D of manganese iron oxide 50 The average particle size of the former is D 50 The average particle size D 50 0.1μm.
[0082] S2: solid-phase sintering the first mixture at 350° C. for 24 hours to obtain a lithium iron manganese phosphate material having a superlattice structure formed by lithium iron manganese phosphate and lithium titanium aluminum phosphate.
[0083] S3: Add PVDF powder into NMP solution, set the solid content to 8%, and then stir to fully dissolve PVDF in NMP to obtain PVDF-NMP solution. Then stir the lithium manganese iron phosphate material obtained in S2 with the PVDF-NMP solution dispersed with LATP to obtain a mixed solution.
[0084] The average particle size of LATP in PVDF-NMP solution is D 50 The average particle size of the lithium manganese iron phosphate material with a superlattice structure is smaller than that of the lithium manganese iron phosphate material with a superlattice structure. 50 The average particle size D 50 The mass percentage of LATP in the PVDF-NMP solution is 10%, and the weight of LATP in the PVDF-NMP solution is 5% of the weight of the lithium manganese iron phosphate material having a superlattice structure.
[0085] S4: calcining the mixed solution obtained in S3 at 300° C. for 24 hours to obtain a modified lithium manganese iron phosphate positive electrode material.
[0086] Example 3
[0087] S1: Manganese iron oxide (Mn 0.1 Fe 0.5 )2O4) and aluminum titanium oxide (Al 0.5 Ti 1.5 O 3.75 ) and lithium carbonate and diammonium phosphate solid phase are mixed to obtain a first mixture.
[0088] The molar weight of aluminum titanium oxide is 5% of the molar weight of manganese iron oxide, the molar weight of lithium carbonate Li2CO3 is 52.5% of the molar weight of manganese iron oxide, and the molar weight of ammonium dihydrogen phosphate is 105% of the molar weight of manganese iron oxide. The average particle size D of manganese iron oxide 50 The average particle size of the former is D 50 The average particle size D 50 is 10μm.
[0089] S2: solid-phase sintering the first mixture at 350° C. for 8 hours to obtain a lithium iron manganese phosphate material having a superlattice structure formed by lithium iron manganese phosphate and lithium titanium aluminum phosphate.
[0090] S3: Add PVDF powder into NMP solution, set the solid content to 8%, and then stir to fully dissolve PVDF in NMP to obtain PVDF-NMP solution. Then stir the lithium manganese iron phosphate material obtained in S2 with the PVDF-NMP solution dispersed with LATP to obtain a mixed solution.
[0091] The average particle size of LATP in PVDF-NMP solution is D 50 The average particle size of the lithium manganese iron phosphate material with a superlattice structure is smaller than that of the lithium manganese iron phosphate material with a superlattice structure. 50 The average particle size D 50 The mass percentage of LATP in the PVDF-NMP solution is 10%, and the weight of LATP in the PVDF-NMP solution is 5% of the weight of the lithium manganese iron phosphate material having a superlattice structure.
[0092] S4: calcining the mixed solution obtained in S3 at 300° C. for 8 h to obtain a modified lithium manganese iron phosphate positive electrode material.
[0093] Example 4
[0094] This embodiment provides a battery, and the preparation process thereof is as follows:
[0095] The binder PVDF is added to NMP in a mass ratio of 1:8 and stirred to obtain a glue solution, and then the modified lithium manganese iron phosphate positive electrode material, the conductive agent acetylene black, and the glue solution prepared in Example 1 are mixed in a mass ratio of 97:1:2, and stirred under the action of a vacuum mixer until the system is uniform to obtain a positive electrode slurry; the positive electrode slurry is evenly coated on the positive electrode collector, and after drying at room temperature, it is transferred to an oven for further drying, and then cold pressed and cut according to the required specifications to obtain a positive electrode sheet. The negative electrode active material graphite, the conductive agent acetylene black, the thickener CMC, and the binder SBR are mixed in a mass ratio of 96.2:0.8:1.2:1.8, and then the solvent deionized water is added to the mixture formed thereby, and stirred under the action of a vacuum mixer until the system is uniform to obtain a negative electrode slurry; the negative electrode slurry is evenly coated on the negative electrode collector, and after drying at room temperature, it is transferred to an oven for further drying, and then cold pressed and cut according to the required specifications to obtain a negative electrode sheet. The positive electrode sheet, the separator, and the negative electrode sheet are stacked in order to obtain a battery cell after assembly. The battery cell assembly is placed in the inner cavity of the battery shell, and after drying, an electrolyte is injected into the inner cavity of the battery shell. The electrolyte solvent is ethylene carbonate and the solute is lithium hexafluorophosphate (1 mol / L); after sealing, standing, forming, and volume separation, a square lithium-ion battery is obtained. The square battery has a capacity of 20Ah, a thickness of 15mm, a width of 119mm, and a height of 208mm.
[0096] Example 5
[0097] This embodiment provides a battery, which differs from Embodiment 4 in that: during the preparation process, the modified lithium iron manganese phosphate positive electrode material prepared in Embodiment 2 is used to replace the modified lithium iron manganese phosphate positive electrode material prepared in Embodiment 1.
[0098] Example 6
[0099] This embodiment provides a battery, which differs from Embodiment 4 in that: during the preparation process, the modified lithium iron manganese phosphate positive electrode material prepared in Embodiment 3 is used to replace the modified lithium iron manganese phosphate positive electrode material prepared in Embodiment 1.
[0100] Comparative Example 1
[0101] Referring to Example 1 of Chinese invention patent CN116364924A, a lithium iron manganese phosphate composite material was prepared. The lithium iron manganese phosphate composite material has a core-shell structure, consisting of an inner core and a coating layer coating the inner core, wherein the inner core is a lithium iron manganese phosphate material, and the coating layer consists of a carbon coating layer and a solid electrolyte coating layer.
[0102] The specific preparation process includes:
[0103] NH4H2PO4, FeC2O4·2H2O, Li2CO3, and MnCO3 are placed in a zirconia ball mill filled with anhydrous ethanol, and sodium oleate is added to the ball mill as a surfactant to promote subsequent ball milling mixing; the ball mill is started, and the material in the ball mill is ball milled at a rotation speed of 400 rpm for 8 hours to obtain a suspension; after filtering the above suspension, the insoluble matter is collected, and the above insoluble matter is vacuum dried at 80°C for 2 hours to obtain a precursor powder; then the above precursor powder and glucose are placed in a ball mill for grinding, and the mixture obtained after ball milling is placed in a reaction chamber of a tubular furnace, Ar is introduced into the tubular reaction chamber to provide inert atmosphere protection, the reaction chamber is heated to 650°C at a heating rate of 5°C / min, and is kept warm for 8 hours, and then the reaction chamber is cooled to room temperature, thereby preparing a carbon-coated lithium manganese iron phosphate material, marked as LMFP@carbon. The LMFP@carbon powder material obtained after the above operation and the LATP in the raw material are placed in a ball mill for grinding, and the mixture obtained after ball milling is placed in the reaction chamber of a tubular furnace. Ar is introduced into the reaction chamber to provide inert atmosphere protection, and the reaction chamber is heated to 650°C at a rate of 5°C / min and kept warm for 8 hours, thereby forming a solid electrolyte coating on the surface of LMFP@carbon; then the reaction chamber is cooled to room temperature, and the product obtained is marked as LMFP@carbon-LATP1.
[0104] Comparative Example 2
[0105] Referring to Example 3 of Chinese invention patent CN116364924A, a lithium iron manganese phosphate composite material was prepared. The lithium iron manganese phosphate composite material has a core-shell structure, consisting of an inner core and a coating layer coating the inner core, wherein the inner core is a lithium iron manganese phosphate material, and the coating layer consists of a carbon coating layer and a solid electrolyte coating layer.
[0106] The specific preparation process includes:
[0107] The NH4H2PO4, FeC2O4·2H2O, Li2CO3 and MnCO3 in the raw materials are placed in a zirconia ball mill filled with anhydrous ethanol, and sodium oleate is added to the ball mill as a surfactant to promote subsequent ball milling mixing; the ball mill is started, and the materials in the ball mill are ball milled at a speed of 400 rpm for 8 hours to obtain a suspension; the suspension is filtered and the insoluble matter is collected, and the insoluble matter is vacuum dried at 80°C for 2 hours to obtain a precursor The precursor powder is then placed in a ball mill for grinding, and the mixture obtained after ball milling is placed in a reaction chamber of a tubular furnace. Ar is introduced into the tubular reaction chamber to provide inert atmosphere protection, and the reaction chamber is first heated to 400°C at a rate of 5°C / min and kept warm for 1 hour, and then the reaction chamber is heated to 650°C at a rate of 5 / min and kept warm for 8 hours, and then the reaction chamber is cooled to room temperature, thereby preparing lithium manganese iron phosphate LMFP, which is used as the core of the lithium manganese iron phosphate composite material. The lithium manganese iron phosphate powder material core obtained according to the above operation and the glucose and commercial LATP in the raw materials are placed in a ball mill for grinding, and the mixture obtained after ball milling is placed in the reaction chamber of a tubular furnace. Ar is introduced into the reaction chamber to provide inert atmosphere protection, and the reaction chamber is heated to 650°C at a rate of 5°C / min and kept warm for 8 hours, thereby forming a coating layer composed of carbon material and LATP on the surface of the lithium manganese iron phosphate; then the reaction chamber is cooled to room temperature, and the product obtained is marked as LMFP@carbon-LATP2.
[0108] Comparative Example 3
[0109] Referring to Example 3 of Chinese invention patent CN116364924A, a lithium iron manganese phosphate composite material was prepared. The lithium iron manganese phosphate composite material has a core-shell structure, consisting of an inner core and a coating layer coating the inner core, wherein the inner core is a lithium iron manganese phosphate material, and the coating layer consists of a carbon coating layer and a solid electrolyte coating layer.
[0110] The specific preparation process includes:
[0111] The NH4H2PO4, FeC2O4·2H2O, Li2CO3 and MnCO3 in the raw materials are placed in a zirconia ball mill filled with anhydrous ethanol, and sodium oleate is added to the ball mill as a surfactant to promote subsequent ball milling mixing; the ball mill is started, and the materials in the ball mill are ball milled at a speed of 400 rpm for 8 hours to obtain a suspension; the suspension is filtered and the insoluble matter is collected, and the insoluble matter is vacuum dried at 80°C for 2 hours to obtain a precursor The precursor powder is then placed in a ball mill for grinding, and the mixture obtained after ball milling is placed in the reaction chamber of a tubular furnace, Ar is introduced into the tubular reaction chamber to provide inert atmosphere protection, and the reaction chamber is first heated to 400°C at a rate of 5°C / min, and kept warm for 1 hour, and then the reaction chamber is heated to 650°C at a rate of 5 / min, and kept warm for 8 hours, and then the reaction chamber is cooled to room temperature, thereby preparing lithium manganese iron phosphate LMFP, which is used as the core of the lithium manganese iron phosphate composite material. The core of the lithium manganese iron phosphate powder material obtained according to the above operation and the glucose in the raw material are placed in a ball mill for grinding, and the mixture obtained after ball milling is placed in the reaction chamber of a tubular furnace, Ar is introduced into the reaction chamber to provide inert atmosphere protection, and the reaction chamber is heated to 650°C at a rate of 5°C / min, and kept warm for 8 hours, thereby forming a coating layer composed of carbon material on the surface of the lithium manganese iron phosphate; then the reaction chamber is cooled to room temperature, and the product obtained is marked as LMFP@carbon.
[0112] Comparative Example 4
[0113] Referring to Example 3 of Chinese invention patent CN116364924A, a lithium iron manganese phosphate composite material was prepared. The lithium iron manganese phosphate composite material has a core-shell structure, consisting of an inner core and a coating layer coating the inner core, wherein the inner core is a lithium iron manganese phosphate material, and the coating layer consists of a carbon coating layer and a solid electrolyte coating layer.
[0114] The specific preparation process includes:
[0115] The NH4H2PO4, FeC2O4·2H2O, Li2CO3 and MnCO3 in the raw materials are placed in a zirconia ball mill filled with anhydrous ethanol, and sodium oleate is added to the ball mill as a surfactant to promote subsequent ball milling mixing; the ball mill is started, and the materials in the ball mill are ball milled at a speed of 400 rpm for 8 hours to obtain a suspension; the suspension is filtered and the insoluble matter is collected, and the insoluble matter is vacuum dried at 80°C for 2 hours to obtain a precursor The precursor powder is then placed in a ball mill for grinding, and the mixture obtained after ball milling is placed in the reaction chamber of a tube furnace, Ar is introduced into the tube reaction chamber to provide inert atmosphere protection, and the reaction chamber is first heated to 400°C at a rate of 5°C / min, and kept warm for 1 hour, and then the reaction chamber is heated to 650°C at a rate of 5 / min, and kept warm for 8 hours, and then the reaction chamber is cooled to room temperature, thereby preparing lithium manganese iron phosphate LMFP, which is used as the core of the lithium manganese iron phosphate composite material. The lithium manganese iron phosphate powder material core obtained according to the above operation and commercial LATP are placed in a ball mill for grinding, and the mixture obtained after ball milling is placed in the reaction chamber of a tube furnace, Ar is introduced into the reaction chamber to provide inert atmosphere protection, and the reaction chamber is heated to 650°C at a rate of 5°C / min, and kept warm for 8 hours, thereby forming a coating layer composed of LATP on the surface of the lithium manganese iron phosphate; then the reaction chamber is cooled to room temperature, and the product obtained is marked as LMFP@LATP.
[0116] Comparative Example 5
[0117] S1: Manganese iron oxide (Mn 0.8 Fe 0.1 )2O4) is mixed with aluminum titanium oxide ((Al2Ti)O5) as well as lithium carbonate and diammonium dihydrogen phosphate in a solid phase to obtain a first mixture.
[0118] The molar weight of aluminum titanium oxide is 5% of the molar weight of manganese iron oxide, the molar weight of lithium carbonate Li2CO3 is 52.5% of the molar weight of manganese iron oxide, and the weight of ammonium dihydrogen phosphate is 105% of the molar weight of manganese iron oxide. The average particle size D of manganese iron oxide 50 The average particle size of aluminum titanium oxide is larger than that of aluminum titanium oxide. 50 The average particle size D 50 is 20μm.
[0119] S2: solid-phase sintering the first mixture at 350° C. for 24 hours to obtain a lithium iron manganese phosphate material having a superlattice structure formed by lithium iron manganese phosphate and lithium titanium aluminum phosphate.
[0120] S3: Add PVDF powder into NMP solution, set the solid content to 8%, and then stir to fully dissolve PVDF in NMP to obtain PVDF-NMP solution. Then stir the lithium manganese iron phosphate material obtained in S2 with the PVDF-NMP solution dispersed with LATP to obtain a mixed solution.
[0121] The average particle size of LATP in PVDF-NMP solution is D 50 The average particle size of the lithium manganese iron phosphate material with a superlattice structure is smaller than that of the lithium manganese iron phosphate material with a superlattice structure. 50 The average particle size D 50 The mass percentage of LATP in the PVDF-NMP solution is 10%, and the weight of LATP in the PVDF-NMP solution is 5% of the weight of the lithium manganese iron phosphate material having a superlattice structure.
[0122] S4: calcining the mixed solution obtained in S3 at 300° C. for 24 hours to obtain a modified lithium manganese iron phosphate positive electrode material.
[0123] Comparative Example 6
[0124] This comparative example provides a battery, which differs from Example 4 in that during the preparation process, the lithium manganese iron phosphate composite material prepared in Comparative Example 1 replaces the modified lithium manganese iron phosphate positive electrode material prepared in Example 1.
[0125] Comparative Example 7
[0126] This comparative example provides a battery, which differs from Example 4 in that during the preparation process, the lithium manganese iron phosphate composite material prepared in Comparative Example 2 replaces the modified lithium manganese iron phosphate positive electrode material prepared in Example 1.
[0127] Comparative Example 8
[0128] This comparative example provides a battery, which differs from Example 4 in that during the preparation process, the lithium manganese iron phosphate composite material prepared in Comparative Example 3 replaces the modified lithium manganese iron phosphate positive electrode material prepared in Example 1.
[0129] Comparative Example 9
[0130] This comparative example provides a battery, which differs from Example 4 in that during the preparation process, the lithium manganese iron phosphate composite material prepared in Comparative Example 4 replaces the modified lithium manganese iron phosphate positive electrode material prepared in Example 1.
[0131] Comparative Example 10
[0132] This comparative example provides a battery, which differs from Example 4 in that during the preparation process, the lithium manganese iron phosphate composite material prepared in Comparative Example 5 replaces the modified lithium manganese iron phosphate positive electrode material prepared in Example 1.
[0133] Test example
[0134] The modified lithium iron manganese phosphate positive electrode material obtained in Examples 1-3 and the lithium iron manganese phosphate composite material obtained in Comparative Examples 1-5 were tested for lithium ion diffusion coefficient and electron conductivity, wherein the lithium ion diffusion coefficient was tested with reference to the "Industry Standard "Test Method for Lithium Ion Diffusion Coefficient of Lithium Ion Battery Materials" (2022-1337T-SJ)", and the electron conductivity was tested using a conductivity meter, and the results are shown in Table 1.
[0135] The 45°C, 1C cycle performance and low-temperature discharge performance of the four batteries obtained in Examples 4-6 and Comparative Examples 6-10 were tested. The battery was charged and discharged at room temperature (25±5)°C to obtain a discharge capacity C1; then the battery was fully charged at room temperature, and then the battery was placed in a -10°C environment, and discharged after standing for 4 hours to obtain a discharge capacity C2. C2 / C1×100% is the low-temperature performance. The test results are shown in Table 2.
[0136] Table 1 Test results
[0137] <![CDATA[Lithium ion diffusion coefficient (cm 2 / s)]]> Electronic conductivity (S / cm) Example 1 <![CDATA[1.5×10 -9 ]]> <![CDATA[1.1×10 -6 ]]> Example 2 <![CDATA[1.4×10 -9 ]]> <![CDATA[1.0×10 -6 ]]> Example 3 <![CDATA[1.2×10 -9 ]]> <![CDATA[1.2×10 -6 ]]> Comparative Example 1 <![CDATA[8.2×10 -10 ]]> <![CDATA[7.4×10 -7 ]]> Comparative Example 2 <![CDATA[8.7×10 -10 ]]> <![CDATA[7.8×10 -7 ]]> Comparative Example 3 <![CDATA[7.3×10 -10 ]]> <![CDATA[6.0×10 -7 ]]> Comparative Example 4 <![CDATA[7.5×10 -10 ]]> <![CDATA[6.1×10 -7 ]]> Comparative Example 5 <![CDATA[9.5×10 -10 ]]> <![CDATA[8.8×10 -7 ]]>
[0138] Table 2 Test results
[0139]
[0140] It can be seen from Table 1 and Table 2 that compared with Comparative Examples 1 and 2, the lithium ion diffusion coefficient of lithium manganese iron phosphate materials in Examples 1, 2 and 3 is increased by 70%, and the electronic conductivity is increased by 30%. Compared with Comparative Example 2, the lithium ion diffusion coefficient and electronic conductivity of LMFP@carbon and LMFP@LATP in Comparative Examples 3 and 4 are worse than those of LMFP@carbon-LATP2. Compared with Example 2, after increasing the particle size of lithium manganese iron oxide, aluminum titanium oxide, LATP and LMFP materials, the lithium ion diffusion coefficient and electronic conductivity of the materials in Comparative Example 5 are significantly reduced.
[0141] In terms of the capacity retention rate of the battery after 1500 cycles at high temperature, Examples 4, 5 and 6 are slightly better than Comparative Examples 7 and 8. Comparative Example 10, in which the particle sizes of manganese iron lithium oxide, aluminum titanium oxide, LATP and LMFP materials are increased, is slightly lower than Examples 4, 5 and 6. However, the cycles of Comparative Examples 8 and 9 are the worst.
[0142] The low temperature discharge performance of the battery, Example 4, Example 5 and Example 6 are improved by 20% compared with Comparative Example 6 and Comparative Example 7. Compared with Comparative Example 7, the low temperature discharge performance of LMFP@carbon and LMFP@LATP in Comparative Example 8 and Comparative Example 9 is worse than that of LMFP@carbon-LATP2. Comparative Example 10, in which the particle sizes of manganese iron lithium oxide, aluminum titanium oxide, LATP and LMFP materials are increased, is slightly lower than that of Example 4, Example 5 and Example 6.
[0143] The battery was charged at a constant current and constant voltage rate of 0.1C at -10°C. Examples 4, 5 and 6 had a higher constant current ratio, which was increased by about 20 compared with Comparative Examples 6 and 7. Comparative Examples 8 and 9 showed that the low temperature charging performance of LMFP@Carbon and LMFP@LATP was worse than that of LMFP@Carbon-LATP2.
[0144] The batteries of Example 4, Example 5, Example 6 and Comparative Example 10 had no lithium deposition at the low-temperature charging interface at -10°C. However, the batteries of Comparative Example 6, Comparative Example 7, Comparative Example 8 and Comparative Example 9 had lithium deposition at the low-temperature charging interface.
[0145] In summary, the modified lithium manganese iron phosphate material provided in the present application has the characteristics of high lithium ion diffusion coefficient and high electronic conductivity. The battery made of this material has excellent low-temperature rate charging and discharging capabilities, no lithium precipitation during low-temperature charging, and high constant current ratio during low-temperature charging.
[0146] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A modified lithium manganese iron phosphate positive electrode material, characterized in that: The modified lithium iron manganese phosphate positive electrode material comprises a lithium iron manganese phosphate core and a coating layer coated on the outside of the lithium iron manganese phosphate core, wherein the lithium iron manganese phosphate core has a superlattice structure formed by lithium iron manganese phosphate and lithium titanium aluminum phosphate; the coating in the coating layer comprises lithium titanium aluminum phosphate and carbon; The preparation of the modified lithium manganese iron phosphate positive electrode material comprises the following steps: Mixing a lithium iron manganese phosphate material having a superlattice structure formed by lithium iron manganese phosphate and lithium titanium aluminum phosphate with a polyvinylidene fluoride solution dispersed with lithium titanium aluminum phosphate to obtain a mixed solution; and calcining the mixed solution; The preparation of the lithium manganese iron phosphate material comprises: solid-phase mixing of manganese iron oxide, aluminum titanium oxide, lithium source and phosphorus source, followed by solid-phase sintering.
2. A method for preparing the modified lithium manganese iron phosphate positive electrode material according to claim 1, characterized in that: The method comprises the following steps: mixing a lithium manganese iron phosphate material having a superlattice structure formed by lithium manganese iron phosphate and lithium titanium aluminum phosphate with a polyvinylidene fluoride solution dispersed with lithium titanium aluminum phosphate to obtain a mixed solution; and calcining the mixed solution; The preparation of the lithium manganese iron phosphate material comprises: solid-phase mixing of manganese iron oxide, aluminum titanium oxide, lithium source and phosphorus source, followed by solid-phase sintering.
3. The preparation method according to claim 2, characterized in that: The chemical formula of the manganese iron oxide is (Mn x Fe 1-x ) m O n , where 0<x<1, 1:1≤m:n≤1:2, 0 <n≤4; Or, the chemical formula of the aluminum titanium oxide is Al x Ti 2-x O k , where 0<x<2, k=4-0.5x; Or, the lithium source includes at least one of lithium hydroxide and lithium carbonate; Alternatively, the phosphorus source includes at least one of lithium dihydrogen phosphate and ammonium dihydrogen phosphate.
4. The preparation method according to claim 2 or 3, characterized in that: The molar weight of the manganese iron oxide is greater than the molar weight of the aluminum titanium oxide; Alternatively, the average particle size of the manganese iron oxide is greater than the average particle size of the aluminum titanium oxide.
5. The preparation method according to claim 2, characterized in that: The temperature of solid phase sintering is 350-900°C, and the time of solid phase sintering does not exceed 24h.
6. The preparation method according to claim 2, characterized in that: The solvent in the polyvinylidene fluoride solution is N-methylpyrrolidone, and the weight percentage of the polyvinylidene fluoride in the polyvinylidene fluoride solution does not exceed 20%; Alternatively, the mass percentage of the lithium aluminum titanium phosphate dispersed in the polyvinylidene fluoride solution does not exceed 10%.
7. The preparation method according to claim 6, characterized in that: The weight of the lithium aluminum titanium phosphate dispersed in the polyvinylidene fluoride solution is less than 20% of the weight of the lithium iron manganese phosphate material; Alternatively, the average particle size of the lithium aluminum titanium phosphate dispersed in the polyvinylidene fluoride solution is smaller than the average particle size of the lithium iron manganese phosphate material.
8. The preparation method according to claim 2, characterized in that: The calcination temperature is 300-800°C, and the calcination time does not exceed 24 hours.
9. A positive electrode sheet, characterized in that: The slurry for preparing the positive electrode sheet contains the modified lithium manganese iron phosphate positive electrode material according to claim 1.
10. The positive electrode sheet according to claim 9, characterized in that: The slurry also contains at least one of a layered polyacid lithium positive electrode material, a spinel-type lithium manganate positive electrode material, a layered manganese-rich lithium-based positive electrode material, an olivine-type lithium iron phosphate positive electrode material, and an olivine-type lithium manganese phosphate positive electrode material.
11. A battery, characterized in that: The battery contains the positive electrode sheet according to claim 9 or 10.