A negative electrode active material and a negative electrode sheet containing the same, and a lithium battery.
By controlling the particle size, aspect ratio, and orientation of the first artificial graphite material, the volume expansion problem of lithium-ion battery anode materials during charging and discharging was solved, achieving high specific capacity and low cycle expansion, thus improving the energy density and dynamic performance of lithium batteries.
Patent Information
- Application Number
- CN202410058107.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-15
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-01-15
AI Technical Summary
The existing graphite anode material for lithium-ion batteries suffers from deterioration in cycle performance and capacity decay due to volume expansion during charging and discharging, especially in power batteries.
Using first-generation artificial graphite with suitable particle size, aspect ratio, and orientation degree as the negative electrode active material, by controlling its particle size to be 11-15 μm, aspect ratio to be 1.5-2.0:1, and orientation degree OI value to be 2.0-2.5, and combining pre-carbonization, graphitization, and liquid-phase coating carbonization treatment, a negative electrode active material with high specific capacity and low cycle expansion is prepared.
This technology achieves high specific capacity and low cycle expansion of the negative electrode active material, improving the energy density and kinetic performance of lithium batteries, reducing the expansion of the electrode during cycling, and improving the cycle stability and fast charging performance of the battery.
Smart Images

Figure BDA0004666113060000101 
Figure BDA0004666113060000111 
Figure BDA0004666113060000112
Abstract
Description
Technical Field
[0001] This invention belongs to the field of lithium battery technology, specifically relating to a negative electrode active material and a negative electrode sheet containing the same, and a lithium battery. Background Technology
[0002] Graphite possesses excellent properties such as high capacity and high compaction, making it a common anode material in lithium-ion batteries. However, during the charge and discharge process of lithium-ion batteries, graphite exhibits a volume expansion effect, which fails to meet the actual requirements of power batteries. This is because, during charge and discharge, the insertion and extraction of lithium ions within the anode material alters the interlayer structure of graphite, causing a series of problems such as increased internal stress and electrode rebound. Simultaneously, excessive consumption of the SEI film at the interlayer interface of graphite leads to electrolyte decomposition and a reduction in active lithium ions, resulting in deterioration of battery cycle performance and capacity decay. Therefore, it is urgent to overcome the shortcomings of existing technologies and develop an anode active material with low cycle expansion. Summary of the Invention
[0003] The purpose of this invention is to provide a negative electrode active material and a negative electrode sheet and lithium battery containing the same. The negative electrode active material has the advantages of high specific capacity and low cycle expansion, enabling the lithium battery containing the same to have both excellent energy density and kinetic performance.
[0004] According to one aspect of the present invention, a negative electrode active material is provided, comprising a first artificial graphite, wherein the first artificial graphite is a secondary particle, the aspect ratio of the first artificial graphite is 1.5 to 2.0:1, the particle size D50 of the first artificial graphite is 11 to 15 μm, and the orientation degree OI value of the first artificial graphite is 2.0 to 2.5; the orientation degree OI value is the ratio of the peak area of the 004 characteristic diffraction peak to the peak area of the 110 characteristic diffraction peak in the XRD diffraction pattern of the first artificial graphite. In the negative electrode active material provided by this invention, the first artificial graphite is a secondary particle with a suitable particle size and needle-like morphology. It has a suitable specific surface area, which can reduce the side reactions of the electrolyte on its surface and reduce the expansion of the electrode during cycling. At the same time, the first artificial graphite has a suitable orientation degree (OI) value, which can ensure the isotropy of the graphite particles and disperse the expansion generated by the graphite particles during lithium intercalation in all directions, thus mitigating the degradation of the negative electrode and battery performance caused by uneven local expansion. Based on this, the first artificial graphite that meets the above conditions can achieve a high compaction density after rolling, thereby increasing the specific capacity of the negative electrode. In summary, by simultaneously controlling the particle size, aspect ratio, and orientation degree of the first artificial graphite, this invention can give it the advantages of high specific capacity and low cycle expansion, thus enabling lithium batteries containing it to have both excellent energy density and kinetic performance.
[0005] If the orientation degree (OI) value of the first artificial graphite is too high, it is difficult to ensure the isotropy of the graphite particles, and the graphite particles will expand in volume during the cycle. If the orientation degree (OI) value of the first artificial graphite is too low, the graphite particles will be arranged in a disordered manner, which is not conducive to the utilization of its capacity.
[0006] Preferably, the preparation method of the first artificial graphite includes the following operations: S1. Using needle coke as raw material, mixing the binder with the raw material and granulating to obtain a semi-finished product; S2. Pre-carbonizing the semi-finished product to obtain a precursor; S3. Graphitizing the precursor to obtain graphitized particles; S4. Liquid-phase coating and carbonizing the graphitized particles with a coating agent to obtain the first artificial graphite. The above preparation method uses needle coke as raw material. Needle coke has the advantages of high compaction and high capacity. By pre-carbonizing, graphitizing, and liquid-phase coating carbonization of the raw material, the first artificial graphite obtained can fully utilize its high specific capacity advantage while further improving its kinetic properties.
[0007] Preferably, the pre-carbonization temperature is ≥1000℃. Low-temperature pre-carbonization before graphitization helps remove volatiles, ensuring the subsequent graphitization effect and improving safety.
[0008] Preferably, the adhesive includes at least one of medium-temperature asphalt, high-temperature asphalt, and epoxy resin.
[0009] Preferably, the granulation temperature is 850–950°C.
[0010] Preferably, the graphitization temperature is 2800–3200℃. By controlling the graphitization temperature, the specific capacity of the artificial graphite particles can be fully utilized.
[0011] Preferably, the carbonization temperature is ≥900℃.
[0012] Preferably, the needle coke has a particle size ≤ 8 μm and a tap density ≥ 0.8 g / cm³. 3 By further limiting the particle size and tap density of needle coke, the kinetic properties of the first artificial graphite produced can be further improved while ensuring that the raw material can fully utilize its high specific capacity advantage.
[0013] Preferably, the coating agent includes at least two of epoxy resin, phenolic resin, medium-temperature pitch, and coal tar. Using the above-mentioned coating agent for coating helps improve the uniformity and density of the coating layer, while also helping to improve surface defects of the coating layer and enhance the structural stability and cycle stability of the first artificial graphite.
[0014] Preferably, the mixture further includes a second artificial graphite, wherein the mass ratio of the first artificial graphite to the second artificial graphite is 50-60:40-50; the second artificial graphite includes artificial graphite A and artificial graphite B, wherein artificial graphite A is a primary particle with a particle size D50 of 8-10 μm and a graphitization degree of 91.5%-93%, and artificial graphite B is a secondary particle with a particle size D50 of 11-14 μm and a graphitization degree of 93%-94%. The second artificial graphite, composed of a mixture of artificial graphite A and artificial graphite B, exhibits excellent fast-charging performance and lithium-ion kinetic transport characteristics. By mixing the second artificial graphite with the first artificial graphite in a specific ratio, the two can fully exert their synergistic effect, so that the resulting negative electrode active material has the advantages of both the first and second artificial graphite. This allows for further improvement of the fast charging performance and lithium-ion transport dynamics of the negative electrode while ensuring its high specific capacity and low cycle expansion.
[0015] Preferably, the tap density of artificial graphite A is 0.95–1.05 g / cm³. 3 .
[0016] According to another aspect of the present invention, a negative electrode sheet is provided, comprising a negative electrode current collector and a negative electrode active coating disposed on the surface of the negative electrode current collector, the negative electrode active coating comprising the aforementioned negative electrode active material.
[0017] Preferably, the areal density of the negative electrode active coating is ≥20 μm. 2 / g. At a low areal density, the negative electrode can maintain a high specific capacity while ensuring a high ion and electron diffusion rate, thereby further improving the kinetic performance of the battery.
[0018] Preferably, the compaction density of the negative electrode active coating is ≥1.8 g / cm³. 3 By rationally setting the compaction density of the negative electrode active coating, the negative electrode active particles in the coating are evenly distributed, which helps to suppress the stress expansion of the negative electrode active particles, promote electron conduction and ion transport, and thus further improve its kinetic characteristics while ensuring the high specific capacity of the negative electrode sheet.
[0019] According to another aspect of the present invention, a lithium battery is provided, comprising the aforementioned negative electrode. The battery provided by the present invention possesses both excellent energy density and kinetic performance. Detailed Implementation
[0020] To enable those skilled in the art to better understand the technical solutions of this invention, the technical solutions of this invention will be clearly and completely described below in conjunction with the embodiments of this invention. Obviously, the described embodiments are only some embodiments of this invention, and not all embodiments. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of this invention.
[0021] Example 1
[0022] This embodiment provides a lithium battery, the preparation method of which includes the following steps:
[0023] 1. Preparation of negative electrode sheet
[0024] S1. Preparation of the first artificial graphite:
[0025] (1) Take high-quality needle coke as raw material; crush and classify the raw material, then mix the binder high-temperature asphalt with the raw material at a mass ratio of 20:100, and granulate in a granulating axe (granulation temperature 850℃, time 7h) to obtain a semi-finished product.
[0026] (2) Heat the semi-finished product to 1000℃ for pre-carbonization treatment for 6 hours;
[0027] (3) The powder obtained after pre-carbonization is heated to 3200℃ for graphitization treatment to obtain graphitized particles C;
[0028] (4) The graphitized particles C were sieved, and the coating agent (epoxy resin, medium-temperature asphalt) was mixed with the graphitized particles C at a mass ratio of 4:100 to coat the graphitized particles C in the liquid phase. Then, the mixture was heated to 1200℃ and carbonized for 7 hours to obtain the first artificial graphite. The first artificial graphite is a secondary particle with an aspect ratio of 1.7:1, a particle size D50 of 13.5 μm, and an orientation degree OI value of 2.3.
[0029] S2, Preparation of the second type of artificial graphite:
[0030] (1) Preparation of artificial graphite A: A particle size D50 of 6 μm and a true density of 2.3 g / cm³ were prepared. 3 Petroleum coke aggregate was used as raw material. The raw material was heated to 3100℃ for graphitization treatment to obtain graphitized particles A. Epoxy resin, a coating agent, was mixed with graphitized particles A at a mass ratio of 5:100 to coat the particles A. Then, the mixture was heated to 1200℃ for carbonization for 7 hours to obtain artificial graphite A. Artificial graphite A consisted of primary particles with a particle size D50 of 9.5 μm, a graphitization degree of 92%, and a tap density of 1.03 g / cm³. 3 .
[0031] (2) Preparation of artificial graphite B: A particle size D50 of 8 μm and a tap density of 0.75 g / cm³ were prepared. 3 Using calcined needle coke (a type of oil-based material) as raw material, medium-temperature pitch (a binder) is mixed with the raw material and granulated in a granulator (granulation temperature 950℃, time 7h) to obtain a semi-finished product. The semi-finished product is then heated to 3150℃ for graphitization treatment to obtain graphitized particles B. Epoxy resin, a coating agent, is mixed with graphitized particles B at a mass ratio of 4.5:100 to coat the graphitized particles B, and then the mixture is heated to 1000℃ for carbonization for 6h to obtain artificial graphite B. Artificial graphite B is a secondary particle with a particle size D50 of 12.5μm and a graphitization degree of 93%.
[0032] (3) Mix the above-mentioned artificial graphite A and artificial graphite B at a mass ratio of 30:70 to obtain the second artificial graphite.
[0033] S4. Preparation of negative electrode active material:
[0034] The first artificial graphite and the second artificial graphite were mixed at a mass ratio of 50:50 to obtain the negative electrode active material of this embodiment.
[0035] S5, Preparation of the negative electrode sheet
[0036] 97.4% of the negative electrode active material and 0.3% of the conductive carbon black were mixed evenly, and then a CMC adhesive solution (CMC content of 1.1%) was added and stirred evenly. Next, 1.2% of SBR was added and stirred evenly to obtain the negative electrode slurry. The negative electrode slurry was then coated onto copper foil and dried in a vacuum environment at 100°C for 12 hours to obtain the negative electrode sheet.
[0037] 2. Preparation of the positive electrode sheet
[0038] The positive electrode active material (lithium cobalt oxide), conductive agent SP, and binder PVDF are mixed evenly in a mass ratio of 94:3:3 and dispersed in NMP to obtain a positive electrode slurry. The positive electrode slurry is coated on aluminum foil and dried in a vacuum environment at 85°C for 24 hours to obtain a positive electrode sheet.
[0039] 3. Preparation of electrolyte
[0040] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed in a volume ratio of 1:1:1 to obtain an organic solvent. Then, fully dried lithium salt LiPF6 was dissolved in the organic solvent to prepare an electrolyte with a concentration of 1 mol / L.
[0041] 4. Selection of diaphragm
[0042] The diaphragm is made of polyethylene film.
[0043] 5. Assembly and formation of lithium batteries
[0044] The positive electrode, separator, and negative electrode are stacked in sequence, with the separator acting as a separator between the positive and negative electrodes. Then, they are wound to obtain a bare cell. The bare cell is placed in an outer packaging shell, dried, and then injected with the electrolyte. After vacuum sealing, standing, formation, and volume determination, a lithium battery is obtained.
[0045] Example 2
[0046] This embodiment refers to the preparation of a lithium battery in Example 1. The difference between this embodiment and Example 1 is that the negative electrode active material used in this embodiment only includes the first type of artificial graphite. Apart from the above differences, the materials and process operations used in this embodiment are strictly consistent with those in Example 1.
[0047] Example 3
[0048] This embodiment refers to the preparation of a lithium battery in Example 1. The difference between this embodiment and Example 1 is that the mass ratio of the first artificial graphite to the second artificial graphite in the negative electrode active material used in this embodiment is 40:60. Apart from the above difference, the materials and process operations used in this embodiment are strictly consistent with those in Example 1.
[0049] Example 4
[0050] This embodiment refers to the preparation of a lithium battery in Example 1. The difference between this embodiment and Example 1 is that the mass ratio of the first artificial graphite to the second artificial graphite in the negative electrode active material used in this embodiment is 60:40. Apart from the above difference, the materials and process operations used in this embodiment are strictly consistent with those in Example 1.
[0051] Example 5
[0052] This embodiment refers to the preparation of a lithium battery in Example 1. The difference between this embodiment and Example 1 is that the mass ratio of the first artificial graphite to the second artificial graphite in the negative electrode active material used in this embodiment is 70:30. Apart from the above difference, the materials and process operations used in this embodiment are strictly consistent with those in Example 1.
[0053] Example 6
[0054] This embodiment refers to the preparation of a lithium battery in Example 1. The difference between this embodiment and Example 1 is that the second artificial graphite in the negative electrode active material used in this embodiment only includes artificial graphite A. Apart from the above difference, the materials and process operations used in this embodiment are strictly consistent with those in Example 1.
[0055] Example 7
[0056] This embodiment refers to the preparation of a lithium battery in Example 1. The difference between this embodiment and Example 1 is that the second artificial graphite in the negative electrode active material used in this embodiment only includes artificial graphite B. Apart from the above difference, the materials and process operations used in this embodiment are strictly consistent with those in Example 1.
[0057] Example 8
[0058] This embodiment refers to the preparation of a lithium battery in Example 1. The difference between this embodiment and Example 1 is that the aspect ratio of the first artificial graphite in the negative electrode active material used in this embodiment is 1.5:1, the particle size D50 is 11 μm, and the orientation degree OI value is 2.0. Apart from the above differences, the materials and process operations used in this embodiment are strictly consistent with those in Example 1.
[0059] The preparation method of the first artificial graphite includes the following steps:
[0060] (1) Take high-quality needle coke with a polarized structure as raw material; crush and classify the raw material to make the aggregate particle size 6-7μm; then mix the binder high temperature asphalt with the raw material at a mass ratio of 1:100 and granulate in a granulating axe (granulation temperature 850℃, time 7h) to obtain a semi-finished product.
[0061] (2) Heat the semi-finished product to 1000℃ for pre-carbonization treatment for 6 hours;
[0062] (3) The powder obtained after pre-carbonization is heated to 3200℃ for graphitization treatment to obtain graphitized particles C;
[0063] (4) The graphitized particles C are screened, and the coating agent (epoxy resin, medium temperature asphalt) is mixed with the graphitized particles C at a mass ratio of 5.5:100 to coat the graphitized particles C in the liquid phase. Then the temperature is raised to 1200℃ for carbonization for 7 hours to obtain the first artificial graphite.
[0064] Example 9
[0065] This embodiment refers to the preparation of a lithium battery in Example 1. The difference between this embodiment and Example 1 is that the aspect ratio of the first artificial graphite in the negative electrode active material used in this embodiment is 2.0:1, the particle size D50 is 15μm, and the orientation degree OI value is 2.5. Apart from the above differences, the materials and process operations used in this embodiment are strictly consistent with those in Example 1.
[0066] The preparation method of the first artificial graphite includes the following steps:
[0067] (1) Take high-quality needle coke with a fibrous structure rich in polarized components as raw material; crush and classify the raw material, and then mix the binder high-temperature asphalt with the raw material at a mass ratio of 15.5:100, and granulate it in a granulator (granulation temperature 850℃, time 8h) to obtain a semi-finished product.
[0068] (2) Heat the semi-finished product to 1000℃ for pre-carbonization treatment for 6 hours;
[0069] (3) The powder obtained after pre-carbonization is heated to 3100℃ for graphitization treatment to obtain graphitized particles C;
[0070] (4) The graphitized particles C are screened, and the coating agent (epoxy resin, medium temperature asphalt) is mixed with the graphitized particles C at a mass ratio of 3.5:100 to coat the graphitized particles C in the liquid phase. Then the temperature is raised to 1200℃ for carbonization for 7 hours to obtain the first artificial graphite.
[0071] Comparative Example 1
[0072] This comparative example uses a lithium battery prepared according to Example 1. The difference between this comparative example and Example 1 is that the particle size D50 of the first artificial graphite in the negative electrode active material used in this example is 9.5 μm. Apart from the above difference, the materials and process operations used in this example are strictly consistent with those in Example 1.
[0073] Comparative Example 2
[0074] This comparative example uses a lithium battery prepared according to Example 1. The difference between this comparative example and Example 1 is that the particle size D50 of the first artificial graphite in the negative electrode active material used in this example is 16.5 μm. Apart from the above difference, the materials and process operations used in this example are strictly consistent with those in Example 1.
[0075] Comparative Example 3
[0076] This comparative example uses a lithium battery prepared according to Example 1. The difference between this comparative example and Example 1 is that the aspect ratio of the first artificial graphite in the negative electrode active material used in this example is 1.3:1, and the particle size D50 = 14 μm. Apart from the above differences, the materials and process operations used in this example are strictly consistent with those in Example 1.
[0077] The preparation method of the first artificial graphite includes the following steps:
[0078] (1) Take isotropic coke with an inlaid structure as raw material; crush and classify the raw material, then mix the binder high temperature asphalt with the raw material at a mass ratio of 13:100, and granulate in a granulating axe (granulation temperature 850℃, time 7h, stirring rate 14HZ (300Kg axe)) to obtain a semi-finished product.
[0079] (2) Heat the semi-finished product to 1000℃ for pre-carbonization treatment for 6 hours;
[0080] (3) The powder obtained after pre-carbonization is heated to 3200℃ for graphitization treatment to obtain graphitized particles C;
[0081] (4) The graphitized particles C are screened, and the coating agent (epoxy resin, medium temperature asphalt) is mixed with the graphitized particles C at a mass ratio of 4:100 to coat the graphitized particles C in the liquid phase. Then the temperature is raised to 1200℃ for carbonization for 7 hours to obtain the first artificial graphite.
[0082] Comparative Example 4
[0083] This comparative example uses a lithium battery prepared according to Example 1. The difference between this comparative example and Example 1 is that the aspect ratio of the first artificial graphite in the negative electrode active material used in this example is 2.2:1. Apart from the above difference, the materials and process operations used in this example are strictly consistent with those in Example 1.
[0084] (1) Take the highly oriented coal-series needle coke with fibrous structure as raw material; crush and classify the raw material, and then mix the binder high temperature asphalt with the raw material at a mass ratio of 15.7:100, and granulate it in a granulation axe (granulation temperature 850℃, time 7h, stirring rate 19HZ (300Kg axe)) to obtain a semi-finished product.
[0085] (2) Heat the semi-finished product to 1000℃ for pre-carbonization treatment for 6 hours;
[0086] (3) The powder obtained after pre-carbonization is heated to 3200℃ for graphitization treatment to obtain graphitized particles C;
[0087] (4) The graphitized particles C are screened, and the coating agent (epoxy resin, medium temperature asphalt) is mixed with the graphitized particles C at a mass ratio of 4:100 to coat the graphitized particles C in the liquid phase. Then the temperature is raised to 1200℃ for carbonization for 7 hours to obtain the first artificial graphite.
[0088] Comparative Example 5
[0089] This comparative example uses a lithium battery prepared according to Example 1. The difference between this comparative example and Example 1 is that the orientation degree (OI) of the first artificial graphite in the negative electrode active material used in this example is 3.5. Apart from the above difference, the materials and process operations used in this example are strictly consistent with those in Example 1.
[0090] (1) Take high-orientation needle coke as raw material; crush and shape the raw material, then mix the binder high-temperature asphalt with the raw material at a mass ratio of 16:100, and granulate in a granulating axe (granulation temperature 850℃, time 7h, stirring rate 18HZ (300Kg axe)) to obtain a semi-finished product.
[0091] (2) Heat the semi-finished product to 1000℃ for pre-carbonization treatment for 6 hours;
[0092] (3) The powder obtained after pre-carbonization is heated to 3200℃ for graphitization treatment to obtain graphitized particles C;
[0093] (4) The graphitized particles C are screened, and the coating agent (epoxy resin, medium temperature asphalt) is mixed with the graphitized particles C at a mass ratio of 4:100 to coat the graphitized particles C in the liquid phase. Then the temperature is raised to 1200℃ for carbonization for 7 hours to obtain the first artificial graphite.
[0094] Comparative Example 6
[0095] This comparative example uses a lithium battery prepared according to Example 1. The difference between this comparative example and Example 1 is that the orientation degree (OI) of the first artificial graphite in the negative electrode active material used in this example is 1.8. Apart from the above difference, the materials and process operations used in this example are strictly consistent with those in Example 1.
[0096] (1) Take highly anisotropic needle coke as raw material; crush and shape the raw material, then mix the binder high temperature asphalt with the raw material at a mass ratio of 13:100, and granulate in a granulating axe (granulation temperature 850℃, time 7h, stirring rate 15HZ (300Kg axe)) to obtain a semi-finished product.
[0097] (2) Heat the semi-finished product to 1000℃ for pre-carbonization treatment for 6 hours;
[0098] (3) The powder obtained after pre-carbonization is heated to 3200℃ for graphitization treatment to obtain graphitized particles C;
[0099] (4) The graphitized particles C are screened, and the coating agent (epoxy resin, medium temperature asphalt) is mixed with the graphitized particles C at a mass ratio of 4:100 to coat the graphitized particles C in the liquid phase. Then the temperature is raised to 1200℃ for carbonization for 7 hours to obtain the first artificial graphite.
[0100] Test Example 1
[0101] 1. Test subject:
[0102] Examples 1-9 and Comparative Examples 1-6 were used as the test subjects in this test case.
[0103] 2. Test items:
[0104] (1) Specific capacity: The specific capacity of the half-cell test material was used. The button cell was made according to the standard graphite button cell installation steps. The actual specific capacity of the graphite material was obtained through testing. The charging and discharging modes were: DC: 0.6mA to 5.0mV, 0.06mA to 5.0mV, CC: 0.6mA to 2.0V.
[0105] (2) Fast charging performance: The battery was tested for 3C direct charging using the Xinwei test cabinet. The cutoff voltage was 4.48V and the cutoff current was 0.025C. The ratio of the 3C direct charging capacity collected by the test cabinet to the total charging capacity is the 3C charging current ratio.
[0106] (3) Capacity retention and volume expansion rate during cycling at different temperatures:
[0107] 1) Room temperature cycling: 1C constant current and constant voltage charging to 4.48V, cutoff at 0.025C, test the initial thickness of the battery; then at 25℃: ① rest for 1 min; ② 1C constant current discharge to 3.0V; ③ rest for 5 min; ④ 3C constant current and constant voltage charging to 4.48V, cutoff at 0.025C; ⑤ rest for 5 min; ⑥ 1C constant current discharge to 3.0V; ⑦ rest for 5 min; ⑧ repeat ④-⑦ cycles for 800 cycles; ⑨ 1.0C constant current and constant voltage charging to 4.48V, cutoff at 0.025C.
[0108] The battery's full-charge thickness was measured after 800 cycles. The ratio of the full-charge thickness after 800 cycles to the initial thickness is the volume expansion rate. The ratio of the remaining capacity after 800 cycles to the discharge capacity of the first cycle is the capacity retention rate.
[0109] 2) 45℃ cycle: The process is the same as in 1), except that it needs to be carried out in a 45℃ constant temperature chamber and tested up to 600 cycles.
[0110] 3) 15℃ cycle: The process is the same as in 1), except that it needs to be carried out in a 15℃ constant temperature chamber and tested up to 400 cycles.
[0111] 3. Test Results:
[0112] Table 1. Relevant parameters of Examples 1-9 and Comparative Examples 1-6
[0113]
[0114]
[0115] Table 2. Relevant parameters of Examples 1-9 and Comparative Examples 1-6
[0116]
[0117]
[0118] The test results are shown in Tables 1 and 2. The performance test results of Example 1 were compared with those of Comparative Examples 1 to 6. Table 1 shows that, under the same conditions of other materials and operations used in battery preparation, the negative electrode active material obtained in Example 1 had a higher specific capacity and a lower volume expansion rate. In contrast, the first artificial graphite used in Comparative Example 1 had a particle size D50 < 11 μm, resulting in a lower specific capacity of the negative electrode active material and a higher volume expansion rate. The first artificial graphite used in Comparative Example 2 had a particle size > 15 μm, resulting in a higher volume expansion rate than that of Example 1. The first artificial graphite used in Comparative Example 3 had an aspect ratio < 1.5:1. The specific capacity of the resulting negative electrode active material is lower than that of Example 1, while the volume expansion rate of the battery is higher than that of Example 1. In Comparative Example 4, the aspect ratio of the first artificial graphite used is >2:1, resulting in a higher volume expansion rate of the battery than that of Example 1. In Comparative Example 5, the orientation degree OI value of the first artificial graphite used is >2.5, resulting in a higher volume expansion rate of the battery than that of Example 1. In Comparative Example 6, the orientation degree OI value of the first artificial graphite used is <2, resulting in a lower specific capacity of the resulting negative electrode active material and a higher volume expansion rate of the battery than that of Example 1. This demonstrates that, compared to Comparative Examples 1-6, the battery provided in Example 1, by simultaneously controlling the particle size, aspect ratio, and orientation degree of the first artificial graphite in the negative electrode active material, can achieve the advantages of high specific capacity and low cycle expansion of the first artificial graphite.
[0119] The performance test results of Example 1 and Example 2 were compared. Table 1 shows that, under the same conditions of other materials and operations in battery preparation, Example 2 did not include second artificial graphite in its negative electrode active material. Therefore, the cycle expansion rate of the battery obtained was higher than that of Example 1, and its fast-charging performance was lower. This indicates that, compared to Example 2, the battery provided in Example 1, by using both second artificial graphite A and second artificial graphite B as negative electrode active materials, suppressed battery expansion during cycling and improved the battery's fast-charging performance.
[0120] The performance test results of Example 1 were compared with those of Examples 3-5. Table 1 shows that, under the same conditions of other materials and operations in battery preparation, the mass ratio of first artificial graphite to second artificial graphite in the negative electrode active material used in Example 3 was <50-60:40-50, resulting in a slightly higher volume expansion rate than Example 1. In Example 5, the mass ratio of first artificial graphite to second artificial graphite in the negative electrode active material was >50-60:40-50, resulting in a slightly higher cycle expansion rate and slightly lower fast-charging performance than Example 1. This indicates that, compared to Examples 3 and 5, the batteries provided in Examples 1 and 4, by reasonably setting the mass ratio of first artificial graphite to second artificial graphite in the negative electrode active material, allow the first and second artificial graphite to work synergistically, thereby further improving the fast-charging performance and lithium-ion transport kinetics of the battery while ensuring the high specific capacity and low volume expansion of the first artificial graphite.
[0121] The performance test results of Example 1 were compared with those of Examples 6 and 7. Table 1 shows that, under the same conditions of other materials and operations in battery preparation, the second artificial graphite used in Example 6 contained only artificial graphite A, resulting in a lower specific capacity of the negative electrode active material and a higher cycle expansion rate than in Example 1. Similarly, the second artificial graphite used in Example 7 contained only artificial graphite B, resulting in a higher cycle expansion rate and lower fast-charging performance than in Example 1. This indicates that, compared to Examples 6 and 7, the battery provided in Example 1, by using a second artificial graphite composed of artificial graphite A and artificial graphite B as the negative electrode active material, allows the first and second artificial graphites to work synergistically, combining the advantages of both. This reduces the cycle expansion of the negative electrode active material, increases its specific capacity, and improves the battery's fast-charging performance and lithium-ion transport kinetics.
[0122] The above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention, but such modifications or substitutions are all within the scope of protection of the present invention.
Claims
1. A negative electrode active material, characterized in that, It includes a first artificial graphite and a second artificial graphite with a mass ratio of 50~60:40~50; the first artificial graphite is a secondary particle, the aspect ratio of the first artificial graphite is 1.5~2.0:1, the particle size D50 of the first artificial graphite is 11~15μm, and the orientation degree OI value of the first artificial graphite is 2.0~2.
5. The orientation degree OI value is the ratio of the peak area of the 004 characteristic diffraction peak to the peak area of the 110 characteristic diffraction peak in the XRD diffraction pattern of the first artificial graphite. The second artificial graphite includes artificial graphite A and artificial graphite B. The artificial graphite A is a primary particle with a particle size D50 of 8~10 μm and a degree of graphitization of 91.5%~92%. The artificial graphite B is a secondary particle with a particle size D50 of 11~14μm and a degree of graphitization of 93%~94%.
2. The negative electrode active material as described in claim 1, characterized in that, The preparation method of the first artificial graphite includes the following operations: S1. Using needle coke as raw material, the binder is mixed with the raw material and granulated to obtain a semi-finished product; S2. The semi-finished product is subjected to pre-carbonization treatment to obtain a precursor; S3. The precursor is graphitized to obtain graphitized particles; S4. The graphitized particles are coated in liquid phase and carbonized using a coating agent to obtain the first artificial graphite.
3. The negative electrode active material as described in claim 2, characterized in that, The needle coke has a particle size ≤ 8 μm and a tap density ≥ 0.8 g / cm³. 3 .
4. The negative electrode active material as described in claim 2, characterized in that, The coating agent includes at least two of epoxy resin, phenolic resin, medium-temperature pitch, and coal tar.
5. The negative electrode active material as described in claim 1, characterized in that, The tap density of the artificial graphite A is 0.95~1.05 g / cm³. 3 .
6. A negative electrode sheet, characterized in that, It includes a negative electrode current collector and a negative electrode active coating disposed on the surface of the negative electrode current collector, wherein the negative electrode active coating includes the negative electrode active material as described in any one of claims 1 to 5.
7. The negative electrode sheet as described in claim 6, characterized in that, The areal density of the negative electrode active coating is ≥20m³. 2 / g.
8. The negative electrode sheet as described in claim 6, characterized in that, The compaction density of the negative electrode active coating is ≥1.8 g / cm³. 3 .
9. A lithium battery, characterized in that, Includes the negative electrode sheet as described in any one of claims 6 to 8.
Citation Information
Patent Citations
Artificial graphite negative-pole material, preparation method therefor and lithium-ion battery
CN110642247A
Electric storage device
CN114144906A
Negative active material, method for preparing same, secondary battery, and device comprising secondary battery
CN114223072A