Heat storage-insulation multifunctional ceramic and preparation method thereof

By ball milling harmless solid waste with composite foaming agent and integrating it with phase change energy storage materials, closed-cell-open-cell double-layer ceramics are solved, and the problem that traditional ceramic materials cannot keep heat and store energy at the same time is realized. The material's heat insulation and heat storage functions are suitable for building insulation materials.

CN117945781BActive Publication Date: 2024-11-05BEIJING UNIV OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410101946.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-24
Publication Date
2024-11-05
Estimated Expiration
2044-01-24

AI Technical Summary

Technical Problem

Traditional porous ceramic materials cannot achieve thermal insulation and energy storage of buildings at the same time, and cannot meet the multifunctional needs of modern building insulation technology, especially in terms of time and space coordination of energy supply.

Method used

Ball milling, homogenizing and spray-drying with harmless solid waste and composite foaming agent to form closed-cell-open-cell double-layer ceramics, and the phase-change energy storage material and ceramic materials are integrated through vacuum impregnation to build heat storage- Heat-insulated multifunctional ceramic.

Benefits of technology

It realizes the heat insulation and heat storage functions of ceramic materials, improves the thermal insulation performance of building, and can coordinate energy supply in time and space, and is suitable for the field of building insulation materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117945781B_ABST
    Figure CN117945781B_ABST
Patent Text Reader

Abstract

The present invention provides a heat storage-insulation multifunctional ceramic and a preparation method thereof, using harmless solid waste as the main raw material, and preparing closed-cell-open-cell double-layer ceramics through processes such as ball milling, homogenization, drying, spreading, and heat treatment, and then preparing heat storage-insulation multifunctional ceramics through vacuum impregnation of closed-cell-open-cell double-layer ceramics and phase change energy storage materials. The present invention constructs a closed-cell-open-cell double-layer ceramic-based composite phase change energy storage material, and the phase change energy storage material loaded by the open-cell ceramic part has good heat storage / release characteristics. The closed-cell ceramic part has a rich closed-cell structure, which makes it have a lower thermal conductivity. While realizing the heat supply of the phase change energy storage material to the heat-requiring space, it can also ensure that the heat rich in the phase change energy storage material is less dissipated to the outside world, and has potential application value in the field of building insulation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of resource recycling and energy storage, and in particular relates to a heat storage-insulation multifunctional ceramic and a preparation method thereof. Background Art

[0002] Building energy consumption accounts for 40% of global energy consumption, and nearly 30% of global greenhouse gas emissions are related to building energy consumption. At present, my country has a huge building area of ​​more than 43 billion square meters, and non-energy-saving buildings account for 95%. The low thermal insulation performance of buildings not only seriously affects the indoor cooling and heating effects, but also increases energy consumption and reduces energy efficiency.

[0003] Porous ceramic materials are often used in many fields such as building insulation due to their low thermal conductivity. Although porous ceramic materials can reduce indoor heat loss in winter, they cannot absorb heat radiation for energy storage in winter; although porous ceramic materials can reduce the impact of external heat on indoor temperature in summer, they cannot maintain indoor temperature for a long time through heat storage / release. Traditional porous ceramic materials can no longer meet the multifunctional requirements of current building insulation technology. Therefore, the development of new building insulation materials to achieve the requirements of coordinated energy supply in time and space is a research focus in the field of building energy conservation, which is of great significance to the national strategic needs of achieving efficient energy conservation, improving resource utilization and sustainable development.

[0004] Phase change energy storage technology can achieve the coordination of energy supply in time and space, which can not only meet people's technical and economic requirements for engineering and products, but also improve energy utilization. Phase change energy storage materials are the material basis of phase change energy storage technology. Phase change energy storage technology stores and releases energy through the change of phase state of phase change energy storage materials during the phase change process.

[0005] Therefore, how to provide a preparation method of heat storage-insulation multifunctional ceramics, prepare porous ceramic materials with harmless solid waste as the main raw material, and vacuum integrate the porous ceramic materials with phase change energy storage materials to construct ceramic-based composite phase change energy storage materials to achieve thermal insulation and heat storage of the materials, is a technical problem that technical personnel in this field urgently need to solve. Summary of the invention

[0006] The object of the present invention is to provide a heat storage-insulation multifunctional ceramic and a preparation method thereof, so as to solve at least one of the above-mentioned technical problems.

[0007] To achieve the above object, the first aspect of the present invention provides a method for preparing a heat storage-insulation multifunctional ceramic, the preparation method comprising:

[0008] Ball-milling the harmless solid waste and the composite foaming agent to obtain a first ball-milled material; the composite foaming agent is composed of sodium carbonate and silicon carbide;

[0009] Homogenizing the first ball mill material to obtain a first homogenized material;

[0010] spray drying the first homogenized material to obtain a first dry material;

[0011] ball-milling the harmless solid waste and silicon carbide to obtain a second ball-milled material;

[0012] homogenizing the second ball mill material to obtain a second homogenized material;

[0013] spray drying the second homogenized material to obtain a second dried material;

[0014] The first dry material is spread to obtain a first raw embryo, and the second dry material is spread on the basis of the first raw embryo to obtain a second raw embryo; the thickness of the first dry material is the same as the thickness of the second dry material;

[0015] heat treating the second green body to obtain a closed-pore-open-pore double-layer ceramic;

[0016] The closed-pore-open-pore double-layer ceramic and the phase-change energy storage material are placed in a beaker and vacuum impregnated to obtain a heat storage-insulation multifunctional ceramic.

[0017] In the first aspect, the harmless solid waste and the composite foaming agent are ball-milled to obtain a first ball-milled material; the composite foaming agent is composed of sodium carbonate and silicon carbide, which specifically includes: wet ball-milling the weighed harmless solid waste, sodium carbonate and silicon carbide, the ball-to-material ratio during the ball milling process is 1:1-3:1, the ball-to-material ratio is 1:1-2:1, the ball milling time is 2-6 hours, and after the ball milling is completed, sieving through an 8-mesh mesh cloth to obtain the first ball-milled material; wherein the mass of the sodium carbonate is 2% to 10% of the dry weight of the harmless solid waste, and the mass of the silicon carbide is 1% to 3% of the dry weight of the harmless solid waste.

[0018] In the first aspect, the homogenizing the first ball mill to obtain the first homogenized material specifically includes: homogenizing the first ball mill, stirring at a speed of 0.5 to 2.0 r / min during the homogenization process, and a homogenization time of 4 to 8 hours. After the homogenization is completed, sieving through a 60-mesh sieve to obtain the first homogenized material.

[0019] In the first aspect, the ball milling of harmless solid waste and silicon carbide to obtain a second ball mill material specifically includes: wet ball milling the weighed harmless solid waste and silicon carbide, wherein the ball-to-material ratio during the ball milling process is 1:1 to 3:1, the ball-to-material ratio is 1:1 to 2:1, and the ball milling time is 2 to 6 hours. After the ball milling is completed, sieving through an 8-mesh mesh cloth to obtain a second ball mill material; wherein the mass of the silicon carbide is 1% to 3% of the dry weight of the harmless solid waste.

[0020] In the first aspect, the second ball mill material is homogenized to obtain a second homogenized material, which specifically includes: homogenizing the second ball mill material, stirring at a speed of 0.5 to 2 r / min during the homogenization process, and a homogenization time of 4 to 8 hours. After the homogenization is completed, the material is sieved through a 60-mesh sieve to obtain a second homogenized material.

[0021] In the first aspect, the heat treatment of the second green embryo to obtain a closed-pore-open-pore double-layer ceramic specifically includes: placing the second green embryo in a muffle furnace for heat treatment, heating the temperature from room temperature to 600-800°C at a heating rate of 3-10°C / min during the heat treatment, keeping the temperature for 30-90 minutes, continuing to heat the temperature to 1000°C-1250°C at a heating rate of 3-10°C / min, keeping the temperature for 30-90 minutes, and cooling to room temperature with the furnace temperature after sintering to obtain a closed-pore-open-pore double-layer ceramic.

[0022] In the first aspect, the closed-pore-open-pore double-layer ceramic and phase change energy storage material are placed in a beaker and vacuum impregnated to obtain heat storage-insulation multifunctional ceramics, which specifically includes: weighing the closed-pore-open-pore double-layer ceramic and the phase change energy storage material and placing them in a beaker, wherein the mass ratio of the closed-pore-open-pore double-layer ceramic to the phase change energy storage material is 1:20; placing the beaker in a vacuum drying oven, setting the temperature of the vacuum drying oven to T, the phase change temperature of the phase change energy storage material to T0, the temperature difference between the temperature T and the phase change temperature T0 is ΔT, ΔT=T-T0, and the ΔT is greater than 10°C; vacuum impregnating in the vacuum drying oven for 2 hours to obtain heat storage-insulation multifunctional ceramics.

[0023] The second aspect of the present invention provides a heat storage-insulation multifunctional ceramic, which includes a closed-pore-open-pore double-layer ceramic and a phase change energy storage material; and is made by the preparation method of the heat storage-insulation multifunctional ceramic described in the first aspect.

[0024] In the second aspect, the closed-pore-open-pore double-layer ceramic includes: a closed-pore ceramic layer, which is fired from harmless solid waste and silicon carbide, and has a heat insulation function; an open-pore ceramic layer, which is fired from harmless solid waste, sodium carbonate and silicon carbide, and has a heat storage function after being loaded with phase change energy storage material.

[0025] In the second aspect, the harmless solid waste includes at least one of lithium mica tailings, waste FCC harmless tailings and fly ash; and the phase change energy storage material includes at least one of paraffin, sodium sulfate decahydrate and polyethylene glycol.

[0026] Beneficial effects:

[0027] The present invention provides a preparation method of a heat storage-insulation multifunctional ceramic. First, harmless solid waste, sodium carbonate and silicon carbide are used as raw materials, and a first dry material is obtained through ball milling, homogenization, drying and other processes. Harmless solid waste and silicon carbide are used as raw materials, and a second dry material is obtained through ball milling, homogenization, drying and other processes. Secondly, the first dry material is spread to obtain a first green embryo, and the second dry material is spread on the basis of the first green embryo to obtain a second green embryo, and the spreading thickness of the first dry material is equal to the spreading thickness of the second dry material, so as to construct a double The first step is to heat-treat the second raw material, during which a layer of raw material containing sodium carbonate and silicon carbide decomposes to produce gas, forming pores, and constructing an open-pored ceramic layer. A layer of raw material containing silicon carbide decomposes to produce gas, forming pores, and constructing a closed-pored ceramic layer. That is, a closed-pored-open-pored double-layer ceramic is obtained after heat treatment. Finally, the closed-pored-open-pored double-layer ceramic is vacuum impregnated in a phase change energy storage material, so that the open-pored ceramic layer is filled with phase change energy storage materials to achieve a heat storage function, and the closed-pored ceramic layer achieves a heat insulation function. The present application uses harmless solid waste as the main raw material to prepare a porous ceramic material, and vacuum integrates the porous ceramic material with a phase change energy storage material to construct a closed-pored-open-pored double-layer ceramic-based composite phase change energy storage material to achieve thermal insulation and heat storage of the material, which can be applied to the field of building thermal insulation materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the embodiments of this specification or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0029] Figure 1 This is a flow chart of a method for preparing a heat storage-insulation multifunctional ceramic in this application. DETAILED DESCRIPTION

[0030] The present invention will be described in detail below in conjunction with specific implementations and examples, and the advantages and various effects of the present invention will be more clearly presented. It should be understood by those skilled in the art that these specific implementations and examples are used to illustrate the present invention, rather than to limit the present invention.

[0031] Throughout the specification, unless otherwise specifically stated, the terms used herein should be understood as meanings commonly used in the art. Therefore, unless otherwise defined, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. In the event of a conflict, the present specification takes precedence.

[0032] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or obtained by existing methods.

[0033] See also Figure 1 The present application provides a method for preparing a heat storage-insulation multifunctional ceramic, the preparation method comprising:

[0034] S1. ball-milling harmless solid waste and a composite foaming agent to obtain a first ball-milled material; the composite foaming agent is composed of sodium carbonate and silicon carbide;

[0035] S2, homogenizing the first ball mill material to obtain a first homogenized material;

[0036] S3, spray drying the first homogenized material to obtain a first dry material;

[0037] S4, ball-milling the harmless solid waste and silicon carbide to obtain a second ball-milled material;

[0038] S5, homogenizing the second ball mill material to obtain a second homogenized material;

[0039] S6, spray drying the second homogenized material to obtain a second dry material;

[0040] S7, spreading the first dry material to obtain a first raw embryo, and spreading the second dry material on the basis of the first raw embryo to obtain a second raw embryo; the thickness of the first dry material is the same as the thickness of the second dry material;

[0041] S8, heat treating the second green body to obtain a closed-pore-open-pore double-layer ceramic;

[0042] S9, placing the closed-pore-open-pore double-layer ceramic and phase-change energy storage material in a beaker, and performing vacuum impregnation to obtain heat storage-insulation multifunctional ceramic.

[0043] Specifically, the present invention provides a preparation method of a heat storage-insulation multifunctional ceramic, firstly, using harmless solid waste, sodium carbonate and silicon carbide as raw materials, through ball milling, homogenization, drying and other processes to obtain a first dry material, using harmless solid waste and silicon carbide as raw materials, through ball milling, homogenization, drying and other processes to obtain a second dry material; secondly, the first dry material is spread to obtain a first green embryo, and the second dry material is spread on the basis of the first green embryo to obtain a second green embryo, and the spreading thickness of the first dry material is equal to the spreading thickness of the second dry material, so that Construct a double-layer ceramic material foundation; then, heat treat the second green embryo, during the heat treatment process, a layer of green embryo containing sodium carbonate and silicon carbide decomposes to produce gas, forming pores, and constructing an open-pored ceramic layer, and a layer of green embryo containing silicon carbide decomposes to produce gas, forming pores, and constructing a closed-pored ceramic layer, that is, a closed-pored-open-pored double-layer ceramic is obtained after heat treatment; finally, the closed-pored-open-pored double-layer ceramic is vacuum impregnated in a phase change energy storage material, so that the open-pored ceramic layer is filled with phase change energy storage materials to achieve a heat storage function, and the closed-pored ceramic layer achieves a heat insulation function. The present application uses harmless solid waste as the main raw material to prepare a porous ceramic material, and vacuum integrates the porous ceramic material with a phase change energy storage material to construct a closed-pored-open-pored double-layer ceramic-based composite phase change energy storage material to achieve thermal insulation and heat storage of the material, which can be applied to the field of building thermal insulation materials.

[0044] In some possible embodiments, the harmless solid waste and the composite foaming agent are ball-milled to obtain a first ball-milled material; the composite foaming agent is composed of sodium carbonate and silicon carbide, which specifically includes: wet ball-milling the weighed harmless solid waste, sodium carbonate and silicon carbide, the ball-to-material ratio during the ball milling process is 1:1 to 3:1, the ball-to-material ratio is 1:1 to 2:1, the ball milling time is 2 to 6 hours, and after the ball milling is completed, sieving through an 8-mesh mesh cloth to obtain the first ball-milled material; wherein the mass of the sodium carbonate is 2% to 10% of the dry weight of the harmless solid waste, and the mass of the silicon carbide is 1% to 3% of the dry weight of the harmless solid waste.

[0045] Those skilled in the art can understand that the harmless solid waste, sodium carbonate and silicon carbide are wet-milled and sieved through an 8-mesh mesh cloth so that the particle size of the first ball mill obtained is uniform, which lays a good foundation for subsequent processes. In addition, in the present application, the mass of sodium carbonate is 2% to 10% of the dry weight of the harmless solid waste, and the mass of silicon carbide is 1% to 3% of the dry weight of the harmless solid waste, that is, a large amount of harmless solid waste can be consumed to achieve resource recycling.

[0046] In some possible embodiments, the homogenizing the first ball mill to obtain a first homogenized material specifically includes: homogenizing the first ball mill, stirring at a speed of 0.5 to 2 r / min during the homogenization process, and a homogenization time of 4 to 8 hours. After the homogenization is completed, sieving through a 60-mesh sieve to obtain the first homogenized material.

[0047] This is because the first ball mill material is homogenized so that sodium carbonate and silicon carbide can be evenly distributed among the harmless solid waste, and is sieved through a 60-mesh sieve to obtain a first homogenized material with a smaller particle size, so as to reduce the distance between components in the subsequent distribution process.

[0048] In some possible embodiments, the ball milling of harmless solid waste and silicon carbide to obtain a second ball mill material specifically includes: wet ball milling the weighed harmless solid waste and silicon carbide, wherein the ball-to-material ratio during the ball milling process is 1:1 to 3:1, the ball-to-material ratio is 1:1 to 2:1, and the ball milling time is 2 to 6 hours. After the ball milling is completed, sieving through an 8-mesh mesh cloth to obtain a second ball mill material; wherein the mass of the silicon carbide is 1% to 3% of the dry weight of the harmless solid waste.

[0049] Those skilled in the art can understand that compared with the first ball mill, sodium carbonate is not added to the second ball mill, so that the first ball mill and the second ball mill will have inconsistent pores during the subsequent heat treatment process, thereby forming an open-pore-closed-pore double-layer structure, and the pores in the open-pore-closed-pore double-layer structure are of different sizes, and the adsorption effect on the molten phase change energy storage material is also different, thereby achieving a heat storage-insulation effect.

[0050] In some possible embodiments, the homogenizing the second ball mill to obtain the second homogenized material specifically includes: homogenizing the second ball mill, stirring at a speed of 0.5 to 2.0 r / min during the homogenization process, and a homogenization time of 4 to 8 hours. After the homogenization is completed, sieving through a 60-mesh sieve to obtain the second homogenized material.

[0051] In some possible embodiments, the heat treatment of the second green embryo to obtain a closed-pore-open-pore double-layer ceramic specifically includes: placing the second green embryo in a muffle furnace for heat treatment, heating the temperature from room temperature to 600-800°C at a heating rate of 3-10°C / min during the heat treatment, keeping the temperature for 30-90 minutes, continuing to heat the temperature to 1000°C-1250°C at a heating rate of 3-10°C / min, keeping the temperature for 30-90 minutes, and cooling to room temperature with the furnace temperature after sintering to obtain a closed-pore-open-pore double-layer ceramic.

[0052] This is because the second green embryo is placed in a muffle furnace for heat treatment, firstly the temperature is raised from room temperature to 600-800°C and kept for 30-90 minutes, so that the glass phase component is produced, in preparation for the rear end heating to produce a porous structure, and then the temperature is continued to be raised to 1000-1250°C and kept for 30-90 minutes, so that a layer of green embryo containing sodium carbonate and silicon carbide decomposes to produce gas, forming pores, and constructing an open-porous ceramic layer, and a layer of green embryo containing silicon carbide decomposes to produce gas, forming pores, and constructing a closed-porous ceramic layer, that is, a closed-porous-open-porous double-layer ceramic is obtained after heat treatment.

[0053] In some possible embodiments, the closed-pore-open-pore double-layer ceramic and phase change energy storage material are placed in a beaker and vacuum impregnated to obtain heat storage-insulation multifunctional ceramics, specifically comprising: weighing the closed-pore-open-pore double-layer ceramic and the phase change energy storage material and placing them in a beaker, wherein the mass ratio of the closed-pore-open-pore double-layer ceramic to the phase change energy storage material is 1:20; placing the beaker in a vacuum drying oven, setting the temperature of the vacuum drying oven to T, the phase change temperature of the phase change energy storage material to T0, the temperature difference between the temperature T and the phase change temperature T0 is ΔT, ΔT=T-T0, and the ΔT is greater than 10°C; vacuum impregnating in the vacuum drying oven for 2 hours to obtain heat storage-insulation multifunctional ceramics.

[0054] Those skilled in the art can understand that the closed-cell-open-cell double-layer ceramic and the phase change energy storage material are placed in a beaker at the same time, and placed in a vacuum drying oven, and the temperature of the vacuum drying oven is adjusted so that the phase change energy storage material heats up and becomes a molten state, and then enters the open-pore structure formed in the closed-cell-open-cell double-layer ceramic, so that the phase change energy storage material can supply heat to the heat-requiring space while ensuring that less heat in the phase change energy storage material is lost to the outside, thereby achieving a heat storage-insulation effect.

[0055] Based on a general inventive concept, the present application also provides a heat storage-insulation multifunctional ceramic, which includes a closed-pore-open-pore double-layer ceramic and a phase change energy storage material; and is made by the preparation method of the heat storage-insulation multifunctional ceramic described in the first aspect.

[0056] In combination with the second aspect of the present application, the closed-pore-open-pore double-layer ceramic includes: a closed-pore ceramic layer, which is fired from harmless solid waste and silicon carbide, and has a heat insulation function; an open-pore ceramic layer, which is fired from harmless solid waste, sodium carbonate and silicon carbide, and has a heat storage function after being loaded with phase change energy storage material.

[0057] In combination with the second aspect of the present application, the harmless solid waste includes at least one of lithium mica tailings, waste FCC harmless tailings and fly ash; the phase change energy storage material includes at least one of paraffin, sodium sulfate decahydrate and polyethylene glycol.

[0058] The present application provides a heat storage-insulation multifunctional ceramic, whose raw materials are mainly composed of harmless solid waste, thus realizing resource utilization and making full use of the characteristics of phase change energy storage materials and the constructed closed-pore-open-pore double-layer ceramic structure, so that the prepared heat storage-insulation multifunctional ceramic has a wide phase change temperature range, a high phase change enthalpy value, and a long cycle life, and can achieve coordinated energy supply in time and space, and can be applied to the field of building thermal insulation materials.

[0059] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.

[0060] Example 1

[0061] In this embodiment, lithium mica tailing mud is used as harmless solid waste, sodium carbonate and silicon carbide are used as foaming agents, and closed-cell-open-cell double-layer ceramics are prepared through processes such as ball milling, homogenization, drying, spreading, and heat treatment. The open-cell part of the closed-cell-open-cell double-layer ceramics uses sodium carbonate and silicon carbide as composite foaming agents, wherein sodium carbonate accounts for 2% of the dry weight of the harmless solid waste, and silicon carbide accounts for 1% of the dry weight of the harmless solid waste; the closed-cell part of the closed-cell-open-cell double-layer ceramics uses silicon carbide as a foaming agent, wherein silicon carbide accounts for 1% of the dry weight of the harmless solid waste; paraffin is used as a phase change energy storage material, and the closed-cell-open-cell double-layer ceramics are used as a carrier, and heat storage-insulation multifunctional ceramics are prepared by vacuum impregnation; its main preparation steps are:

[0062] (1) Weighing the lithium mica tail mud, sodium carbonate and silicon carbide is wet ball milled, the ball-to-material ratio is 1:1 during the ball milling process, the ball-to-material ratio is 1:1, the ball milling time is 2 hours, and after the ball milling is completed, it is sieved through an 8-mesh mesh cloth to obtain a first ball milling material;

[0063] (2) homogenizing the first ball mill material, with a stirring speed of 0.5 r / min and a homogenization time of 4 h. After the homogenization, sieving through a 60-mesh sieve to obtain a first homogenized material;

[0064] (3) spray drying the first homogenized material to obtain a first dried material;

[0065] (4) Wet ball milling the weighed lithium mica tail mud and silicon carbide, with a ball-to-material ratio of 1:1 during the ball milling process, and a ball-to-material ratio of 1:1 for 2 hours. After the ball milling is completed, the ball is sieved through an 8-mesh mesh cloth to obtain a second ball mill material;

[0066] (5) homogenizing the second ball mill material, with a stirring speed of 0.5 r / min and a homogenization time of 4 h. After the homogenization is completed, sieving through a 60-mesh sieve to obtain a second homogenized material;

[0067] (6) spray drying the second homogenized material to obtain a second dried material;

[0068] (7) Weaving the first dry material to obtain a first raw embryo, and weaving the second dry material based on the first raw embryo to obtain a second raw embryo; wherein the thickness of the first dry material is the same as the thickness of the second dry material;

[0069] (8) placing the second green embryo in a muffle furnace for heat treatment, during the heat treatment process, heating from room temperature to 600° C. at a heating rate of 3° C. / min, keeping the temperature for 30 min, and then heating to 1000° C. at a heating rate of 10° C. / min, keeping the temperature for 30 min, and cooling to room temperature with the furnace temperature after sintering to obtain a closed-pore-open-pore double-layer ceramic;

[0070] (9) Weighing the closed-cell-open-cell double-layer ceramic and paraffin wax and placing them in a beaker, the mass ratio of the closed-cell-open-cell double-layer ceramic and the paraffin wax is 1:20; placing the beaker in a vacuum drying oven, setting the temperature of the vacuum drying oven to 70°C, and then vacuum impregnating for 2 hours to obtain heat storage-insulation multifunctional ceramics.

[0071] The heat storage-insulation multifunctional ceramic prepared in this embodiment has a true porosity of 85.6%, a closed porosity of 83.1%, and a thermal conductivity of 0.012 W·m -1 ·k -1 The phase change energy storage temperature of the heat storage ceramic part of the heat storage-insulation multifunctional ceramic is 56.4℃, and the phase change enthalpy is 216.4J / g; the thermal conductivity is 0.13W·m -1 ·k -1 The compressive strength of the heat storage-insulation multifunctional ceramic is 26.38MPa and the flexural strength is 7.63MPa.

[0072] Example 2

[0073] In this embodiment, lithium mica tailing mud is used as harmless solid waste, sodium carbonate and silicon carbide are used as foaming agents, and closed-cell-open-cell double-layer ceramics are prepared through processes such as ball milling, homogenization, drying, spreading, and heat treatment. The open-cell part of the closed-cell-open-cell double-layer ceramics uses sodium carbonate and silicon carbide as composite foaming agents, wherein sodium carbonate accounts for 10% of the dry weight of the harmless solid waste, and silicon carbide accounts for 2% of the dry weight of the harmless solid waste; the closed-cell part of the closed-cell-open-cell double-layer ceramics uses silicon carbide as a foaming agent, wherein silicon carbide accounts for 3% of the dry weight of the harmless solid waste; sodium sulfate decahydrate is used as a phase change energy storage material, and the closed-cell-open-cell double-layer ceramics are used as a carrier, and heat storage-insulation multifunctional ceramics are prepared by vacuum impregnation; its main preparation steps are:

[0074] (1) Weighing the lithium mica tail mud, sodium carbonate and silicon carbide is wet ball milled, the ball-to-material ratio is 2:1, the ball-to-material ratio is 1:1, the ball milling time is 4 hours, and after the ball milling is completed, it is sieved through an 8-mesh mesh cloth to obtain a first ball milling material;

[0075] (2) homogenizing the first ball mill material, with a stirring speed of 1.0 r / min and a homogenization time of 6 h. After the homogenization is completed, sieving through a 60-mesh sieve to obtain a first homogenized material;

[0076] (3) spray drying the first homogenized material to obtain a first dried material;

[0077] (4) Wet ball milling the weighed lithium mica tail mud and silicon carbide, with a ball-to-material ratio of 2:1 and a ball-to-material ratio of 1:1 during the ball milling process, and the ball milling time is 4 hours. After the ball milling is completed, the ball milling is sieved through an 8-mesh mesh cloth to obtain a second ball milling material;

[0078] (5) homogenizing the second ball mill material, with a stirring speed of 1.0 r / min and a homogenization time of 6 h. After the homogenization is completed, sieving through a 60-mesh sieve to obtain a second homogenized material;

[0079] (6) spray drying the second homogenized material to obtain a second dried material;

[0080] (7) Weaving the first dry material to obtain a first raw embryo, and weaving the second dry material based on the first raw embryo to obtain a second raw embryo; wherein the thickness of the first dry material is the same as the thickness of the second dry material;

[0081] (8) placing the second green embryo in a muffle furnace for heat treatment, during the heat treatment process, heating from room temperature to 800° C. at a heating rate of 10° C. / min, keeping the temperature for 90 min, and then heating to 1250° C. at a heating rate of 10° C. / min, keeping the temperature for 90 min, and cooling to room temperature along with the furnace temperature after sintering to obtain a closed-pore-open-pore double-layer ceramic;

[0082] (9) Weigh the closed-cell-open-cell double-layer ceramic and sodium sulfate decahydrate and place them in a beaker, wherein the mass ratio of the closed-cell-open-cell double-layer ceramic to the sodium sulfate decahydrate is 1:20; place the beaker in a vacuum drying oven, set the temperature of the vacuum drying oven to 50°C, and then vacuum impregnate for 2 hours to obtain a heat storage-insulation multifunctional ceramic.

[0083] The heat storage-insulation multifunctional ceramic prepared in this embodiment has a true porosity of 93.4%, a closed porosity of 90.3%, and a thermal conductivity of 0.008 W·m -1 ·k -1 The phase change energy storage temperature of the heat storage ceramic part of the heat storage-insulation multifunctional ceramic is 33.7℃, and the phase change enthalpy is 198.7J / g; the thermal conductivity is 0.22W·m -1 ·k -1 The compressive strength of the heat storage-insulation multifunctional ceramic is 20.48MPa and the flexural strength is 5.69MPa.

[0084] Example 3

[0085] In this embodiment, waste FCC harmless tailings are used as harmless solid waste, sodium carbonate and silicon carbide are used as foaming agents, and closed-cell-open-cell double-layer ceramics are prepared through processes such as ball milling, homogenization, drying, spreading, and heat treatment. The open-cell part of the closed-cell-open-cell double-layer ceramics uses sodium carbonate and silicon carbide as composite foaming agents, wherein sodium carbonate accounts for 5% of the dry weight of the harmless solid waste, and silicon carbide accounts for 3% of the dry weight of the harmless solid waste; the closed-cell part of the closed-cell-open-cell double-layer ceramics uses silicon carbide as a foaming agent, wherein silicon carbide accounts for 2% of the dry weight of the harmless solid waste; paraffin is used as a phase change energy storage material, and the closed-cell-open-cell double-layer ceramics are used as a carrier to prepare heat storage-insulation multifunctional ceramics through vacuum impregnation; its main preparation steps are:

[0086] (1) Weighing the waste FCC harmless tailings, sodium carbonate and silicon carbide was wet-milled, the ball-to-material ratio was 3:1, the ball-to-material ratio was 2:1, the ball-milling time was 4 hours, and after the ball-milling, it was sieved through an 8-mesh mesh cloth to obtain a first ball-milled material;

[0087] (2) homogenizing the first ball mill material, with a stirring speed of 1.0 r / min and a homogenization time of 6 h. After the homogenization is completed, sieving through a 60-mesh sieve to obtain a first homogenized material;

[0088] (3) spray drying the first homogenized material to obtain a first dried material;

[0089] (4) Wet-milling the weighed waste FCC harmless tailings and silicon carbide, with a ball-to-material ratio of 3:1 and a ball-to-material ratio of 2:1 during the ball milling process, and the ball milling time is 4 hours. After the ball milling is completed, the material is sieved through an 8-mesh mesh cloth to obtain a second ball mill material;

[0090] (5) homogenizing the second ball mill material, with a stirring speed of 1.0 r / min and a homogenization time of 6 h. After the homogenization is completed, sieving through a 60-mesh sieve to obtain a second homogenized material;

[0091] (6) spray drying the second homogenized material to obtain a second dried material;

[0092] (7) Weaving the first dry material to obtain a first raw embryo, and weaving the second dry material based on the first raw embryo to obtain a second raw embryo; wherein the thickness of the first dry material is the same as the thickness of the second dry material;

[0093] (8) placing the second green embryo in a muffle furnace for heat treatment, during the heat treatment process, heating from room temperature to 800° C. at a heating rate of 5° C. / min, keeping the temperature for 90 min, and then heating to 1200° C. at a heating rate of 5° C. / min, keeping the temperature for 90 min, and cooling to room temperature along with the furnace temperature after sintering to obtain a closed-pore-open-pore double-layer ceramic;

[0094] (9) Weighing the closed-cell-open-cell double-layer ceramic and paraffin wax and placing them in a beaker, the mass ratio of the closed-cell-open-cell double-layer ceramic and the paraffin wax is 1:20; placing the beaker in a vacuum drying oven, setting the temperature of the vacuum drying oven to 70°C, and then vacuum impregnating for 2 hours to obtain heat storage-insulation multifunctional ceramics.

[0095] The heat storage-insulation multifunctional ceramic prepared in this embodiment has a true porosity of 88.5%, a closed porosity of 85.2%, and a thermal conductivity of 0.01 W·m -1 ·k -1 The phase change energy storage temperature of the heat storage ceramic part of the heat storage-insulation multifunctional ceramic is 55.9℃, and the phase change enthalpy is 221.4J / g; the thermal conductivity is 0.12W·m -1 ·k -1 The compressive strength of the heat storage-insulation multifunctional ceramic is 23.78MPa and the flexural strength is 6.94MPa.

[0096] Example 4

[0097] In this embodiment, waste FCC harmless tailings are used as harmless solid waste, sodium carbonate and silicon carbide are used as foaming agents, and closed-cell-open-cell double-layer ceramics are prepared through processes such as ball milling, homogenization, drying, spreading, and heat treatment. The open-cell part of the closed-cell-open-cell double-layer ceramics uses sodium carbonate and silicon carbide as composite foaming agents, wherein sodium carbonate accounts for 8% of the dry weight of the harmless solid waste, and silicon carbide accounts for 3% of the dry weight of the harmless solid waste; the closed-cell part of the closed-cell-open-cell double-layer ceramics uses silicon carbide as a foaming agent, wherein silicon carbide accounts for 3% of the dry weight of the harmless solid waste; sodium sulfate decahydrate is used as a phase change energy storage material, and the closed-cell-open-cell double-layer ceramics are used as a carrier to prepare heat storage-insulation multifunctional ceramics through vacuum impregnation; its main preparation steps are:

[0098] (1) Weighing the waste FCC harmless tailings, sodium carbonate and silicon carbide and subjecting them to wet ball milling, wherein the ball-to-material ratio is 2:1 and the ball-to-material ratio is 1:1 during the ball milling process, and the ball milling time is 6 hours. After the ball milling is completed, the material is sieved through an 8-mesh mesh cloth to obtain a first ball milling material;

[0099] (2) homogenizing the first ball mill material, with a stirring speed of 2.0 r / min and a homogenization time of 6 h. After the homogenization is completed, sieving through a 60-mesh sieve to obtain a first homogenized material;

[0100] (3) spray drying the first homogenized material to obtain a first dried material;

[0101] (4) Wet ball milling of the weighed waste FCC harmless tailings and silicon carbide, with a ball-to-material ratio of 2:1 and a ball-to-material ratio of 1:1 during the ball milling process, and a ball milling time of 6 hours. After the ball milling is completed, the ball milling is sieved through an 8-mesh mesh cloth to obtain a second ball milling material;

[0102] (5) homogenizing the second ball mill material, with a stirring speed of 2.0 r / min and a homogenization time of 6 h. After the homogenization is completed, sieving through a 60-mesh sieve to obtain a second homogenized material;

[0103] (6) spray drying the second homogenized material to obtain a second dried material;

[0104] (7) Weaving the first dry material to obtain a first raw embryo, and weaving the second dry material based on the first raw embryo to obtain a second raw embryo; wherein the thickness of the first dry material is the same as the thickness of the second dry material;

[0105] (8) placing the second green embryo in a muffle furnace for heat treatment, during the heat treatment process, heating from room temperature to 800° C. at a heating rate of 8° C. / min, keeping the temperature for 360 min, and then heating to 1100° C. at a heating rate of 8° C. / min, keeping the temperature for 60 min, and cooling to room temperature along with the furnace temperature after sintering to obtain a closed-pore-open-pore double-layer ceramic;

[0106] (9) Weigh the closed-cell-open-cell double-layer ceramic and sodium sulfate decahydrate and place them in a beaker, wherein the mass ratio of the closed-cell-open-cell double-layer ceramic to the sodium sulfate decahydrate is 1:20; place the beaker in a vacuum drying oven, set the temperature of the vacuum drying oven to 50°C, and then vacuum impregnate for 2 hours to obtain a heat storage-insulation multifunctional ceramic.

[0107] The heat storage-insulation multifunctional ceramic prepared in this embodiment has a true porosity of 91.6%, a closed porosity of 88.7%, and a thermal conductivity of 0.009 W·m -1 ·k -1 The phase change energy storage temperature of the heat storage ceramic part of the heat storage-insulation multifunctional ceramic is 32.9°C, and the phase change enthalpy is 201.3J / g; the thermal conductivity is 0.18W·m -1 ·k -1 The compressive strength of the heat storage-insulation multifunctional ceramic is 19.37MPa and the flexural strength is 5.12MPa.

[0108] Example 5

[0109] In this embodiment, fly ash is used as harmless solid waste, sodium carbonate and silicon carbide are used as foaming agents, and closed-cell-open-cell double-layer ceramics are prepared through processes such as ball milling, homogenization, drying, spreading, and heat treatment. The open-cell part of the closed-cell-open-cell double-layer ceramics uses sodium carbonate and silicon carbide as composite foaming agents, wherein sodium carbonate accounts for 10% of the harmless solid waste (dry weight), and silicon carbide accounts for 2% of the harmless solid waste (dry weight); the closed-cell part of the closed-cell-open-cell double-layer ceramics uses silicon carbide as a foaming agent, wherein silicon carbide accounts for 2% of the harmless solid waste (dry weight); polyethylene glycol is used as a phase change energy storage material, and the closed-cell-open-cell double-layer ceramics are used as a carrier to prepare heat storage-insulation multifunctional ceramics by vacuum impregnation. Its main preparation steps are:

[0110] (1) Weighing fly ash, sodium carbonate and silicon carbide were wet-milled, with a ball-to-material ratio of 2:1 and a ball-to-material ratio of 1:1 during the ball milling process. The ball milling time was 6 hours. After the ball milling was completed, the mixture was sieved through an 8-mesh mesh cloth to obtain a first ball milling material;

[0111] (2) homogenizing the first ball mill material, with a stirring speed of 2.0 r / min and a homogenization time of 6 h. After the homogenization is completed, sieving through a 60-mesh sieve to obtain a first homogenized material;

[0112] (3) spray drying the first homogenized material to obtain a first dried material;

[0113] (4) Wet ball milling the weighed fly ash and silicon carbide, with a ball-to-material ratio of 2:1 and a ball-to-material ratio of 1:1 during the ball milling process, and the ball milling time is 6 hours. After the ball milling is completed, the mixture is sieved through an 8-mesh mesh cloth to obtain a second ball mill material;

[0114] (5) homogenizing the second ball mill material, with a stirring speed of 2.0 r / min and a homogenization time of 6 h. After the homogenization is completed, sieving through a 60-mesh sieve to obtain a second homogenized material;

[0115] (6) spray drying the second homogenized material to obtain a second dried material;

[0116] (7) Weaving the first dry material to obtain a first raw embryo, and weaving the second dry material based on the first raw embryo to obtain a second raw embryo; wherein the thickness of the first dry material is the same as the thickness of the second dry material;

[0117] (8) placing the second green embryo in a muffle furnace for heat treatment, during the heat treatment process, heating from room temperature to 800° C. at a heating rate of 10° C. / min, keeping the temperature for 60 min, and then heating to 1200° C. at a heating rate of 10° C. / min, keeping the temperature for 60 min, and cooling to room temperature with the furnace temperature after sintering to obtain a closed-pore-open-pore double-layer ceramic;

[0118] (9) Weighing closed-cell-open-cell double-layer ceramics and polyethylene glycol and placing them in a beaker, the mass ratio of the closed-cell-open-cell double-layer ceramics to the polyethylene glycol is 1:20; placing the beaker in a vacuum drying oven, setting the temperature of the vacuum drying oven to 80°C, and then vacuum impregnating for 2 hours to obtain heat storage-insulation multifunctional ceramics.

[0119] The heat storage-insulation multifunctional ceramic prepared in this embodiment has a true porosity of 95.1%, a closed porosity of 89.3%, and a thermal conductivity of 0.006 W·m -1 ·k -1 The phase change energy storage temperature of the heat storage ceramic part of the heat storage-insulation multifunctional ceramic is 58.7℃, and the phase change enthalpy is 156.2J / g; the thermal conductivity is 0.12W·m -1 ·k -1 The compressive strength of the heat storage-insulation multifunctional ceramic is 17.63MPa and the flexural strength is 4.79MPa.

[0120] In summary, the present invention provides a method for preparing a heat storage-insulation multifunctional ceramic. First, using harmless solid waste, sodium carbonate and silicon carbide as raw materials, a first dry material is obtained through ball milling, homogenization, drying and other processes, and using harmless solid waste and silicon carbide as raw materials, a second dry material is obtained through ball milling, homogenization, drying and other processes; secondly, the first dry material is spread to obtain a first green embryo, and the second dry material is spread on the basis of the first green embryo to obtain a second green embryo, and the spreading thickness of the first dry material is equal to the spreading thickness of the second dry material, so that A double-layer ceramic material foundation is constructed; then, the second green embryo is heat-treated, during which a layer of green embryo containing sodium carbonate and silicon carbide decomposes to produce gas, forming pores, thereby constructing an open-porous ceramic layer; a layer of green embryo containing silicon carbide decomposes to produce gas, forming pores, thereby constructing a closed-porous ceramic layer, that is, a closed-porous-open-porous double-layer ceramic is obtained after heat treatment; finally, the closed-porous-open-porous double-layer ceramic is vacuum-impregnated in a phase change energy storage material, so that the open-porous ceramic layer is filled with the phase change energy storage material to realize the heat storage function, and the closed-porous ceramic layer realizes the heat insulation function.

[0121] The present invention constructs a closed-cell-open-cell double-layer ceramic-based composite phase-change energy storage material. The phase-change energy storage material loaded by the open-cell ceramic part has good heat storage / release characteristics. The closed-cell ceramic part is used for a rich closed-cell structure, which makes it have a lower thermal conductivity. While realizing the heat supply of the phase-change energy storage material to the heat-requiring space, it can also ensure that the heat rich in the phase-change energy storage material is less lost to the outside world, reflecting the "insulation-heating" multifunctional characteristics of heat storage-insulation multifunctional ceramics. The present invention not only gives heat storage-insulation multifunctional ceramics different functional characteristics, but also has a simple preparation process, low cost, and easy industrialization, and has potential application value in the field of building insulation.

[0122] Finally, it should be noted that the terms "comprises," "includes," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements that are inherent to such process, method, article, or apparatus.

[0123] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0124] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing a heat storage-insulation multifunctional ceramic, characterized in that: The preparation method comprises: Ball-milling the harmless solid waste and the composite foaming agent to obtain a first ball-milled material; the composite foaming agent is composed of sodium carbonate and silicon carbide; Homogenizing the first ball mill material to obtain a first homogenized material; spray drying the first homogenized material to obtain a first dry material; ball-milling the harmless solid waste and silicon carbide to obtain a second ball-milled material; homogenizing the second ball mill material to obtain a second homogenized material; spray drying the second homogenized material to obtain a second dried material; The first dry material is spread to obtain a first raw embryo, and the second dry material is spread on the basis of the first raw embryo to obtain a second raw embryo; the thickness of the first dry material is the same as the thickness of the second dry material; heat treating the second green body to obtain a closed-pore-open-pore double-layer ceramic; The closed-pore-open-pore double-layer ceramic and the phase-change energy storage material are placed in a beaker and vacuum impregnated to obtain a heat storage-insulation multifunctional ceramic; The method of ball-milling the harmless solid waste and silicon carbide to obtain the second ball mill material specifically includes: wet ball-milling the weighed harmless solid waste and silicon carbide, wherein the ball-to-material ratio during the ball milling process is 1:1 to 3:1, and the ball milling time is 2 to 6 hours. After the ball milling is completed, the second ball mill material is sieved through an 8-mesh mesh cloth to obtain the second ball mill material; wherein the mass of the silicon carbide is 1% to 3% of the dry weight of the harmless solid waste; The step of homogenizing the second ball mill material to obtain the second homogenized material specifically comprises: homogenizing the second ball mill material, wherein the stirring speed during the homogenization process is 0.5 to 2.0 r / min, the homogenization time is 4 to 8 hours, and after the homogenization is completed, the second ball mill material is sieved through a 60-mesh sieve to obtain the second homogenized material; The step of heat treating the second green body to obtain the closed-pore-open-pore double-layer ceramic specifically includes: placing the second green body in a muffle furnace for heat treatment, heating the temperature from room temperature to 600-800° C. at a heating rate of 3-10° C. / min during the heat treatment, keeping the temperature for 30-90 min, continuing to heat the temperature to 1000-1250° C. at a heating rate of 3-10° C. / min, keeping the temperature for 30-90 min, and cooling the temperature to room temperature with the furnace temperature after sintering to obtain the closed-pore-open-pore double-layer ceramic; The method of placing the closed-pore-open-pore double-layer ceramic and the phase-change energy storage material in a beaker and performing vacuum impregnation to obtain the heat storage-insulation multifunctional ceramic specifically includes: weighing the closed-pore-open-pore double-layer ceramic and the phase-change energy storage material and placing them in a beaker, wherein the mass ratio of the closed-pore-open-pore double-layer ceramic to the phase-change energy storage material is 1:20; placing the beaker in a vacuum drying oven, setting the temperature of the vacuum drying oven to T, the phase change temperature of the phase change energy storage material to T0, the temperature difference between the temperature T and the phase change temperature T0 to ΔT, wherein ΔT=T-T0, and the ΔT is greater than 10°C; vacuum impregnating in the vacuum drying oven for 2 hours to obtain the heat storage-insulation multifunctional ceramic; The harmless solid waste includes at least one of lithium mica tailings, waste FCC harmless tailings and fly ash.

2. The method for preparing the heat storage-insulation multifunctional ceramic according to claim 1, characterized in that: The process of ball-milling the harmless solid waste and the composite foaming agent to obtain the first ball-milled material specifically comprises: The weighed harmless solid waste, sodium carbonate and silicon carbide are wet-milled with a ball-to-material ratio of 1:1 to 3:1 during the ball milling process, and the ball milling time is 2 to 6 hours. After the ball milling, the material is sieved through an 8-mesh mesh cloth to obtain a first ball mill material; wherein the mass of the sodium carbonate is 2% to 10% of the dry weight of the harmless solid waste, and the mass of the silicon carbide is 1% to 3% of the dry weight of the harmless solid waste.

3. The method for preparing the heat storage-insulation multifunctional ceramic according to claim 2, characterized in that: The step of homogenizing the first ball mill material to obtain a first homogenized material specifically includes: The first ball mill material is homogenized, the stirring speed during the homogenization process is 0.5-2 r / min, the homogenization time is 4-8 hours, and after the homogenization is completed, it is sieved through a 60-mesh sieve to obtain a first homogenized material.

4. A heat storage-insulation multifunctional ceramic, characterized in that: The heat storage-insulation multifunctional ceramic comprises a closed-pore-open-pore double-layer ceramic and a phase change energy storage material; Made by the preparation method of the heat storage-insulation multifunctional ceramic according to any one of claims 1 to 3; The closed-pore-open-pore double-layer ceramic comprises: A closed-cell ceramic layer, wherein the closed-cell ceramic layer is made by firing harmless solid waste and silicon carbide, and the closed-cell ceramic layer has a heat insulation function; An open-pored ceramic layer, wherein the open-pored ceramic layer is formed by firing harmless solid waste, sodium carbonate and silicon carbide, and the open-pored ceramic layer has a heat storage function after being loaded with a phase-change energy storage material; The harmless solid waste includes at least one of lithium mica tailings, waste FCC harmless tailings and fly ash; The phase change energy storage material includes at least one of paraffin, sodium sulfate decahydrate and polyethylene glycol.

Citation Information

Patent Citations

  • Intelligent temperature-adjusting decorative ceramic plate and preparation method thereof

    CN111792911A

  • Method for preparing ecological foamed ceramic from lepidolite tail mud full waste

    CN114907139A