Modified cathode materials, their preparation methods and applications

By introducing a carbon coating layer containing CF bonds into the cathode material, the problems of high viscosity and low solid content of the cathode material slurry were solved, the compaction density and capacity of the battery were improved, and the production cost was reduced.

CN117954593BActive Publication Date: 2026-11-17SHENZHEN DYNANONIC CO LTD +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311818839.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-26
Publication Date
2026-11-17
Estimated Expiration
2043-12-26

AI Technical Summary

Technical Problem

The existing cathode materials produce slurries with high viscosity and low solid content, resulting in low capacity of secondary batteries.

Method used

A carbon coating layer containing CF bonds is used. By adding a fluorinated carbon source during the sintering process, two tightly bonded coating regions are formed, which reduces the surface tension and surface energy of the carbon coating layer, reduces solvent absorption, and increases the solid content of the slurry.

Benefits of technology

Reducing slurry viscosity and increasing solid content enhances the compaction density of cathode materials and battery capacity, thereby reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117954593B_ABST
    Figure CN117954593B_ABST
Patent Text Reader

Abstract

This application relates to the field of lithium-ion battery technology, and more particularly to modified cathode materials, their preparation methods, and applications. The modified cathode material includes a core and a carbon coating layer. The core contains the cathode material, and the carbon coating layer coats the core. The carbon coating layer includes a first coating region close to the core and a second coating region away from the core, the second coating region containing C-F bonds. These C-F bonds help reduce the surface tension and surface energy of the carbon coating layer. When this modified cathode material is used to prepare slurry, it can reduce solvent absorption, lower the discharge viscosity, and increase the solid content of the slurry, thereby increasing the compaction density of the prepared electrode and improving the capacity of the prepared battery. The preparation method involves sintering a precursor including the cathode material and a carbon source in a protective atmosphere; wherein a fluorinated carbon source is also added during the sintering process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of lithium-ion battery technology, and in particular to modified cathode materials, their preparation methods and applications. Background Technology

[0002] The cathode material is a crucial factor determining the performance of lithium-ion batteries. Common cathode materials include phosphate-based cathode materials and lithium-containing metal oxide cathode materials. Among them, lithium iron phosphate has become a widely commercialized cathode material due to its low price, non-toxicity, high operating voltage platform, long cycle life, and good safety.

[0003] However, the low conductivity of cathode materials such as lithium iron phosphate limits their rate performance and cycle life. To address this issue, existing technologies have explored modifications such as ion doping, surface coating, and particle nano-sizing. Among these, surface carbon coating not only enhances the conductivity of cathode materials like lithium iron phosphate but also inhibits particle growth, weakens electrode polarization, and thus improves rate performance and extends cycle life. However, carbon coating can lead to low solids content and high viscosity in the slurry prepared from lithium iron phosphate cathode materials. To ensure coating effectiveness, the slurry viscosity cannot be too high; otherwise, the resulting slurry will have a low solids content, reducing the cathode material content and resulting in low electrode compaction and cathode material loading, which is detrimental to the development of high-density, high-capacity batteries. Summary of the Invention

[0004] The purpose of this application is to provide a modified cathode material and its preparation method, aiming to solve the problems of high viscosity and low solid content in the slurry prepared from cathode materials in the prior art.

[0005] Another objective of this application is to provide a positive electrode and a secondary battery, which aims to solve the problem of low capacity of secondary batteries in the prior art.

[0006] To achieve the above-mentioned objectives, the technical solution adopted in this application is as follows:

[0007] In a first aspect, this application provides a modified cathode material, comprising:

[0008] The core contains positive electrode material;

[0009] A carbon coating layer that coats a core, wherein the carbon coating layer includes a first coating region close to the core and a second coating region far from the core, the second coating region containing CF bonds.

[0010] In this application, the modified cathode material contains a carbon coating layer that, in addition to carbon, also contains CF bonds, and the carbon coating layer comprises two coating regions. The second coating region contains CF bonds, which help reduce the surface tension and surface energy of the carbon coating layer. Thus, the carbon coating layer acts as a core coating layer, modifying the cathode material. Compared to existing cathode material preparation slurries, the preparation slurry using the modified cathode material of this application can reduce solvent absorption, lower the discharge viscosity, and simultaneously increase the solid content of the prepared slurry, thereby increasing the compaction density of the resulting electrode and improving the capacity of the battery.

[0011] Secondly, this application provides a method for preparing the modified cathode material described in the above application, comprising the following steps:

[0012] In a protective atmosphere, a precursor including a cathode material and a carbon source are sintered; a fluorinated carbon source is also added during the sintering process.

[0013] The preparation method of this application includes sintering a cathode material precursor and a carbon source to form the cathode material. During the sintering process, a fluorinated carbon source is added. The carbon source and the fluorinated carbon source, after sintering, form two tightly bonded, non-demarcated coating regions. The second coating region contains CF bonds, collectively forming a carbon coating layer that coats the cathode material, reducing the surface tension and surface energy of the carbon coating layer. Therefore, the preparation method of this application can produce the modified cathode material described in this application. During the preparation of the modified cathode material into a slurry, solvent absorption is reduced, which is beneficial for reducing slurry viscosity and increasing solid content. The preparation method is process-controllable, and the obtained modified cathode material has stable structure and physicochemical properties.

[0014] Thirdly, this application provides a positive electrode, including a current collector and a positive electrode active layer bonded to the current collector, wherein the positive electrode active layer contains the positive electrode material modified in the above application or the modified positive electrode material prepared by the preparation method of the above application.

[0015] Compared to existing technologies, the electrode slurry prepared by the modified cathode material of this application has low viscosity and high solid content, which can reduce the use of solvents (such as NMP) required for viscosity adjustment during slurry discharge, reduce the energy consumption of equipment during cathode sheet preparation, and significantly reduce production costs. Because the cathode active layer contains the modified cathode material described above, the cathode of this application has high compaction density, high energy density, and high capacity.

[0016] Fourthly, this application provides a secondary battery, including a positive electrode, which is the positive electrode described in this application.

[0017] Because the secondary battery of this application contains the positive electrode described above, the secondary battery of this application has high energy density and high capacity. Attached Figure Description

[0018] To more clearly illustrate the technical solutions in the embodiments of this application, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0019] Figure 1 This is a schematic diagram of the structure of the modified cathode material according to an embodiment of this application;

[0020] Figure 2 This is a TEM image of the modified cathode material in Example A2;

[0021] Figure 3 These are TEM images of the modified cathode material in Comparative Example A1;

[0022] Figure 4 These are the 0.1C charge-discharge curves of the lithium-ion batteries in Example B2 and Comparative Example B2;

[0023] Figure 5 These are the 1C charge / discharge curves of lithium-ion batteries in Example B1 and Comparative Example B2.

[0024] Figure label:

[0025] 1-Nucleus; 2-Carbon coating. Detailed Implementation

[0026] To make the technical problems, technical solutions, and beneficial effects of this application clearer, the following detailed description is provided in conjunction with embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the scope of this application.

[0027] In this application, the term "and / or" describes the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, or B existing alone. A and B can be singular or plural. The character " / " generally indicates that the preceding and following related objects have an "or" relationship.

[0028] In this application, "at least one" means one or more, and "more than one" means two or more. "At least one of the following" or similar expressions refer to any combination of these items, including any combination of single or multiple items. For example, "at least one of a, b, or c", or "at least one of a, b, and c", can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple.

[0029] It should be understood that in the various embodiments of this application, the order of the above processes does not imply the order of execution. Some or all steps may be executed in parallel or sequentially. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of this application.

[0030] The terminology used in the embodiments of this application is for the purpose of describing particular embodiments only and is not intended to be limiting of this application. The singular forms "a" and "the" as used in the embodiments of this application and the appended claims are also intended to include the plural forms, unless the context clearly indicates otherwise.

[0031] The weights of the relevant components mentioned in the embodiments of this application can refer not only to the specific content of each component, but also to the proportional relationship between the weights of the components. Therefore, any scaling up or down of the content of the relevant components according to the embodiments of this application is within the scope disclosed in the embodiments of this application. Specifically, the mass in the embodiments of this application can be a well-known unit of mass in the chemical industry, such as μg, mg, g, or kg.

[0032] The terms "first" and "second" are used for descriptive purposes only, to distinguish objects, such as substances, from one another, and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. For example, without departing from the scope of the embodiments of this application, "first XX" may also be referred to as "second XX," and similarly, "second XX" may also be referred to as "first XX." Thus, features defined with "first" and "second" may explicitly or implicitly include one or more of that feature.

[0033] The first aspect of this application provides a modified cathode material. As an embodiment of this application, the structure of the modified cathode material is as follows: Figure 1 As shown, it includes a core 1 and a carbon coating layer 2, with the carbon coating layer 2 coating the core 1. The core 1 contains a positive electrode material, and the carbon coating layer 2 includes a first coating region close to the core 1 and a second coating region away from the core, the second coating region containing CF bonds.

[0034] The coating region refers to two regions in the carbon coating layer 2. The two regions belong to the carbon coating layer 2 as a whole, but the different regions contain different components. The different regions are tightly bound together and there is no clear boundary. Therefore, the two coating regions do not mean that there are two layers in the carbon coating layer 2.

[0035] In this embodiment of the modified cathode material, the carbon coating layer 2 contains not only carbon material but also CF bonds, and the carbon coating layer 2 includes two coating regions. The second coating region contains CF bonds, which help reduce the surface tension and surface energy of the carbon coating layer 2. Thus, the carbon coating layer 2 acts as a coating layer for the core 1, modifying the cathode material. Compared with existing cathode material preparation slurries, the preparation slurry of the modified cathode material in this embodiment can reduce solvent absorption, lower the discharge viscosity, and increase the solid content of the prepared slurry, thereby increasing the compaction density of the obtained electrode and improving the capacity of the obtained battery.

[0036] Regarding nucleus 1:

[0037] The core 1 contains a positive electrode material. The type of positive electrode material is not limited; it can be a phosphate-based positive electrode material, a lithium metal oxide-containing positive electrode material, etc. In the embodiments, it may include at least one of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, lithium manganese iron phosphate, lithium vanadium phosphate, lithium vanadium oxide phosphate, lithium fluorinated vanadium phosphate, lithium titanate, lithium nickel cobalt manganese oxide, and lithium nickel cobalt aluminum oxide. In some embodiments, the positive electrode material includes at least one of lithium iron phosphate and lithium manganese iron phosphate. Due to the technical problem of low conductivity, lithium iron phosphate and lithium manganese iron phosphate, after carbon coating modification, result in a slurry with high viscosity and low solid content. The modified positive electrode material in the embodiments of this application greatly improves the solid content and reduces the viscosity of the obtained slurry, solving the above-mentioned technical problems.

[0038] Regarding carbon coating layer 2

[0039] A carbon coating layer 2 coats the core 1. In some embodiments, the total thickness of the carbon coating layer 2 is 2–10 nm. In exemplary examples, it may include, but is not limited to, 2 nm, 4 nm, 6 nm, 8 nm, 10 nm, and any two of these values. These thicknesses of the carbon coating layer 2 are beneficial for improving the conductivity of the modified cathode material, further reducing surface tension and binding energy, and improving the processing performance of the modified cathode material.

[0040] The carbon coating layer 2 contains carbon material, which can be amorphous carbon. The first coating region contains carbon material, and in some embodiments, the second coating region also contains carbon material. The carbon material in the first coating region can be continuous or discontinuous, and the components in the second coating region can cover the less dense portions of the first coating region, increasing the continuity of the carbon coating layer. Furthermore, the second coating region contains CF bonds, which is beneficial for improving the processing performance of the modified cathode material.

[0041] In some embodiments, the thickness of the first coating region is 1–8 nm. In exemplary embodiments, it may include, but is not limited to, 1 nm, 3 nm, 5 nm, 8 nm, or any two of these values. In some embodiments, the mass content of the first coating region in the modified cathode material may be 0.8%–1.2%. In exemplary embodiments, it may include, but is not limited to, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, or any two of these values. These thicknesses or mass contents of the first coating region are beneficial for improving the conductivity and other properties of the modified cathode material.

[0042] The second coating region of the carbon coating layer 2 contains CF bonds. In some embodiments, the thickness of the second coating region is 1–3 nm. In exemplary embodiments, it may include, but is not limited to, 1 nm, 1.5 nm, 2 nm, 2.5 nm, 3 nm, and any two of these values. In some embodiments, the mass content of the second coating region in the modified cathode material is 0.2%–0.4%. In exemplary embodiments, it may include, but is not limited to, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, and any two of these values. These thicknesses or mass contents of the second coating region are beneficial for improving the modification effect of CF bonds on the carbon coating layer 2, reducing surface tension and binding energy, and improving the processing performance of the modified cathode material.

[0043] Therefore, by setting a carbon coating layer 2 including a first coating region and a second coating region, the conductivity and other properties of the modified cathode material can be effectively improved. More importantly, the surface tension and surface energy of the carbon coating layer 2 are further reduced. As a coating layer of the core 1, the carbon coating layer 2 modifies the cathode material, which is beneficial to improving the processing performance of the modified cathode material.

[0044] The second aspect of this application provides a method for preparing the modified cathode material described in the above-described embodiments, comprising the following steps:

[0045] S10. In a protective atmosphere, a precursor including a cathode material and a carbon source are sintered; wherein, a fluorinated carbon source is added during the sintering process.

[0046] The preparation method of this application includes sintering a cathode material precursor and a carbon source to form the cathode material. During the sintering process, a fluorinated carbon source is added. The carbon source and the fluorinated carbon source, after sintering, form two tightly bonded, non-demarcated coating regions. The second coating region contains CF bonds, collectively forming a carbon coating layer that coats the cathode material, reducing the surface tension and surface energy of the carbon coating layer. Therefore, the preparation method of this application can produce the modified cathode material described in the previous application. During the slurry preparation of the modified cathode material, solvent absorption can be reduced, which is beneficial for reducing slurry viscosity and increasing solid content. The preparation method is process-controllable, and the obtained modified cathode material has stable structure and physicochemical properties.

[0047] The precursor of the cathode material in step S10 can be used to prepare the cathode material. The type of cathode material can refer to the types of cathode materials modified in the embodiments of the above application. In the example, it can include at least one of lithium iron phosphate and lithium manganese iron phosphate. The precursor of the cathode material can be prepared by liquid phase method, solid phase method, etc. In the example, it can include at least one of lithium iron phosphate precursor and lithium manganese iron phosphate precursor.

[0048] The protective atmosphere during the sintering process can be an oxygen-isolated atmosphere, which may include at least one of nitrogen, argon, and helium.

[0049] The addition of a fluorocarbon source can be achieved by continuously or discontinuously transporting the fluorocarbon source to the sintering environment through methods such as gasification or atomization, followed by vapor deposition during sintering to ultimately form a carbon coating layer together with the carbon source. Alternatively, the sintering process can be carried out in stages, with the fluorocarbon source mixed with the sintered material after one stage has cooled before the sintering process continues. Of course, a combination of these methods can also be used to form the carbon coating layer.

[0050] The sintering temperature should be at least high enough to allow the fluorinated carbon source and carbon source to react at high temperatures to form CF bonds and carbon materials. In the embodiments, this can be 550–650°C. In the exemplary embodiments, this includes, but is not limited to, 550°C, 580°C, 600°C, 620°C, 650°C, and any two of these values. Furthermore, the sintering temperature should be at least high enough to allow the precursor of the cathode material to react at high temperatures to form the cathode material. In the embodiments, this can be 450–780°C. In the exemplary embodiments, this includes, but is not limited to, 450°C, 500°C, 600°C, 700°C, 780°C, and any two of these values. Additionally, the sintering time should be at least long enough to form the cathode material and the carbon coating layer.

[0051] Therefore, the sintering process can be carried out in stages, and staged sintering can better control the particle size and crystallinity of the cathode material particles. The two optional methods of step S10 will be further described below: (1) and (2). Both methods are carried out in a protective atmosphere, and the relevant content of the protective atmosphere will not be repeated below.

[0052] In some embodiments, the sintering process includes any one of the following methods (1) and (2):

[0053] Regarding method (1), the following steps are included:

[0054] S11. The precursor is pre-sintered to obtain a pre-sintered product;

[0055] S12. After mixing the pre-sintered product with the carbon source, a post-sintering treatment is performed, and a fluorinated carbon source is added during the post-sintering treatment.

[0056] (1) The method is divided into two-stage sintering: pre-sintering treatment and post-sintering treatment. This can better form a carbon coating layer containing two coating regions, and the carbon coating layer coats the cathode material to obtain a modified cathode material.

[0057] The preparation method of the cathode material precursor in step S11 can be referred to the above. In the embodiment, the preparation method of the lithium iron phosphate precursor involves placing a lithium source, an iron source, and a phosphorus source in a ball mill jar according to a certain stoichiometric ratio, adding a certain amount of dispersant, ball milling for a period of time, and then drying to obtain the cathode material precursor. The lithium source can be at least one of lithium acetate, lithium nitrate, lithium carbonate, and lithium hydroxide, and the actual amount of lithium source added can be 5% more than the stoichiometric ratio; the iron source can be at least one of ferric acetate, ferric nitrate, ferric sulfate, and ferrous sulfate; and the phosphorus source can be at least one of ammonium dihydrogen phosphate and diammonium hydrogen phosphate. In addition, a reducing carbon source can be added to the ball mill jar to fully reduce the metal elements in the raw materials, ensuring the activity of the cathode material. Furthermore, the reducing carbon source can provide carbon, which helps in the subsequent formation of the carbon coating layer. The reducing carbon source can be a carbon source containing only C, H, and O elements. In the examples, it can include at least one of glucose, polyethylene glycol (PEG), citric acid, and sucrose. The addition ratio can be 1% to 20% of the sum of the mass of the lithium source, iron source, and phosphorus source. The dispersant can be at least one of water and ethanol. The ratio of solid raw materials to dispersant can be 1:(1.5 to 3). The ball milling speed is 360 to 480 r / min, and the ball milling time is 6 to 8 h.

[0058] In some embodiments, the pre-sintering temperature can be 450–550°C, the holding time can be 4–8 hours, and the temperature can be increased to the pre-sintering temperature at a heating rate of 2–5°C / min. The pre-sintered product, i.e., the prototype of the cathode material, is obtained after the pre-sintering treatment.

[0059] In some embodiments, the carbon source in step S12 can be at least one of glucose, polyethylene glycol (PEG), citric acid, and sucrose, and the addition ratio can be 1% to 15% of the pre-sintered product.

[0060] In some embodiments, the temperature of the post-sintering treatment can be 680 to 780°C. In exemplary cases, it can be, but is not limited to, 680°C, 700°C, 730°C, 750°C, 780°C and any two of these values. The holding time can be 4 to 8 hours, and the temperature can be increased to the post-sintering treatment temperature at a heating rate of 2 to 5°C / min.

[0061] In some embodiments, the fluorocarbon source can be deposited via vapor deposition, either in a gaseous or atomized form into the post-sintering environment. In some embodiments, the fluorocarbon source is introduced into the post-sintering environment at a flow rate of 150–500 mL / min. This method allows the fluorocarbon source to form CF-bonded deposited carbon through vapor deposition (CVD) followed by post-sintering, forming a carbon coating layer with the carbon source. The carbon coating layer has two coating regions, with the region furthest from the core containing CF bonds.

[0062] In some embodiments, the fluorocarbon source can also be dissolved in a volatile organic solvent, such as ethanol, acetone, toluene, benzene, or diethyl ether, to prepare a solution for vapor deposition. The mass ratio of the fluorocarbon source can be 5 wt% to 15 wt%, and in exemplary cases, it can include, but is not limited to, 5 wt%, 8 wt%, 10 wt%, 12 wt%, 15 wt%, and any two of these values. The solubility can be 50 to 300 mL / kg, and in exemplary cases, it can include, but is not limited to, 50 mL / kg, 100 mL / kg, 150 mL / kg, 200 mL / kg, or 300 mL / kg. After atomization, the solution is introduced into the post-sintering environment, or vaporized and introduced into the post-sintering environment. The flow rate can be 50 to 300 mL / min, and in exemplary cases, it can include, but is not limited to, 50 mL / min, 100 mL / min, 150 mL / min, 200 mL / min, 300 mL / min, and any two of these values. A fluorocarbon source is introduced using a protective gas as the carrier gas. The methods for preparing these parameters can further improve the vapor deposition effect.

[0063] In some embodiments, the fluorocarbon source can be a volatile fluorinated organic compound, including at least one of difluorostyrene, 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, hexafluoroisopropanol, etc. These fluorocarbon sources are suitable for vapor deposition and can better form the desired carbon coating layer.

[0064] Regarding method (2), the following steps are included:

[0065] S21. The precursor is subjected to a first sintering treatment to obtain a first-sintering product;

[0066] S22. The product from the first calcination is mixed with a carbon source and then subjected to a second sintering process to obtain the product from the second calcination.

[0067] S23. The second sintering product is subjected to a third sintering treatment, wherein a fluorinated carbon source is added during the third sintering treatment.

[0068] Through this three-stage sintering process, the first sintering product is the prototype of the cathode material, the second sintering product is the cathode material coated with carbon material, and then a third sintering process is carried out. In the process, a fluorinated carbon source is added to better form a carbon coating layer containing two coating regions, and the carbon coating layer coats the cathode material to obtain a modified cathode material.

[0069] Steps S21 and S22 are steps for preparing the second sintering product, namely the cathode material coated with carbon material. In some embodiments, the preparation method of the cathode material precursor, the temperature control method of the first sintering treatment (refer to the pre-sintering treatment), the amount of carbon source, and the temperature control method of the second sintering treatment (refer to the post-sintering treatment) in method (2) can all refer to the relevant content in method (1), the difference being that no fluorinated carbon source is added.

[0070] Step S23 is the third sintering process. In some embodiments, the temperature of the third sintering process is 550-650°C. In exemplary cases, it may include, but is not limited to, 550°C, 580°C, 600°C, 630°C, 650°C and any two of these values, in order to produce the modified cathode material of the embodiments described in this application.

[0071] In some embodiments, step S23 includes at least one of the following methods (21) and (22):

[0072] (21) Method: S231. A fluorocarbon source is introduced into the environment of the third sintering treatment at a certain flow rate;

[0073] (22) Method: S232. Mix the fluorocarbon source with the second sintering product and then perform a third sintering treatment.

[0074] Both methods can form a carbon coating layer with two coating regions, and methods (21) and (22) can be used in combination.

[0075] Regarding method (21):

[0076] The type of fluorocarbon source added, the method of addition, and the flow rate in step S231 can refer to the vapor deposition method in method (1) above. In this method, after the second sintering treatment in step S22 is completed, the temperature can be kept at 550-650℃ for 4-8 hours.

[0077] Regarding method (22):

[0078] In step S232, a fluorocarbon source is mixed with the secondary calcination product, and the fluorocarbon source is coated on the surface of the secondary calcination product. After a third sintering treatment, the modified cathode material of the above-described embodiment can be obtained.

[0079] In some embodiments, the fluorocarbon source accounts for 0.3% to 5% of the mass of the dicalcined product. In exemplary embodiments, this may include, but is not limited to, 0.3%, 0.8%, 1.5%, 3%, 5%, and any two of these values. In some embodiments, the fluorocarbon source may be a non-volatile solid fluorocarbon source, which may include at least one of polyvinylidene fluoride (PVDF), 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, and perfluorododecanoic acid.

[0080] In some embodiments, the mixing is carried out by ball milling or other methods. After the second sintering treatment is completed and the temperature is cooled to room temperature, the second sintering product is mixed with a fluorocarbon source, and then heated to the temperature of the third sintering treatment at a heating rate of 0.5 to 5 °C / min and held at that temperature for 4 to 10 hours.

[0081] The above methods are optional and do not constitute a limitation on the preparation method of the embodiments of this application. All of the above methods can ultimately produce the modified cathode material of the embodiments of this application, but the addition methods are different, and the process flow, energy consumption, and cost are also different in actual production. The methods can be used in combination.

[0082] A third aspect of this application provides a positive electrode, including a current collector and a positive electrode active layer bonded to the current collector, wherein the positive electrode active layer contains a modified positive electrode material as described in the above application embodiments or a modified positive electrode material prepared by the preparation method described in the above application embodiments.

[0083] In some embodiments, the positive electrode active layer may contain binders and conductive agents in addition to the modified positive electrode material. In these embodiments, the binder may be a commonly used electrode binder, such as at least one selected from polyvinylidene chloride, soluble polytetrafluoroethylene, styrene-butadiene rubber, hydroxypropyl methylcellulose, methylcellulose, carboxymethyl cellulose, polyvinyl alcohol, acrylonitrile copolymer, sodium alginate, chitosan, and chitosan derivatives. In these embodiments, the conductive agent may be a commonly used conductive agent, such as at least one selected from graphite, carbon black, acetylene black, graphene, carbon fiber, C60, and carbon nanotubes. Of course, the positive electrode active layer may also contain other electrode active materials, such as at least one selected from lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, lithium manganese iron phosphate, lithium vanadium phosphate, lithium vanadium oxide phosphate, lithium fluorinated vanadium phosphate, lithium titanate, lithium nickel cobalt manganese oxide, and lithium nickel cobalt aluminum oxide.

[0084] In this embodiment, the positive electrode preparation process can be as follows: mixing positive electrode active material, conductive agent, and binder to obtain electrode slurry; coating the electrode slurry onto a current collector; and preparing the positive electrode sheet through steps such as drying, rolling, and die-cutting. Compared with the prior art, the electrode slurry prepared from the modified positive electrode material in this embodiment has low viscosity and high solid content. The solid content of the slurry prepared from the positive electrode material in the prior art is increased by at least 4%, which can reduce the use of solvents (e.g., NMP) required to adjust the viscosity during the slurry discharge process, reduce the energy consumption of equipment in the positive electrode sheet preparation process, and greatly reduce production costs.

[0085] In the embodiment, conductive carbon black (SP) and PVDF were added in a mass ratio of modified cathode material:SP:PVDF = 96.5:1.3:2.2. The mixture was stirred and dispersed according to the existing technical process. N-methylpyrrolidone (NMP) was added according to the designed solid content. The discharge viscosity was suitable for subsequent coating, and the solid content was significantly improved, resulting in ideal processing performance.

[0086] The positive electrode active layer contains the modified positive electrode material described in the above-mentioned application embodiments, so the positive electrode of this application embodiments has high compaction density, high energy density, and high capacity.

[0087] The fourth aspect of this application provides a secondary battery, including a positive electrode, which is the positive electrode of the above-described embodiment.

[0088] The secondary battery of this application embodiment includes essential components such as a positive electrode, a negative electrode, a separator, and an electrolyte, as well as other necessary or auxiliary components. The positive electrode is the positive electrode described in this application embodiment, meaning that the positive electrode active layer contains the modified positive electrode material described in the application embodiment above. Because the secondary battery of this application embodiment contains the modified positive electrode material described in the application embodiment above, the secondary battery of this application embodiment has high energy density and high capacity.

[0089] The following description is based on specific embodiments.

[0090] Example A1

[0091] This embodiment provides a modified cathode material and its preparation method. The modified cathode material includes a core and a carbon coating layer. The core contains lithium iron phosphate, and the carbon coating layer includes a first coating region close to the core and a second coating region away from the core. The first coating region contains amorphous carbon, and the second coating region contains CF bonds.

[0092] The method for preparing the modified cathode material, using the method described in (21) above, includes the following steps:

[0093] S1: First sintering treatment

[0094] Lithium carbonate, ferric nitrate, and ammonium dihydrogen phosphate were dissolved in an ethanol-water solution at a molar ratio of 0.525:1:1, with the ethanol-water solution having a mass twice that of the total lithium, iron, and phosphorus sources. Glucose (acting as a reducing carbon source, reducing iron and providing some carbon) was added to the solution at 10% of the total mass of the lithium, iron, and phosphorus sources. Zirconium beads were then added, and the mixture was ball-milled at 360 rpm for 8 hours. The resulting product was then dried in an oven at 80°C to obtain the precursor. The precursor was then subjected to a first sintering treatment in a tube furnace under a nitrogen atmosphere, with the temperature increased to 530°C at a rate of 5°C / min and held for 6.5 hours. After cooling, the first-sintered product was obtained.

[0095] S2: Second sintering treatment

[0096] After crushing the first calcination product of step S1, glucose (carbon source) at a mass ratio of 3% of the first calcination product is uniformly mixed in, and then the temperature is raised to 750℃ at 5℃ / min and held for 8 hours in a tube furnace to obtain the second calcination product.

[0097] S3: Third sintering treatment

[0098] After the heat preservation in step S2 is completed, the temperature is lowered to 600°C at 2°C / min. An ethanol solution containing hexafluoroisopropanol (containing a fluorocarbon source) is continuously introduced into the solution using nitrogen gas. The concentration of hexafluoroisopropanol in the solution is 10%, and the flow rate is 0.3 L / min. The third sintering treatment is carried out at 600°C. After heat preservation for 5 hours, the temperature is naturally lowered to obtain the modified cathode material of this embodiment.

[0099] Example A2

[0100] This embodiment provides a modified cathode material and its preparation method. The only difference from Embodiment A1 is that the flow rate in step S3 is changed to 0.1 L / min, while all other aspects are the same.

[0101] The modified cathode material in this embodiment was prepared using the method described in this embodiment.

[0102] Example A3

[0103] This embodiment provides a modified cathode material and its preparation method. The only difference from Embodiment A1 is that the fluorinated carbon source in step S3 is replaced with difluorostyrene, and all other aspects are the same.

[0104] The modified cathode material in this embodiment was prepared using the method described in this embodiment.

[0105] Example A4

[0106] This embodiment provides a modified cathode material and its preparation method. The only difference from Example A1 is that the fluorinated carbon source in step S3 is replaced with 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether. All other aspects are the same.

[0107] The modified cathode material in this embodiment was prepared using the method described in this embodiment.

[0108] Example A5

[0109] This embodiment provides a modified cathode material and its preparation method. The modified cathode material includes a core and a carbon coating layer. The core contains lithium iron phosphate, and the carbon coating layer includes a first coating region close to the core and a second coating region away from the core. The first coating region contains amorphous carbon, and the second coating region contains CF bonds.

[0110] The method for preparing the modified cathode material, using method (1) in the above-mentioned specification, includes the following steps:

[0111] S1: Pre-sintering treatment

[0112] Lithium carbonate, ferric nitrate, and ammonium dihydrogen phosphate were dissolved in an ethanol-water solution at a molar ratio of 0.525:1:1, with the ethanol-water solution having a mass twice that of the total lithium, iron, and phosphorus sources. Glucose (acting as a reducing carbon source, reducing iron and providing some carbon) was added to the solution at 10% of the total mass of the lithium, iron, and phosphorus sources. Zirconium beads were then added, and the mixture was ball-milled at 360 rpm for 8 hours. The resulting product was then dried in an oven at 80°C to obtain the precursor. The precursor was placed in a tube furnace and pre-sintered at 530°C for 6.5 hours under a nitrogen atmosphere, with the temperature increased at 5°C / min. After cooling, a pre-sintered product was obtained.

[0113] S2: Post-sintering treatment

[0114] After crushing the pre-sintered product from step S1, glucose (carbon source) at a mass ratio of 3% of the pre-sintered product is uniformly mixed in. At the same time, an ethanol solution containing hexafluoroisopropanol is continuously passed into the solution, with a concentration of hexafluoroisopropanol of 10% and a flow rate of 0.3 L / min. The solution is then heated to 750°C at a rate of 5°C / min and held for 8 hours. After sintering and cooling, the modified cathode material of this embodiment can be obtained.

[0115] Example A6

[0116] This embodiment provides a modified cathode material and its preparation method. The modified cathode material includes a core and a carbon coating layer. The core contains lithium iron phosphate, and the carbon coating layer includes a first coating region close to the core and a second coating region away from the core. The first coating region contains amorphous carbon, and the second coating region contains CF bonds.

[0117] The method for preparing the modified cathode material, using the method described in (22) above, includes the following steps:

[0118] S1: First sintering treatment

[0119] Lithium carbonate, ferric nitrate, and ammonium dihydrogen phosphate were dissolved in an ethanol-water solution at a molar ratio of 0.525:1:1, with the ethanol-water solution having a mass twice that of the total lithium, iron, and phosphorus sources. Glucose (acting as a reducing carbon source, reducing iron and providing some carbon) was added to the solution at 10% of the total mass of the lithium, iron, and phosphorus sources. Zirconium beads were then added, and the mixture was ball-milled at 360 rpm for 8 hours. The resulting product was then dried in an oven at 80°C to obtain the precursor. The precursor was then subjected to a first sintering treatment in a tube furnace under a nitrogen atmosphere, with the temperature increased to 530°C at a rate of 5°C / min and held for 6.5 hours. After cooling, the first-sintered product was obtained.

[0120] S2: Second sintering treatment

[0121] After crushing the product from step S1, glucose (carbon source) at a mass ratio of 3% of the product from the first calcination is uniformly mixed in. The product is then heated to 750°C at 5°C / min in a tube furnace and held for 8 hours. After cooling to room temperature, the product from the second calcination is obtained.

[0122] S3: Preparation of modified cathode materials

[0123] The dicalcined product obtained in step S2 was thoroughly mixed with PVDF (a fluorocarbon source) at a mass ratio of 1.5% of the dicalcined product. The mixture was placed in a tube furnace and heated to 600°C at a rate of 5°C / min under a nitrogen atmosphere. The temperature was then maintained for 6.5 hours. After the temperature maintenance was completed, the mixture was cooled to room temperature to obtain the modified cathode material of this embodiment.

[0124] Example A7

[0125] This embodiment provides a modified cathode material and its preparation method. The only difference from Example A6 is that the fluorinated carbon source in step S3 is replaced with 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane. All other aspects are the same.

[0126] The modified cathode material in this embodiment was prepared using the method described in this embodiment.

[0127] Example A8

[0128] This embodiment provides a modified cathode material and its preparation method. The only difference from Example A6 is that the fluorinated carbon source in step S3 is replaced with perfluorododecanoic acid, and all other aspects are the same.

[0129] The modified cathode material in this embodiment was prepared using the method described in this embodiment.

[0130] Comparative Example A1

[0131] This comparative example provides a carbon-coated modified cathode material and its preparation method. The modified cathode material includes a core and a carbon coating layer, wherein the core contains lithium iron phosphate and the carbon coating layer contains amorphous carbon and has no CF bonds.

[0132] The only difference between this comparative preparation method and Example A1 is that step S3 is omitted, and the calcined product (carbon-coated cathode material) obtained in step S2 is used as the modified cathode material in this comparative example.

[0133] Comparative Example A2

[0134] This comparative example provides a modified cathode material and its preparation method. The modified cathode material includes a core and a carbon coating layer. The core contains lithium iron phosphate, and the carbon coating layer contains amorphous carbon and CF bonds, which are randomly doped in the carbon coating layer.

[0135] The preparation method of modified cathode materials includes the following steps:

[0136] S1: Pre-firing treatment

[0137] Lithium carbonate, ferric nitrate, and ammonium dihydrogen phosphate were dissolved in an ethanol-water solution at a molar ratio of 0.525:1:1, with the ethanol-water solution having a mass twice that of the total lithium, iron, and phosphorus sources. Glucose (acting as a reducing carbon source, reducing iron and providing some carbon) was added to the solution at 10% of the total mass of the lithium, iron, and phosphorus sources. Zirconium beads were then added, and the mixture was ball-milled at 360 rpm for 8 hours. The resulting product was then dried in an oven at 80°C to obtain the precursor. The precursor was placed in a tube furnace and pre-calcined at 530°C for 6.5 hours under a nitrogen atmosphere, with the temperature increased at 5°C / min. After cooling, the pre-calcined material was obtained.

[0138] S2: Preparation of modified cathode materials

[0139] After crushing the pre-burned material obtained in step S1, PVDF accounting for 5% of the mass of the pre-burned material is mixed in, and the mixture is placed in a tube furnace and heated to 750℃ at 5℃ / min and held for 8 hours. After the holding period, the temperature is lowered to obtain the comparative modified cathode material.

[0140] The differences between Examples A1 to A8 and Comparative Examples A1 to A2 are shown in Table 1. In Table 1, "carbon source" refers to carbon sources other than fluorinated carbon sources, such as glucose in each case.

[0141] Table 1

[0142]

[0143] Example of a lithium-ion battery:

[0144] The modified cathode materials provided in Examples A1 to A8 and Comparative Examples A1 to A2 were assembled into cathode electrodes and lithium-ion batteries respectively according to the following methods:

[0145] Positive electrode: The modified positive electrode material, SP (conductive agent), and PVDF (solvent) were mixed in a mass ratio of 96.5:1.3:2.2 and ball-milled to obtain a positive electrode slurry. The positive electrode slurry was coated on the surface of aluminum foil, rolled, and vacuum dried overnight at 110°C to obtain a positive electrode sheet.

[0146] Negative electrode: Lithium metal sheet;

[0147] Electrolyte: Ethyl carbonate and methyl ethyl carbonate are mixed in a volume ratio of 3:7, and LiPF6 is added to form an electrolyte with a concentration of 1 mol / L.

[0148] Diaphragm: Polypropylene microporous diaphragm;

[0149] Lithium-ion battery assembly: Lithium-ion batteries are assembled in an inert atmosphere glove box according to the assembly sequence of negative electrode - separator - electrolyte - positive electrode.

[0150] In this example, the modified cathode material in Example A1 corresponds to the preparation of lithium-ion Example B1, the modified cathode material in Example A2 corresponds to the preparation of lithium-ion Example B2, and so on. The modified cathode material in Example A8 corresponds to the preparation of lithium-ion Example B8, the modified cathode material in Comparative Example A1 corresponds to the preparation of lithium-ion Comparative Example B1, and the modified cathode material in Comparative Example A2 corresponds to the preparation of lithium-ion Comparative Example B2.

[0151] Relevant performance tests and results analysis

[0152] 1. Relevant Tests for Modified Cathode Materials

[0153] 1.1 Thickness of the carbon coating layer

[0154] The modified cathode materials provided in Examples A1 to A8 and Comparative Examples A1 to A2 were tested by transmission electron microscopy (TEM), and the results are shown in Table 2.

[0155] The TEM image of comparative example A1 is shown below. Figure 3 It is a modified cathode material obtained by coating with a certain amount of glucose, and the total thickness of the carbon coating layer is 3.14 nm.

[0156] TEM image of Example A2 is shown below Figure 2 This is a modified cathode material obtained using the same amount of glucose and a certain amount of fluorinated carbon source. The carbon coating layer includes a first coating region and a second coating region, with no clear boundary between them. The total thickness of the carbon coating layer is 4.8 nm. Figure 2 , Figure 3 It can be seen that, Figure 2 The carbon coating in Figure 3 The carbon coating layer in it is thick.

[0157] 1.2 Slurry viscosity test

[0158] The modified cathode materials provided in Examples A1 to A8 and Comparative Examples A1 to A2 were prepared into slurries according to the following methods:

[0159] Weigh 20g of dry modified cathode material into a 100mL ball mill jar. Add the corresponding conductive carbon black (SP) and PVDF according to the mass ratio of modified cathode material:SP:PVDF = 96.5:1.3:2.2. Add the corresponding weight of N-methylpyrrolidone (NMP) according to the designed solid content. Add 10 zirconium beads with diameters of 10mm, 6mm and 3mm respectively, and ball mill at 480r / min for 6h. Then pour the slurry into a test tube and test it with an NDJ-8S digital viscometer. Select rotor 4 and speed 30 at 25℃. Take three parallel measurements and obtain the average value. The discharge viscosity and viscosity after standing for 24h for each case are shown in Table 2.

[0160] Table 2

[0161]

[0162]

[0163] Referring to Table 1, Table 2 shows that the modified cathode materials in Examples A1 to A8 of this application, when prepared into slurries using the same method as the modified cathode material in Comparative Example A1, exhibit lower slurry viscosity but higher solid content (up to 57%), resulting in better processing performance and improved density of the subsequently produced electrode sheets, thus increasing battery capacity. In contrast, the modified cathode material in Comparative Example A1 has a low solid content, but its slurry viscosity is very high (exceeding the instrument's measurement range), remaining above the range even after standing, indicating unsatisfactory processing performance.

[0164] It can also be seen that although the carbon coating layer of the modified cathode material in Comparative Example A2 also contains CF bonds, these CF bonds are randomly doped into the carbon coating layer. The solid content at discharge is low (only 53%). Although the slurry viscosity is low, it increases significantly after standing for 24 hours, exceeding the instrument's measurement range. Therefore, while randomly doping the carbon coating layer with CF bonds may improve processing performance to some extent, the resulting slurry is difficult to store, and subsequent processing performance remains unsatisfactory, failing to achieve the effects of the modified cathode material described in this application.

[0165] 2. Example of a lithium-ion battery:

[0166] The electrochemical performance of lithium-ion batteries from Examples B1 to B8 and Comparative Examples B1 to B2 was tested under the following conditions:

[0167] In a constant temperature test chamber, the electrochemical performance was tested at 25°C using a LAND blue electric current tester at charge-discharge rates of 0.1C, 1C, 2C, 3C, 5C, 10C, and 20C.

[0168] The 0.1C charge-discharge curves of the lithium-ion batteries in Example B2 and Comparative Example B2 are shown below. Figure 4 As shown, the 1C charge-discharge curves of the lithium-ion batteries in Example B1 and Comparative Example B2 are as follows: Figure 5 As shown; the test results are shown in Table 3 below:

[0169] Table 3

[0170]

[0171] Combining Tables 1 and 2, it can be seen from Table 3 that the modified cathode material prepared by various preparation methods in the embodiments of this application has a carbon coating layer containing two coating regions, and the second coating region contains CF bonds. In addition to the improved processing performance of the modified cathode material, the electrochemical performance of the battery is also improved.

[0172] from Figure 4 It can be seen that after adding a fluorinated carbon source to the preparation method, the second coating region of the carbon coating layer contains CF bonds, which improves the 0.1C charge-discharge performance of the battery made by modifying the cathode material.

[0173] from Figure 5 It can be seen that after adding a fluorinated carbon source to the preparation method, the second coating region of the carbon coating layer contains CF bonds, which improves the 1C charge-discharge performance of the battery made by modifying the cathode material.

[0174] The test results from Examples A1 and A6, and Examples B1 and B6 show that although the methods of adding fluorinated carbon sources differ, the second coating region of the carbon coating layer contains CF bonds, and the test results are similar. This indicates that different addition methods have little impact on the chemical rate performance of the battery prepared from the modified cathode material. Therefore, the preparation method of this application can effectively modify the cathode material by adding different fluorinated carbon sources.

[0175] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of this application should be included within the protection scope of this application.

Claims

1. A modified cathode material, characterized in that, include: The core contains positive electrode material; A carbon coating layer covers the core, wherein the carbon coating layer includes a first coating region close to the core and a second coating region away from the core, the second coating region containing CF bonds; the thickness of the second coating region is 1-3 nm; the mass content of the second coating region in the modified cathode material is 0.2%-0.4%; the thickness of the first coating region is 1-8 nm; the mass content of the first coating region in the modified cathode material is 0.8%-1.2%; the total thickness of the carbon coating layer is 2-10 nm; the cathode material includes at least one of lithium iron phosphate and lithium manganese iron phosphate.

2. The method for preparing the modified cathode material according to claim 1, characterized in that, Includes the following steps: In a protective atmosphere, a precursor comprising a cathode material and a carbon source are sintered; wherein, a fluorinated carbon source is also added during the sintering process.

3. The method for preparing the modified cathode material according to claim 2, characterized in that, The sintering process includes any one of the following methods (1) and (2): (1) The precursor is pre-sintered to obtain a pre-sintered product; The pre-sintered product is mixed with the carbon source and then subjected to post-sintering treatment, during which the fluorinated carbon source is added. (2) The precursor is subjected to a first sintering treatment to obtain a sintered product; The first calcination product is mixed with the carbon source and then subjected to a second sintering process to obtain the second calcination product. The second sintering product is subjected to a third sintering treatment, wherein the fluorinated carbon source is added during the third sintering treatment.

4. The preparation method according to claim 3, characterized in that: In the manner described in (1), The temperature of the pre-sintering treatment is 450–550°C; and / or The post-sintering treatment temperature is 680–780°C; and / or The fluorocarbon source is introduced into the post-sintering environment at a certain flow rate; and / or The fluorocarbon source includes at least one of difluorostyrene, 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, and hexafluoroisopropanol.

5. The preparation method according to claim 3, characterized in that: In the manner described in (2), The temperature of the first sintering treatment is 450–550 °C; and / or The temperature of the second sintering treatment is 680–780 °C; and / or The temperature of the third sintering treatment is 550–650°C.

6. The preparation method according to claim 3 or 5, characterized in that: The method (2) includes at least one of the following methods (21) and (22): (21) The fluorocarbon source is introduced into the environment of the third sintering treatment at a certain flow rate; (22) The fluorinated carbon source is mixed with the second sintering product and then subjected to the third sintering treatment.

7. The preparation method according to claim 6, characterized in that: In the manner described in (21), the fluorocarbon source includes at least one of difluorostyrene, 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, and hexafluoroisopropanol; and / or In the method described in (22), the fluorocarbon source includes at least one of polyvinylidene fluoride, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, and perfluorododecanoic acid; and / or In the method described in (22), the fluorocarbon source accounts for 0.3% to 5% of the mass of the dicalcined product.

8. A positive electrode, characterized in that: It includes a current collector and a positive electrode active layer bonded to the current collector, wherein the positive electrode active layer contains the modified positive electrode material according to claim 1 or the modified positive electrode material prepared by any one of claims 2-7.

9. A secondary battery, comprising a positive electrode, characterized in that: The positive electrode is the positive electrode as described in claim 8.

Citation Information

Patent Citations

  • Cathode material with low water content, preparation method thereof and lithium ion battery

    CN114899371A