A method for preparing selenium-enriched modified biochar, selenium-enriched modified biochar and its applications
Selenium-enriched modified biochar was prepared by hydrothermal carbonization, which solved the problems of high cost and insufficient adsorption capacity of selenium-modified biochar, and achieved efficient adsorption and fixation of arsenic, making it suitable for the remediation of arsenic pollutants and plant cultivation.
Patent Information
- Application Number
- CN202410093649.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-23
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-01-23
AI Technical Summary
The preparation cost of selenium-modified biochar in existing technologies is high and it is difficult to promote. Traditional methods have insufficient adsorption capacity for arsenic and are difficult to effectively fix arsenic pollutants.
Selenium-enriched modified biochar was prepared by heating and carbonizing selenium-enriched biomass. The specific methods included high-temperature carbonization and hydrothermal carbonization. Hydrothermal carbonization was preferred to retain the selenium content and functional groups on the surface of the biochar. After pulverization, the biochar was sieved to obtain selenium-enriched modified biochar of suitable size.
It significantly improves the adsorption effect of arsenic, reduces the preparation cost, and achieves efficient fixation and adsorption of arsenic pollutants. It is suitable for the remediation of arsenic-containing water bodies and soils and reduces the absorption and translocation of arsenic by plants.
Smart Images

Figure CN117945388B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of biochar preparation technology, and in particular to a method for preparing selenium-enriched modified biochar, the selenium-enriched modified biochar and its applications. Background Technology
[0002] Arsenic (As) is a toxic nonmetal that exists naturally worldwide. The inorganic form of arsenic is considered highly toxic, causing serious environmental problems. It has a strong bioaccumulation property and is harmful to organisms. It has been identified by the European Union as a highly hazardous toxic substance and a carcinogen. Arsenic has toxic, non-biodegradable, persistent, bioaccumulative, and potentially carcinogenic properties. It can accumulate in the human body through the food chain, drinking water, and other pathways, posing a serious threat to human health and the environment.
[0003] Some studies have shown that biochar has the ability to immobilize As (As) in water and soil. In existing technologies, biomass prepared from waste materials that can be used to adsorb As(V) and As(III) includes: oak, corn stalks, perennial grasses, hybrid poplar, pine bark, and rice husks. In fact, biochar has been successfully applied in the in-situ remediation of groundwater and soil, where it can immobilize arsenic in the soil, improve soil health, and is an environmentally friendly method for fixing carbon in soil. Therefore, biochar is a promising carbon material for arsenic remediation and has received considerable attention as a treatment medium. Biochar itself possesses excellent physical / chemical surface properties (porous structure and high specific surface area), associated with a high density of active surface functional groups.
[0004] However, while biochar possesses a strong ability to immobilize heavy metal cations (arsenic) but a relatively low adsorption capacity for anionic arsenic, it is necessary to modify it to improve its adsorption performance. Modified biochar is considered a novel method for inducing and promoting As adsorption or surface immobilization. Currently, the traditional approach to selenium-modified biochar involves direct blending, as illustrated in patent CN201910114450.6, which discloses a method for reducing the enrichment of inorganic mercury and methylmercury in rice using sodium selenite-modified biochar. This method involves dissolving sodium selenite in water, adding low-temperature dried biochar, stirring and mixing, and then drying to obtain sodium selenite-modified biochar. This method is costly and difficult to promote, and research on the adsorption mechanism of arsenic using selenium-modified biochar remains lacking both domestically and internationally. Summary of the Invention
[0005] The main objective of this invention is to provide a method for preparing selenium-enriched modified biochar, the selenium-enriched modified biochar and its applications, aiming to improve the technical problems of high cost and difficulty in promotion of existing selenium-modified biochars which use direct blending.
[0006] To achieve the above objectives, this invention proposes a method for preparing selenium-enriched modified biochar, comprising the following steps:
[0007] S1. Selenium-enriched biomass is heated and carbonized to obtain selenium-enriched biochar;
[0008] S2. The selenium-enriched biochar is pulverized and then sieved to obtain the selenium-enriched modified biochar.
[0009] The aforementioned selenium-enriched biomass (such as selenium-enriched rice straw) is pretreated by spraying selenium-enriched foliar fertilizer during the key growth stages of rice (tillering and grain-filling stages). The main component of the selenium-enriched foliar fertilizer includes organic selenium, with a concentration of 5 g / L. After harvesting the rice, the rice straw is collected. The selenium content of the selenium-enriched rice straw used in this scheme is 481.3 ug / kg. According to the standard (DB / T 22499—2008), a selenium content of 0.04–0.30 mg / kg is acceptable for selenium-enriched rice. Therefore, the selenium content of the selenium-enriched rice used in this scheme can be above 0.04 mg / kg.
[0010] This invention directly prepares selenium-enriched modified biochar from selenium-enriched biomass (selenium-enriched straw) through heating and carbonization. The resulting selenium-enriched modified biochar effectively immobilizes arsenic through multiple mechanisms, significantly improving the removal efficiency of arsenic from wastewater or soil. By using selenium-enriched biomass as a carrier to immobilize selenium in biochar, increasing selenium stability, this not only provides a new possibility for the resource utilization of straw but also offers a new approach to arsenic remediation. Compared to traditional sodium selenite-modified biochar, the selenium-enriched biochar obtained by this method exhibits better arsenic removal performance.
[0011] Preferably, the heating carbonization includes high-temperature carbonization or hydrothermal carbonization. There are various carbonization methods for preparing selenium-enriched biochar from selenium-enriched biomass; this scheme selects either high-temperature carbonization or hydrothermal carbonization. Compared to hydrothermal carbonization, high-temperature carbonization results in the decomposition or loss of raw materials during high-temperature pyrolysis, leading to a lower selenium content in the final selenium-enriched biochar, and most of the retained selenium is ineffective, resulting in relatively low preparation efficiency. Hydrothermal carbonization, on the other hand, yields selenium-enriched biochar with better overall performance. During pyrolysis, it significantly retains the content and availability of selenium in the biochar, exhibiting better adsorption performance in the subsequent arsenic adsorption process.
[0012] Preferably, during hydrothermal carbonization, the selenium-enriched biomass is mixed with water and then subjected to a hydrothermal reaction at 150-250℃ for 8-12 hours. The heating rate during the hydrothermal reaction is 5-10℃ / min. After the hydrothermal carbonization is completed, the hydrothermal product is washed until neutral and dried to obtain the selenium-enriched biochar. The solid-liquid ratio of the selenium-enriched biomass to water is 1:5-8.
[0013] The specific steps of hydrothermal carbonization are as described above. Under the constraints of the above parameters, the selenium-enriched biochar obtained has a high selenium content, and the functional groups on the surface of the biochar are also preserved to the maximum extent. The type, quantity and position of the functional groups of biochar will affect the adsorption effect of biochar on heavy metals (arsenic). Therefore, the above hydrothermal carbonization steps effectively protect the performance of selenium-enriched biochar and enable it to maximize its adsorption effect.
[0014] In addition, the selenium-enriched biochar obtained using the above-mentioned hydrothermal carbonization parameters has a porous characteristic, and the pores of the prepared selenium-enriched biochar are evenly distributed and relatively uniform in size. The biochar has small pores on its side, which increases the pore area and makes the selenium-enriched modified biochar have a high adsorption rate when adsorbing arsenic.
[0015] Preferably, the drying temperature is 105-115℃, and the drying time is 10-12 hours. The drying process can remove moisture from the selenium-enriched biochar, ensuring that the selenium-enriched modified biochar has a good adsorption effect on arsenic.
[0016] Preferably, the heating temperature during high-temperature carbonization is 350-750℃, and the heating time is 2-4 hours. When using high-temperature carbonization, the heating temperature should not be too high, otherwise it will easily lead to the loss of selenium during the high-temperature pyrolysis of selenium-enriched biomass. The high-temperature carbonization temperature set in this scheme is limited to below 550℃ as much as possible, so that the obtained selenium-enriched biochar can retain a relatively higher selenium content and has a better adsorption effect on arsenic.
[0017] Preferably, the size of the selenium-enriched biochar after pulverization is 0.05-0.3 mm. Since selenium-enriched biochar may aggregate after heating and carbonization, it needs to be pulverized before use. The size of the pulverized selenium-enriched biochar is 0.05-0.3 mm. Selenium-enriched biochar with this size can further improve the stability of the adsorption effect of selenium-enriched modified biochar on arsenic when the concentration fluctuates.
[0018] Preferably, the selenium-enriched biomass is crushed before heating and carbonization, and the size of the crushed selenium-enriched biomass is 7-8 cm. In order to ensure that the selenium-enriched biochar after heating and carbonization has better adsorption characteristics, this method pre-crushes the selenium-enriched biomass to obtain selenium-enriched biochar with a size of 7-8 cm. This size better reduces the loss of selenium elements in the straw during the carbonization process, and at the same time prevents uneven carbonization during heating and carbonization, which would affect the quality of the selenium-enriched biochar.
[0019] Preferably, the selenium-enriched biomass is selenium-enriched straw. In this solution, the selenium-enriched biomass is rice straw, but it can also be selenium-enriched straw from other crops or selenium-enriched rice husks, etc.
[0020] In addition, this invention also proposes a selenium-enriched modified biochar, prepared by any of the methods described above. The selenium-enriched modified biochar prepared by the above methods has the same beneficial effects as those methods, and will not be elaborated further here.
[0021] This invention also proposes an application of the above-mentioned selenium-enriched modified biochar in the adsorption of arsenic in water or soil. In the prior art, arsenic is an anionic substance, such as arsenate or arsenite. Due to the influence of the negative surface charge, biochar's adsorption effect on arsenic is poor. However, the selenium-enriched modified biochar obtained through the above modification steps can be used as an adsorbent for arsenic-polluted water or soil, exhibiting improved adsorption performance and inducing and promoting the adsorption or surface immobilization of As.
[0022] This invention also proposes the application of selenium-enriched modified biochar in the cultivation of plants in arsenic-containing aquatic bodies. Plants that can be cultivated include root, stem, and leaf plants such as water spinach. Besides the adsorption effect of selenium-enriched modified biochar on arsenic itself, since plants absorb and transport selenium and arsenic in the same way, this method, by using selenium for modification, can increase the adsorption performance of the selenium-enriched modified biochar. Simultaneously, by utilizing the elemental absorption competition relationship, it can also reduce the absorption and transport of arsenic by plants, allowing plants to absorb selenium, which is more beneficial to their growth.
[0023] Compared with the prior art, the preparation method of selenium-enriched modified biochar and the obtained selenium-enriched modified biochar of the present invention have the following beneficial effects:
[0024] 1. This scheme uses selenium-enriched biomass (such as the straw left over after planting selenium-enriched rice) as the main raw material for preparing selenium-enriched biochar. This can reduce the input of sodium selenite, save costs, and also realize the recycling and reuse of agricultural waste, which is energy-saving and environmentally friendly.
[0025] 2. The selenium-enriched modified biochar obtained by this scheme through hydrothermal method and high-temperature carbonization both have a certain adsorption effect on arsenic. However, after comparing the hydrothermal method and high-temperature carbonization, it was determined that the hydrothermal method can effectively retain the selenium content and can more effectively improve the adsorption effect on arsenic in sewage or harmful soil compared with high-temperature carbonization. Moreover, since it is a low-temperature hydrothermal carbonization, the entire preparation process consumes less energy and the reaction is milder than the traditional high-temperature carbonization preparation method, which meets the low-carbon requirements.
[0026] 3. The selenium-enriched modified biochar in this solution is particularly suitable for use when planting plants in arsenic-polluted water bodies. Since plants absorb and transport selenium and arsenic in the same way, when selenium-enriched biomass is modified by heating and carbonization, the adsorption performance of the selenium-enriched modified biochar can be increased. At the same time, by utilizing the element absorption competition relationship, the absorption and transport of arsenic by plants can be reduced, further reducing the absorption effect of arsenic by plants. Attached Figure Description
[0027] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.
[0028] Figure 1 This is a summary chart of the selenium content of the selenium-enriched biomass in this scheme and the selenium-enriched modified biochar obtained under different preparation methods.
[0029] Figure 2 Scanning electron microscope images of selenium-enriched modified biochar obtained by different preparation methods;
[0030] Figure 3 Infrared scans of selenium-enriched modified biochar obtained under different preparation methods;
[0031] Figure 4 A summary graph of the arsenic adsorption capacity of selenium-enriched modified biochar obtained under different preparation methods at 120 min;
[0032] Figure 5 This is a summary chart showing the arsenic content in the roots, stems, and leaves of plants harvested after using selenium-enriched modified biochar prepared under different methods in arsenic-containing wastewater for plant cultivation.
[0033] The realization of the purpose, functional features and advantages of this application will be further explained in conjunction with the embodiments and with reference to the accompanying drawings. Detailed Implementation
[0034] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0035] Furthermore, the technical solutions of the various embodiments can be combined with each other, but only if they are feasible for those skilled in the art. If the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such combination of technical solutions does not exist and is not within the scope of protection claimed by this invention.
[0036] A method for preparing selenium-enriched modified biochar includes the following steps:
[0037] S01. Selenium-enriched biomass, such as selenium-enriched straw, is first crushed. The size of the crushed selenium-enriched biomass is 7-8cm.
[0038] S1. The crushed selenium-enriched biomass is carbonized at high temperature or hydrothermally to obtain selenium-enriched biochar.
[0039] S2. The selenium-enriched biochar is pulverized and then sieved. The size of the pulverized selenium-enriched biochar is 0.05-0.3 mm, thus obtaining the selenium-enriched modified biochar.
[0040] During high-temperature carbonization, the heating temperature is 350-750℃ and the heating time is 2-4 hours.
[0041] During hydrothermal carbonization, selenium-enriched biomass is mixed with water and subjected to a hydrothermal reaction at 150-250℃ for 8-12 hours. After hydrothermal carbonization, the hydrothermal product is washed until neutral and dried to obtain the selenium-enriched biochar. The solid-liquid ratio of the selenium-enriched biomass to water is 1:5-8. The drying temperature is 105-115℃ and the drying time is 10-12 hours.
[0042] The aforementioned selenium-enriched modified biochar can be applied to arsenic-containing water or soil to adsorb arsenic. This selenium-enriched modified biochar is particularly suitable for use in the cultivation of plants in arsenic-containing aquatic environments.
[0043] The technical solution of the present invention will be further described in detail below with reference to specific embodiments. It should be understood that the following embodiments are only used to explain the present invention and are not intended to limit the present invention.
[0044] All the selenium-enriched biomass in the following examples is selenium-enriched rice straw, produced by a farm in Shaoguan City, Guangdong Province. This farm pre-treated the rice by spraying it with selenium-enriched foliar fertilizer during the key growth stages (tillering and grain-filling stages). The main component of the selenium-enriched foliar fertilizer is organic selenium, and the spraying concentration was 5 g / L. The average selenium content in the harvested rice straw from this selenium-enriched crop was 481.3 ug / kg (measured after pulverizing and mixing), meeting the selenium-enrichment standard.
[0045] Example 1
[0046] A method for preparing selenium-enriched modified biochar includes the following steps:
[0047] S01. The selenium-enriched rice straw is dried and crushed, and then crushed using a medium-sized pulverizer to obtain selenium-enriched biomass with a size of 7-8cm.
[0048] S1. The crushed selenium-enriched rice straw is subjected to hydrothermal carbonization to obtain selenium-enriched biochar. During hydrothermal carbonization, 20 ml of deionized water is added to 70 g of selenium-enriched biomass for soaking. After complete soaking, the mixture is transferred to the inner liner of a high-pressure reactor. The high-pressure reactor is sealed and placed in an oven. The oven is set to heat at 200°C for 12 hours. After the high-pressure reactor cools to room temperature, the reactants are taken out and dispensed into centrifuge tubes. The tubes are washed three times with deionized water and three times with anhydrous ethanol. The centrifuge conditions are 8000 r / min, each lasting 5 minutes. After washing, the tubes are placed in an oven and dried at 80°C to obtain the selenium-enriched biochar. The solid-liquid ratio of the selenium-enriched biomass to water is 1:6.
[0049] S2. The selenium-enriched biochar is pulverized and then sieved. The size of the pulverized selenium-enriched biochar is 0.2 mm, thus obtaining selenium-enriched modified biochar.
[0050] Example 2
[0051] A method for preparing selenium-enriched modified biochar includes the following steps:
[0052] S01. The selenium-enriched rice straw is dried and crushed, and then crushed using a medium-sized pulverizer to obtain selenium-enriched biomass with a size of 7-8cm.
[0053] S1. The crushed selenium-enriched biomass is carbonized at high temperature to obtain selenium-enriched biochar; the high-temperature carbonization temperature is 350℃ and the heating time is 2h.
[0054] S2. After cooling, the selenium-enriched biochar is pulverized and sieved. At this time, the size of the pulverized selenium-enriched biochar is 0.2 mm, thus obtaining selenium-enriched modified biochar.
[0055] Example 3
[0056] In this embodiment, all preparation steps and parameters are the same as in Example 2, except that the high-temperature carbonization temperature is adjusted to 550℃.
[0057] Example 4
[0058] In this embodiment, all preparation steps and parameters are the same as in Example 2, except that the high-temperature carbonization temperature is adjusted to 750℃.
[0059] Selenium content detection: The modified biochar prepared in Examples 1-4 was subjected to selenium content detection (the detection process involved weighing 0.2g of the selenium-enriched modified biochar sample obtained in the above examples, adding nitric acid for microwave digestion, and using inductively coupled plasma mass spectrometry to determine the selenium content of the prepared biochar). Specific detection data are as follows: Figure 1As shown, the selenium content of rice straw after selenium-enriched planting was 481.3 ug / kg. Data from the modified biochar tests of the four examples above indicate that the selenium content in the hydrothermal method-prepared selenium-enriched straw modified biochar was 417.61 ug / kg, with the least selenium loss. In contrast, the selenium content in the high-temperature carbonization-prepared selenium-enriched straw biochar increased with increasing temperature, which may be related to the unit weight; the selenium content of the modified biochar carbonized at 350℃ was only 310.72 ug / kg. Therefore, the hydrothermal method for preparing selenium-enriched modified biochar exhibits less selenium loss, lower preparation temperature, reduced energy consumption, and lower carbon emissions, making it the most suitable preparation condition.
[0060] Performance determination of modified biochar: The modified biochar prepared in Examples 1-4 were subjected to scanning electron microscopy (SEM) to investigate the surface structure changes of the modified biochar under different preparation conditions. Figure 2 As shown, the modified biochar prepared by the hydrothermal method has small pores on its side and the pores are relatively uniformly distributed, which can enhance the adsorption effect of arsenic. The shape of the pores is similar to that of the modified biochar prepared by high-temperature carbonization at 350℃, which is approximately circular. However, the pore size of the biochar prepared by the high-temperature carbonization method is not uniform, and as the carbonization temperature increases, the pore folding strength of the modified biochar is greater and the pores become flatter.
[0061] The modified biochar prepared in Examples 1-4 were subjected to Fourier transform infrared (FTIR) scanning. The position, intensity, and shape of the spectral bands, as well as the relationship between absorption bands and temperature and aggregation state, were analyzed to observe the changes in functional groups of the modified biochar prepared under different treatment methods. Figure 3 Fourier transform infrared spectroscopy results showed that modified biochar prepared by hydrothermal carbonization had more functional groups on its surface, while modified biochar prepared by high-temperature carbonization had fewer functional groups as the carbonization temperature increased.
[0062] Arsenic adsorption experiment: in 10 mg L -1 40 mg of the modified biochar prepared in Examples 1-4 was added to an aqueous solution contaminated with arsenic as an adsorbent. The mixture was shaken in an air bath at 25 °C for 120 min, extracted, filtered through a 0.22 μm filter membrane, and the concentration of residual arsenic was analyzed. Figure 4 The test data show that among the biochar prepared by different methods, the arsenic adsorption capacity of selenium-enriched straw modified biochar prepared by hydrothermal method is 104.417 mg-As / g, which is 34.96%, 11.49%, 7.98%, and 6.38% higher than that of the blank control group and biochar prepared by high-temperature carbonization method (350℃, 550℃, 750℃), respectively. It can be seen that the adsorption capacity of biochar prepared by hydrothermal method is the strongest; while the adsorption capacity of modified biochar prepared by high-temperature carbonization method for arsenic increases with the increase of preparation temperature.
[0063] Water spinach cultivation experiment: Water spinach seedlings of uniform length were grown hydroponically for 3 weeks. Six treatment groups were set up (each replicated three times): blank control - ordinary water (treatment 1), As-contaminated water (50 μg / L) (treatment 2), As-contaminated water with the addition of selenium-enriched biochar prepared by hydrothermal method (treatment 3), As-contaminated water with the addition of selenium-enriched biochar prepared at 350℃ (treatment 4), As-contaminated water with the addition of selenium-enriched biochar prepared at 550℃ (treatment 5), and As-contaminated water with the addition of selenium-enriched biochar prepared at 750℃ (treatment 6). The arsenic content of water spinach roots, stems, and leaves was collected and analyzed. Figure 5 The test data shows that when selenium-enriched biochar prepared at 750℃ was added to arsenic-contaminated water, the arsenic content in the roots of water spinach was the lowest; when selenium-enriched biochar prepared by hydrothermal method was added to arsenic-contaminated water, the arsenic content in the stems and leaves of water spinach was the lowest. Since water spinach is a leafy vegetable, and the edible parts are the stems and leaves, it is evident that selenium-enriched biochar prepared by hydrothermal method has the best effect on arsenic adsorption in water spinach, effectively reducing the accumulation of arsenic in the stems and leaves.
[0064] Therefore, selenium-enriched modified biochar prepared by the hydrothermal method is particularly suitable for use in the cultivation of foliage plants in arsenic-contaminated water bodies. Selenium-enriched modified biochar prepared by the high-temperature carbonization method (carbonization temperature of 750℃) is particularly suitable for use in the cultivation of root plants in arsenic-contaminated water bodies.
[0065] Example 5
[0066] In this embodiment, all preparation steps and parameters are the same as in Example 1, except that the size of the selenium-enriched biochar after pulverization is different, as shown in the table below:
[0067] Size of selenium-enriched biochar after pulverization Example 1 0.2mm Example 5-1 0.05mm Example 5-2 0.1mm Example 5-3 0.15mm Example 5-4 0.25mm Example 5-5 0.3mm Examples 5-6 0.4mm Examples 5-7 0.5mm
[0068] Arsenic adsorption experiment: 40 mg of the modified biochar prepared in Example 5 was added to an aqueous solution contaminated with As as an adsorbent. The mixture was shaken in an air bath shaker at 25 °C, extracted, and filtered through a 0.22 μm filter membrane. The concentration of residual arsenic was analyzed. The time taken for each group of modified biochar to adsorb As to reach adsorption equilibrium was observed and recorded. Detailed data are shown in the table below:
[0069] Adsorption time / min Example 1 120 Example 5-1 100 Example 5-2 105 Example 5-3 110 Example 5-4 115 Example 5-5 120 Examples 5-6 125 Examples 5-7 130
[0070] The test data in the table above show that the size of the selenium-enriched biochar after pulverization can be 0.05-0.3 mm, at which point the adsorption efficiency for arsenic is relatively high. When the size of the selenium-enriched biochar after pulverization is further limited to 0.05-0.15 mm, the adsorption efficiency for arsenic can be further improved, and the time for adsorption of As to reach adsorption equilibrium can be controlled within 110 min (i.e., ≤110 min).
[0071] Example 6
[0072] In this embodiment, all preparation steps and parameters are the same as in Examples 5-5, except that the hydrothermal carbonization temperature is different, as detailed in the table below:
[0073]
[0074] Arsenic adsorption experiment: 40 mg of the modified biochar prepared in Example 6 was added to an aqueous solution contaminated with As as an adsorbent. The mixture was shaken in an air bath shaker at 25 °C, extracted, and filtered through a 0.22 μm filter membrane. The concentration of residual arsenic was analyzed. The time taken for each group of modified biochar to adsorb As to reach adsorption equilibrium was observed and recorded. Detailed data are shown in the table below:
[0075] Adsorption time / min Adsorption time / min Example 6-1-1 125 Example 6-4-1 120 Example 6-1-2 125 Example 6-4-2 120 Example 6-1-3 130 Example 6-4-3 125 Example 6-1-4 130 Example 6-4-4 125 Example 6-2-1 130 Example 6-5-1 125 Example 6-2-2 130 Example 6-5-2 125 Example 6-2-3 130 Example 6-5-3 130 Example 6-2-4 130 Example 6-5-4 130 Example 6-3-1 120 Example 6-6-1 125 Example 6-3-2 120 Example 6-6-2 125 Example 6-3-3 125 Example 6-6-3 130 Example 6-3-4 125 Example 6-6-4 130
[0076] The test data in the table above show that hydrothermal carbonization at temperatures between 150-250℃ exhibits good adsorption effects on arsenic. When the hydrothermal carbonization temperature is 180-220℃ and the heating rate is 5-6℃ / min, the resulting selenium-enriched biochar has a more uniform pore distribution and pore size, resulting in a faster adsorption rate and a quicker attainment of adsorption equilibrium for arsenic.
[0077] The above description is merely a preferred embodiment of the present invention and does not limit the patent scope of the present invention. Any equivalent structural transformations made using the contents of the present invention under the inventive concept of the present invention, or direct / indirect applications in other related technical fields, are included within the patent protection scope of the present invention.
Claims
1. The application of selenium-enriched modified biochar for arsenic adsorption in the cultivation of plants in arsenic-containing aquatic bodies, characterized in that, Includes the following steps: S1. Selenium-enriched biomass is heated and carbonized to obtain selenium-enriched biochar; S2. The selenium-enriched biochar is pulverized and then sieved to obtain the selenium-enriched modified biochar. The heating carbonization includes high-temperature carbonization or hydrothermal carbonization; During the hydrothermal carbonization, selenium-enriched biomass is mixed with water and then subjected to a hydrothermal reaction at 150-250℃ for 8-12 h. The heating rate during the hydrothermal reaction is 5-10℃ / min. After the hydrothermal carbonization is completed, the hydrothermal product is washed until neutral and dried to obtain the selenium-enriched biochar. The solid-liquid ratio of the selenium-enriched biomass to water is 1:5-8. Selenium-enriched modified biochar prepared by hydrothermal method is particularly suitable for use in the cultivation of foliage plants in arsenic-polluted water bodies, while selenium-enriched modified biochar prepared by high-temperature carbonization method at 750℃ is particularly suitable for use in the cultivation of root plants in arsenic-polluted water bodies. Selenium-enriched modified biochar is particularly suitable for use in arsenic-polluted water bodies. Since plants absorb and transport selenium and arsenic in the same way, when selenium-enriched biochar is modified by heating and carbonization, the adsorption performance of selenium-enriched modified biochar is increased. At the same time, by utilizing the element absorption competition relationship, the absorption and transport of arsenic by plants is reduced, further reducing the absorption effect of arsenic by plants.
2. The application of selenium-enriched modified biochar for arsenic adsorption according to claim 1 in the cultivation of plants in arsenic-containing aquatic bodies, characterized in that, The drying temperature is 105-115℃, and the drying time is 10-12h.
3. The application of selenium-enriched modified biochar for arsenic adsorption according to claim 1 in the cultivation of plants in arsenic-containing aquatic bodies, characterized in that, The heating time for high-temperature carbonization is 2-4 hours.
4. The application of selenium-enriched modified biochar for arsenic adsorption according to claim 1 in the cultivation of plants in arsenic-containing aquatic bodies, characterized in that, The selenium-enriched biomass is crushed before heating and carbonization, and the size of the crushed selenium-enriched biomass is 7-8 cm. In step S2, the size of the selenium-enriched biochar after pulverization is 0.05-0.3 mm.
5. The application of selenium-enriched modified biochar for arsenic adsorption according to claim 1 in the cultivation of plants in arsenic-containing aquatic bodies, characterized in that, The selenium-enriched biomass is selenium-enriched straw.
Citation Information
Patent Citations
Method for reducing paddy rice enriched inorganic mercury and methyl mercury with sodium selenite modified biochar
CN109719123A
Preparation method of rice straw biochar
CN104724694A
Preparation method of selenium-rich modified charcoal for adsorbing cadmium
CN115337917A