A hydrophilic polytetrafluoroethylene microporous membrane, a preparation method and application thereof
By polymerizing and hydrolyzing condensation reactions on PTFE microporous membranes, a three-dimensional network is constructed to introduce hydrophilic groups, which solves the problems of poor hydrophilicity and insufficient stability of PTFE microporous membranes. This results in PTFE microporous membranes with high hydrophilicity and stability, suitable for water filtration equipment.
Patent Information
- Application Number
- CN202410216219.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-27
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-02-27
AI Technical Summary
The hydrophilicity of PTFE microporous membranes is not as expected and the stability of the hydrophilic network is insufficient, which limits their application in water filtration equipment.
By mixing polytetrafluoroethylene microporous membranes with alkenylamide-containing hydrophilic agents, alkenylsilane-containing crosslinking agents, free radical initiators, and organic solvents, a hydrophilic polytetrafluoroethylene microporous membrane is formed. A Si-O-Si structure is generated by hydrolysis and condensation reaction, and a three-dimensional network is constructed to densely introduce hydrophilic groups.
It significantly improves the hydrophilicity and stability of PTFE microporous membranes, reducing the initial water contact angle to below 88° and achieving a pure water flux of 2242 L/m2·h. After 14 days of continuous operation, the water contact angle remains below 95°, and the pure water flux still reaches 2137 L/m2·h. Moreover, it is simple to operate, safe and convenient, and has low energy consumption.
Smart Images

Figure CN117959943B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a hydrophilic polytetrafluoroethylene microporous membrane, its preparation method, and its application. Background Technology
[0002] Polytetrafluoroethylene (PTFE) microporous membranes are hydrophobic microporous films produced by premixing, extrusion, calendering, and unidirectional or bidirectional stretching of PTFE dispersion resin. They possess excellent chemical resistance, thermal stability, aging resistance, and electrical insulation properties. PTFE microporous membranes have a wide range of applications, such as separating and filtering liquids and gases, encapsulating semiconductors and electronic components, and producing high-performance cables and wires. However, PTFE's completely symmetrical carbon-fluorine bond structure and extremely low surface energy result in strong hydrophobicity, thus limiting the application of PTFE microporous membranes in water filtration equipment.
[0003] To address the aforementioned issues, hydrophilic modification of PTFE microporous membranes is typically required. Surface crosslinking is one of the commonly used methods for hydrophilic modification of PTFE microporous membranes. This method involves encapsulating substances containing hydrophilic groups onto the fibers of the PTFE microporous membrane through physical entanglement, thereby generating a relatively stable entangled structure. This method achieves hydrophilic modification without damaging the PTFE microporous membrane structure, and because it involves physical entanglement, a wide range of hydrophilic agents can be selected, making it of significant research value. However, in existing technologies, the surface crosslinking method still suffers from problems such as less-than-expected hydrophilic effects and insufficient stability of the hydrophilic network. Summary of the Invention
[0004] The technical problem this invention aims to solve is to overcome the shortcomings of PTFE microporous membranes, such as unsatisfactory hydrophilicity and insufficient stability of the hydrophilic network. This invention provides a hydrophilic polytetrafluoroethylene (PTFE) microporous membrane, its preparation method, and its applications. The preparation method of the hydrophilic PTFE microporous membrane provided by this invention can greatly improve the hydrophilicity of PTFE microporous membranes. Furthermore, the hydrophilically modified PTFE microporous membrane exhibits excellent stability. Moreover, the preparation method of this invention is simple, safe, convenient, and has low energy consumption.
[0005] This invention provides a method for preparing a hydrophilic polytetrafluoroethylene microporous membrane, which includes the following steps:
[0006] S1. Polytetrafluoroethylene microporous membrane is mixed with an alkenylamide-containing hydrophilic agent, an alkenylsilane-containing crosslinking agent, a free radical initiator and an organic solvent to carry out a polymerization reaction to obtain a precursor.
[0007] S2. The precursor undergoes a hydrolysis-condensation reaction to obtain a hydrophilic polytetrafluoroethylene microporous membrane.
[0008] In this invention, in step S1, the alkenylamide-based hydrophilic agent may contain one or more carbon-carbon double bonds.
[0009] Wherein, when the alkenylamide-containing hydrophilic agent contains a carbon-carbon double bond, the alkenylamide-containing hydrophilic agent is preferably any one or more of acrylamide, methacrylamide, and N-ethylacrylamide, such as acrylamide.
[0010] When the alkenylamide-containing hydrophilic agent contains two carbon-carbon double bonds, the alkenylamide-containing hydrophilic agent is preferably N,N-methylenebisacrylamide.
[0011] In some preferred embodiments, the alkenylamide-containing hydrophilic agent includes alkenylamide-containing hydrophilic agents containing one carbon-carbon double bond and alkenylamide-containing hydrophilic agents containing two carbon-carbon double bonds.
[0012] In some preferred embodiments, the alkenylamide-containing hydrophilic agent includes acrylamide and N,N-methylenebisacrylamide.
[0013] The mass ratio of the acrylamide to the N,N-methylenebisacrylamide is preferably 1:(0.5-2), for example 1:1.
[0014] In this invention, in step S1, the alkenylsilane-containing crosslinking agent may be any one or more of vinyltrimethoxysilane, vinyltriethoxysilane, vinyltriisopropoxysilane and methylvinyldimethoxysilane, preferably vinyltriethoxysilane.
[0015] In some preferred embodiments, the alkenylamide-containing hydrophilic agent is acrylamide and N,N-methylenebisacrylamide, and the alkenylsilane-containing crosslinking agent is vinyltriethoxysilane.
[0016] In this invention, in step S1, the free radical initiator can be any initiator commonly used for free radical polymerization of olefins, preferably any one or more of azobisisobutyronitrile, dimethyl azobisisobutyrate, and azobisisoheptanenitrile, such as azobisisobutyronitrile.
[0017] In this invention, in step S1, the organic solvent is preferably one or more of acetone, ethyl acetate, and triethyl phosphate, for example, triethyl phosphate. The polymerization reaction of this invention is carried out in an organic solvent and belongs to solution polymerization.
[0018] In this invention, in step S1, the mass ratio of the amide hydrophilic agent, the silane crosslinking agent, the free radical initiator, and the organic solvent can be 1:(0.05-20):(0.001-0.1):(10-200), preferably 1:(2-20):(0.01-0.1):(50-100), for example 1.5:11.2:0.08:100.
[0019] In some specific embodiments, the alkenylamide-containing hydrophilic agent is acrylamide and N,N-methylenebisacrylamide, the alkenylsilane-containing crosslinking agent is vinyltriethoxysilane, the free radical initiator is azobisisobutyronitrile, and the organic solvent is triethyl phosphate; wherein, preferably, the mass ratio of acrylamide, N,N-methylenebisacrylamide, vinyltriethoxysilane, azobisisobutyronitrile and triethyl phosphate is 1:0.5:11.2:0.08:100.
[0020] In some specific embodiments, the alkenylamide-containing hydrophilic agent is acrylamide and N,N-methylenebisacrylamide, the alkenylsilane-containing crosslinking agent is vinyltriethoxysilane, the free radical initiator is azobisisobutyronitrile, and the organic solvent is triethyl phosphate; wherein, preferably, the mass ratio of acrylamide, N,N-methylenebisacrylamide, vinyltriethoxysilane, azobisisobutyronitrile, and triethyl phosphate is 0.75:0.75:11.2:0.08:100.
[0021] In some specific embodiments, the alkenylamide-containing hydrophilic agent is acrylamide and N,N-methylenebisacrylamide, the alkenylsilane-containing crosslinking agent is vinyltriethoxysilane, the free radical initiator is azobisisobutyronitrile, and the organic solvent is triethyl phosphate; wherein, preferably, the mass ratio of acrylamide, N,N-methylenebisacrylamide, vinyltriethoxysilane, azobisisobutyronitrile and triethyl phosphate is 0.5:1:11.2:0.08:100.
[0022] In some specific embodiments, the alkenylamide-containing hydrophilic agent is acrylamide, the alkenylsilane-containing crosslinking agent is vinyltriethoxysilane, the free radical initiator is azobisisobutyronitrile, and the organic solvent is triethyl phosphate; wherein, preferably, the mass ratio of acrylamide, vinyltriethoxysilane, azobisisobutyronitrile, and triethyl phosphate is 1.5:11.2:0.08:100.
[0023] In some specific embodiments, the alkenylamide-containing hydrophilic agent is N,N-methylenebisacrylamide, the alkenylsilane-containing crosslinking agent is vinyltriethoxysilane, the free radical initiator is azobisisobutyronitrile, and the organic solvent is triethyl phosphate; wherein, preferably, the mass ratio of N,N-methylenebisacrylamide, vinyltriethoxysilane, azobisisobutyronitrile, and triethyl phosphate is 1.5:11.2:0.08:100.
[0024] In this invention, step S1, the mixing operation preferably includes: first dissolving the alkenylamide-containing hydrophilic agent, the alkenylsilane-containing crosslinking agent, and the free radical initiator in the organic solvent, then adding the polytetrafluoroethylene microporous membrane, and stirring. Preferably, the stirring is performed under nitrogen protection; preferably, the stirring is performed at room temperature; and preferably, the stirring time is 10–60 min, more preferably 25–35 min, for example, 30 min.
[0025] In this invention, in step S1, the temperature of the polymerization reaction can be 60-100°C, preferably 75-85°C, for example 80°C.
[0026] In this invention, in step S1, the polymerization reaction time can be 4 to 12 hours, preferably 5 to 6 hours, for example 5 hours.
[0027] In some specific embodiments, the polymerization reaction is carried out at a temperature of 80°C and for a duration of 5 hours.
[0028] In this invention, in step S1, the polytetrafluoroethylene microporous membrane can be a polytetrafluoroethylene flat sheet membrane, a polytetrafluoroethylene hollow fiber membrane, or a polytetrafluoroethylene capillary membrane.
[0029] Preferably, the surface pore size of the polytetrafluoroethylene capillary membrane is 0.1 to 10 μm; here, 0.1 to 10 μm means that the surface pore size of the same polytetrafluoroethylene capillary membrane is a minimum of 0.1 μm and a maximum of 10 μm.
[0030] Preferably, the outer diameter of the polytetrafluoroethylene capillary membrane is 2.0 to 2.4 mm, for example, 2.2 mm; and the inner diameter of the polytetrafluoroethylene capillary membrane is preferably 1.0 to 1.2 mm, for example, 1.1 mm.
[0031] In this invention, step S1 may further include pretreatment of the polytetrafluoroethylene microporous membrane before the polymerization reaction; the pretreatment operation preferably includes washing, drying, and immersing the polytetrafluoroethylene microporous membrane in an immersion solution until it becomes transparent and colorless.
[0032] The soaking solution is preferably one or more of methanol, ethanol, ethylene glycol, glycerol, isopropanol, acetone and ethyl acetate, for example, ethanol.
[0033] The soaking time is preferably 1 to 60 minutes, for example, 60 minutes.
[0034] The washing operation can be performed in a manner conventional in the art; preferably, the washing operation is performed using deionized water.
[0035] The drying operation can be carried out in a manner conventional in the art; the drying temperature is preferably 60-80°C, for example 70°C; and the drying time is preferably 2-8 hours, for example 4 hours.
[0036] In this invention, in step S2, the hydrolysis-condensation reaction can cause the siloxane group in the alkenylsilane-containing crosslinking agent to hydrolyze and condense to form a Si-O-Si structure; the hydrolysis-condensation reaction can be carried out under acidic conditions, and the substance providing the acidic conditions is preferably any one or more of hydrochloric acid, acetic acid and citric acid monohydrate aqueous solution.
[0037] In this invention, in step S2, the temperature of the hydrolysis-condensation reaction can be 40-80°C, preferably 65-75°C, for example 70°C.
[0038] In this invention, in step S2, the hydrolysis-condensation reaction time can be 1 to 12 hours, preferably 4 to 5 hours, for example 4 hours.
[0039] In some preferred embodiments, the hydrolysis-condensation reaction is carried out in an aqueous solution of citric acid monohydrate.
[0040] The mass fraction of the citric acid monohydrate aqueous solution is preferably 0.1-10%, more preferably 1%-3%, for example 2%; % is the mass percentage of citric acid monohydrate in the total mass of the citric acid monohydrate aqueous solution.
[0041] The volume ratio of the citric acid monohydrate aqueous solution to the precursor is preferably 1:(0.1-10), more preferably 1:(0.5-2), for example 1:1.
[0042] In some specific embodiments, the mass fraction of the citric acid monohydrate aqueous solution is 2%; the volume ratio of the citric acid monohydrate aqueous solution to the precursor is 1:1; the temperature of the hydrolysis-condensation reaction is 70°C; and the time of the hydrolysis-condensation reaction is 4 hours.
[0043] In this invention, step S2 may include washing and drying operations after the hydrolysis-condensation reaction.
[0044] The washing operation can be performed in a manner conventional in the art; preferably, the washing operation is performed using deionized water.
[0045] The drying operation can be carried out in a manner conventional in the art; the drying temperature is preferably 60-80°C, for example 70°C; and the drying time is preferably 2-8 hours, for example 4 hours.
[0046] This invention provides a hydrophilic polytetrafluoroethylene microporous membrane, which is prepared by the method described above for preparing hydrophilic polytetrafluoroethylene microporous membranes.
[0047] The present invention provides a hydrophilic polytetrafluoroethylene microporous membrane, comprising a polytetrafluoroethylene microporous membrane and a hydrophilic layer physically entangled on the polytetrafluoroethylene microporous membrane; the hydrophilic layer has a three-dimensional network structure; the hydrophilic layer comprises a polymer containing amide groups and Si-O-Si bonds.
[0048] In this invention, the initial water contact angle of the hydrophilic polytetrafluoroethylene microporous membrane is preferably 42–88°.
[0049] In this invention, the initial pure water flux of the hydrophilic polytetrafluoroethylene microporous membrane is preferably 1580–2242 L / m. 2 ·h.
[0050] The present invention also provides the application of the hydrophilic polytetrafluoroethylene microporous membrane in water filtration equipment.
[0051] Based on common knowledge in the field, the above-mentioned preferred conditions can be combined arbitrarily to obtain various preferred embodiments of the present invention.
[0052] The reagents and raw materials used in this invention are all commercially available.
[0053] The positive and progressive effects of this invention are as follows:
[0054] The method for preparing hydrophilic polytetrafluoroethylene (PTFE) microporous membranes provided by this invention modifies PTFE microporous membranes through surface crosslinking, constructing a three-dimensional network to densely introduce hydrophilic groups. Simultaneously, the molecular chains already physically entangled on the PTFE microporous membrane continue to anchor the hydrophilic groups in three dimensions, thereby significantly improving its hydrophilic properties. Furthermore, the Si-O-Si bond structure generated by hydrolysis and condensation under acidic conditions allows the hydrophilic three-dimensional network to stably entangle on the fiber nodes of the PTFE microporous membrane. The amide groups and Si-O-Si bonds in this three-dimensional network are highly stable and not easily detached. Therefore, the hydrophilic PTFE microporous membrane prepared by this invention exhibits excellent stability. Moreover, the preparation method provided by this invention is simple, safe, convenient, and energy-efficient, and does not alter the morphology and structure of the original PTFE microporous membrane.
[0055] Specifically:
[0056] (1) The method for preparing hydrophilic polytetrafluoroethylene microporous membranes provided by this invention can greatly improve the hydrophilicity of PTFE microporous membranes. The initial water contact angle of the prepared hydrophilic polytetrafluoroethylene microporous membranes is 88° or below, with the best reaching 42°. At the same time, it has a high initial pure water flux, with the best reaching 2242 L / m. 2 •h, and no large-scale pore blockage occurred;
[0057] (2) The hydrophilic polytetrafluoroethylene microporous membrane prepared by this invention has excellent stability. After 14 days of continuous operation, its water contact angle remains at or below 95°, and the optimal pure water flux can reach 2137 L / m. 2 ·h;
[0058] (3) The method for preparing hydrophilic polytetrafluoroethylene microporous membrane provided by the present invention has the advantages of simple operation, safety and convenience and low energy consumption, and will not change the morphology and structure of the original PTFE microporous membrane. Attached Figure Description
[0059] Figure 1 The infrared spectra of the hydrophilic polytetrafluoroethylene microporous membranes of Examples 1-5 and Comparative Example 1 of this invention are shown.
[0060] Figure 2 This is a SEM image of the hydrophilic polytetrafluoroethylene microporous membrane of Example 1 of the present invention.
[0061] Figure 3 This is a SEM image of the hydrophilic polytetrafluoroethylene microporous membrane of Example 2 of the present invention.
[0062] Figure 4 This is a SEM image of the hydrophilic polytetrafluoroethylene microporous membrane of Example 3 of the present invention.
[0063] Figure 5 This is a SEM image of the hydrophilic polytetrafluoroethylene microporous membrane of Example 4 of the present invention.
[0064] Figure 6 This is a SEM image of the hydrophilic polytetrafluoroethylene microporous membrane of Example 5 of the present invention.
[0065] Figure 7 This is a SEM image of the polytetrafluoroethylene microporous membrane of Comparative Example 1 of the present invention.
[0066] Figure 8 This is a bar chart showing the water contact angle measurements of the hydrophilic polytetrafluoroethylene microporous membranes of Examples 1-5 and Comparative Example 1 of the present invention. Detailed Implementation
[0067] The present invention is further illustrated below by way of embodiments, but the invention is not limited to the scope of the embodiments described herein. Experimental methods in the following embodiments that do not specify specific conditions were performed according to conventional methods and conditions, or as selected according to the product instructions.
[0068] The reaction routes in the preparation process of the hydrophilic polytetrafluoroethylene microporous membranes in Examples 2-5 are shown in Formula 1:
[0069]
[0070] Example 1:
[0071] The preparation method of hydrophilic polytetrafluoroethylene microporous membrane is as follows:
[0072] S1. Preparation of precursors:
[0073] (1) Pretreatment: The PTFE capillary membrane with an outer diameter of 2.2 mm, an inner diameter of 1.1 mm, and a surface pore size of 0.1-10 μm was thoroughly washed with deionized water, dried at 70°C for 4 h, and then soaked in ethanol for 60 min to completely wet it, so that the PTFE capillary membrane appears transparent and colorless.
[0074] (2) Add 1.50g acrylamide, 11.20g vinyltriethoxysilane and 0.08g azobisisobutyronitrile to the reaction vessel and dissolve them in 100g triethyl phosphate.
[0075] (3) The PTFE capillary membrane treated in step (1) is placed in a reaction vessel. The solution in the reaction vessel completely wets the PTFE capillary membrane. The mixture is stirred at room temperature for 30 min under nitrogen protection and then polymerized at 80°C for 5 h to obtain the precursor.
[0076] S2, hydrolysis-condensation reaction:
[0077] (4) The precursor obtained in step (3) is transferred to a 2% citric acid monohydrate aqueous solution for hydrolysis and condensation reaction. The volume ratio of the 2% citric acid monohydrate aqueous solution to the precursor is 1:1. The reaction is then carried out at 70°C for 4 hours.
[0078] (5) The PTFE capillary membrane obtained in step (4) is thoroughly washed with deionized water and dried at 70°C for 4 hours to obtain a hydrophilic polytetrafluoroethylene microporous membrane.
[0079] Example 2:
[0080] The preparation method of hydrophilic polytetrafluoroethylene microporous membrane is as follows:
[0081] S1. Preparation of precursors:
[0082] (1) Pretreatment: The PTFE capillary membrane with an outer diameter of 2.2 mm, an inner diameter of 1.1 mm, and a surface pore size of 0.1-10 μm was thoroughly washed with deionized water, dried at 70°C for 4 h, and then soaked in ethanol for 60 min to completely wet it, so that the PTFE capillary membrane appears transparent and colorless.
[0083] (2) Add 1.00g acrylamide, 0.50g N,N-methylenebisacrylamide, 11.20g vinyltriethoxysilane and 0.08g azobisisobutyronitrile to the reaction vessel and dissolve them in 100g triethyl phosphate.
[0084] (3) The PTFE capillary membrane treated in step (1) is placed in a reaction vessel. The solution in the reaction vessel completely wets the PTFE capillary membrane. The mixture is stirred at room temperature for 30 min under nitrogen protection and then polymerized at 80°C for 5 h to obtain the precursor.
[0085] S2, hydrolysis-condensation reaction:
[0086] (4) The precursor obtained in step (3) is transferred to a 2% citric acid monohydrate aqueous solution for hydrolysis and condensation reaction. The volume ratio of the 2% citric acid monohydrate aqueous solution to the precursor is 1:1. The reaction is then carried out at 70°C for 4 hours.
[0087] (5) The PTFE capillary membrane obtained in step (4) is thoroughly washed with deionized water and dried at 70°C for 4 hours to obtain a hydrophilic polytetrafluoroethylene microporous membrane.
[0088] Example 3:
[0089] The preparation method of hydrophilic polytetrafluoroethylene microporous membrane is as follows:
[0090] S1. Preparation of precursors:
[0091] (1) Pretreatment: The PTFE capillary membrane with an outer diameter of 2.2 mm, an inner diameter of 1.1 mm, and a surface pore size of 0.1-10 μm was thoroughly washed with deionized water, dried at 70°C for 4 h, and then soaked in ethanol for 60 min to completely wet it, so that the PTFE capillary membrane appears transparent and colorless.
[0092] (2) Add 0.75g acrylamide, 0.75g N,N-methylenebisacrylamide, 11.20g vinyltriethoxysilane and 0.08g azobisisobutyronitrile to the reaction vessel and dissolve them in 100g triethyl phosphate.
[0093] (3) The PTFE capillary membrane treated in step (1) is placed in a reaction vessel. The solution in the reaction vessel completely wets the PTFE capillary membrane. The mixture is stirred at room temperature for 30 min under nitrogen protection and then polymerized at 80°C for 5 h to obtain the precursor.
[0094] S2, hydrolysis-condensation reaction:
[0095] (4) The precursor obtained in step (3) is transferred to a 2% citric acid monohydrate aqueous solution for hydrolysis and condensation reaction. The volume ratio of the 2% citric acid monohydrate aqueous solution to the precursor is 1:1. The reaction is then carried out at 70°C for 4 hours.
[0096] (5) The PTFE capillary membrane obtained in step (4) is thoroughly washed with deionized water and dried at 70°C for 4 hours to obtain a hydrophilic polytetrafluoroethylene microporous membrane.
[0097] Example 4:
[0098] The preparation method of hydrophilic polytetrafluoroethylene microporous membrane is as follows:
[0099] S1. Preparation of precursors:
[0100] (1) Pretreatment: The PTFE capillary membrane with an outer diameter of 2.2 mm, an inner diameter of 1.1 mm, and a surface pore size of 0.1-10 μm was thoroughly washed with deionized water, dried at 70°C for 4 h, and then soaked in ethanol for 60 min to completely wet it, so that the PTFE capillary membrane appears transparent and colorless.
[0101] (2) Add 0.50g acrylamide, 1.00g N,N-methylenebisacrylamide, 11.20g vinyltriethoxysilane and 0.08g azobisisobutyronitrile to the reaction vessel and dissolve them in 100g triethyl phosphate.
[0102] (3) The PTFE capillary membrane treated in step (1) is placed in a reaction vessel. The solution in the reaction vessel completely wets the PTFE capillary membrane. The mixture is stirred at room temperature for 30 min under nitrogen protection and then polymerized at 80°C for 5 h to obtain the precursor.
[0103] S2, hydrolysis-condensation reaction:
[0104] (4) The precursor obtained in step (3) is transferred to a 2% citric acid monohydrate aqueous solution for hydrolysis and condensation reaction. The volume ratio of the 2% citric acid monohydrate aqueous solution to the precursor is 1:1. The reaction is then carried out at 70°C for 4 hours.
[0105] (5) The PTFE capillary membrane obtained in step (4) is thoroughly washed with deionized water and dried at 70°C for 4 hours to obtain a hydrophilic polytetrafluoroethylene microporous membrane.
[0106] Example 5:
[0107] The preparation method of hydrophilic polytetrafluoroethylene microporous membrane is as follows:
[0108] S1. Preparation of precursors:
[0109] (1) Pretreatment: The PTFE capillary membrane with an outer diameter of 2.2 mm, an inner diameter of 1.1 mm, and a surface pore size of 0.1-10 μm was thoroughly washed with deionized water, dried at 70°C for 4 h, and then soaked in ethanol for 60 min to completely wet it, so that the PTFE capillary membrane appears transparent and colorless.
[0110] (2) Add 1.50g N,N-methylenebisacrylamide, 11.20g vinyltriethoxysilane and 0.08g azobisisobutyronitrile to the reaction vessel and dissolve them in 100g triethyl phosphate.
[0111] (3) The PTFE capillary membrane treated in step (1) is placed in a reaction vessel. The solution in the reaction vessel completely wets the PTFE capillary membrane. The mixture is stirred at room temperature for 30 min under nitrogen protection and then polymerized at 80°C for 5 h to obtain the precursor.
[0112] S2, hydrolysis-condensation reaction:
[0113] (4) The precursor obtained in step (3) is transferred to a 2% citric acid monohydrate aqueous solution for hydrolysis and condensation reaction. The volume ratio of the 2% citric acid monohydrate aqueous solution to the precursor is 1:1. The reaction is then carried out at 70°C for 4 hours.
[0114] (5) The PTFE capillary membrane obtained in step (4) is thoroughly washed with deionized water and dried at 70°C for 4 hours to obtain a hydrophilic polytetrafluoroethylene microporous membrane.
[0115] Comparative Example 1:
[0116] (1) Pretreatment: The PTFE capillary membrane with an outer diameter of 2.2 mm, an inner diameter of 1.1 mm, and a surface pore size of 0.1-10 μm was thoroughly washed with deionized water, dried at 70°C for 4 h, and then soaked in ethanol for 60 min to completely wet it, so that the PTFE capillary membrane appears transparent and colorless.
[0117] (2) Without hydrophilic modification, the PTFE capillary membrane treated in step (1) is thoroughly washed with deionized water and dried at 70°C for 4 hours to obtain the treated polytetrafluoroethylene microporous membrane.
[0118] Example 1
[0119] Infrared testing
[0120] ①Testing methods
[0121] The PTFE microporous membrane was characterized using an attenuated total reflectance Fourier transform infrared spectroscopy (Nicolet 5700, USA). A resolution of 2 cm⁻¹ was used. -1 The infrared scanning step size is 4000–600 cm. -1 .
[0122] ②Test Results
[0123] The infrared test results of the PTFE microporous membranes of Examples 1-5 and Comparative Example 1 are as follows: Figure 1 As shown, by Figure 1 It can be seen that all PTFE microporous membranes are at 1146 cm⁻¹ -1 and 1201cm -1 Two sharp peaks are observed at this point, corresponding to the stretching vibration of –CF2. For the hydrophilic polytetrafluoroethylene microporous membranes of Examples 1-5, at 1089 cm⁻¹... -1 A new characteristic peak appears at 1655 cm⁻¹, which is attributed to the Si-O-Si bonds formed after the hydrolysis and condensation of vinyltriethoxysilane; -1 The absorption peak at 1420 cm⁻¹ corresponds to the stretching vibration of the C=O bond in the amide group. -1 The absorption peak appearing at the point corresponds to the stretching vibration of the CN bond in the amide group, indicating that the amide group has been successfully introduced into the PTFE microporous membrane.
[0124] Example 2
[0125] Scanning electron microscopy test
[0126] ①Testing methods
[0127] The morphology of PTFE microporous membranes was analyzed using a scanning electron microscope (S-4800, Hitachi, Japan). Long strips of PTFE microporous membrane samples were cut and then subjected to vacuum gold sputtering.
[0128] ②Test Results
[0129] The SEM test results of the PTFE microporous membranes in Examples 1-5 and Comparative Example 1 are as follows: Figures 2-7 As shown, by Figures 2-7As can be seen, each sample exhibits a regularly arranged porous structure. This microporous membrane is composed of numerous PTFE fibers and nodes. Furthermore, the structure of the PTFE microporous membrane did not change significantly before and after hydrophilic modification, and its dimensions remained stable. This indicates that the hydrophilic modification method does not alter the original porous structure of the PTFE membrane. In addition, the fiber surface of the PTFE microporous membrane in Comparative Example 1 was relatively smooth. However, after hydrophilic modification, due to the hydrophilic three-dimensional network generated by free radical polymerization and silane hydrolysis condensation adhering and entangled on the fiber surface of the PTFE microporous membrane, granular agglomerates appeared on the fibers of the PTFE microporous membrane.
[0130] Example 3
[0131] Water contact angle test
[0132] ①Testing methods
[0133] The water contact angle of the PTFE microporous membrane surface was determined using a static water contact angle meter (JY82B, China). A piece of PTFE microporous membrane was placed on a glass slide and then mounted on the meter. Deionized water (3 μL) was dropped onto the surface of the PTFE microporous membrane. The average value of five measurements was taken.
[0134] ②Test Results
[0135] Table 1
[0136]
[0137] Note: # in the table represents untested.
[0138] The bar charts showing the initial water contact angle measurements of the PTFE microporous membranes in Examples 1-5 and Comparative Example 1 are shown below. Figure 8 As shown, the specific values of the initial water contact angle are shown in Table 1. Figure 8 As shown in Table 1, the initial water contact angle of the unmodified PTFE microporous membrane in Comparative Example 1 is as high as 120°, demonstrating strong hydrophobicity. Compared with the unmodified PTFE microporous membrane, Examples 1-5 all exhibit better hydrophilicity. Among them, the initial water contact angle of Example 1 decreased to 88°, indicating a significant improvement in hydrophilicity; Example 3 showed the smallest initial water contact angle of 42°, indicating excellent hydrophilicity.
[0139] This is because both acrylamide and N,N-methylenebisacrylamide contain amide groups. During free radical polymerization, these amide groups are introduced into the long chains of the macromolecules produced, thus physically entangled on the fiber nodes of the PTFE microporous membrane. As polar groups, the amide groups successfully improve the wettability of the PTFE microporous membrane, enhancing its hydrophilicity. Simultaneously, vinyltriethoxysilane contains ethoxy groups. During free radical polymerization, the ethoxy groups are also introduced into the three-dimensional hydrophilic network. Subsequently, under acidic conditions, the ethoxy groups undergo hydrolysis to generate silanols, which then undergo a condensation reaction. The interaction between the silanols forms a Si-O-Si structure. This structure makes the physical entanglement between the hydrophilic three-dimensional network and the PTFE microporous membrane denser and more stable, resulting in PTFE microporous membranes exhibiting both excellent hydrophilicity and high stability.
[0140] Example 4
[0141] Pure water flux test
[0142] ①Testing methods
[0143] The pure water flux of the PTFE microporous membrane was tested using a filtration system (moist-02hfm). Prior to testing, the PTFE microporous membrane specimen loaded in the filtration tank was pressurized with deionized water at 0.2 MPa for at least 1 hour to ensure stable membrane flux. The pure water flux (J) was measured using deionized water under a transmembrane pressure of 0.1 MPa. w The initial pure water flux of each PTFE microporous membrane was measured separately, and the formula is shown below:
[0144]
[0145] Among them, J w It is the permeate pure water flux (L / m 2 ·h), where A is the effective permeation area of the membrane (m²). 2 V is the permeation volume (L) within the time interval Δt(h).
[0146] ②Test Results
[0147] The specific values of the initial pure water flux of the PTFE microporous membranes in Examples 1-5 and Comparative Example 1 are shown in Table 1. As can be seen from Table 1, the initial pure water flux of the unmodified PTFE microporous membrane is 0, indicating its strong hydrophobicity. Examples 1-5 all exhibit high initial pure water flux, with Example 3 reaching an initial pure water flux of 2242 L / m³. 2•h. Because the hydrophilic polytetrafluoroethylene microporous membrane contains a Si-O-Si bond structure, which has high bond energy and a very stable structure, it is not easy to react or degrade. Therefore, under high-purity water flux conditions, the good hydrophilic effect of the hydrophilic polytetrafluoroethylene microporous membrane can still be maintained stably, and there is no large-area blockage of the membrane pores.
[0148] Example 5
[0149] Stability test
[0150] ①Testing methods
[0151] The water contact angle and pure water flux of the hydrophilic PTFE microporous membranes of Examples 1-5 were measured after 14 days of continuous operation. The testing methods for water contact angle and pure water flux were the same as those for Examples 3 and 4.
[0152] ②Test Results
[0153] Table 1 shows the water contact angle and pure water flux of the hydrophilic PTFE microporous membranes from Examples 1-5 after 14 days of continuous operation. It can be seen that the water contact angle of the hydrophilic PTFE microporous membranes from Examples 1-5 remained at or below 95° after 14 days of operation, and the pure water flux reached 1096 L / m³. 2 •h. In Example 3, the water contact angle remained at 42° after 14 days of operation, and the pure water flux was 2137 L / m³. 2 The excellent stability is demonstrated by the ·h value. The superior stability of the hydrophilic modified polytetrafluoroethylene (PTFE) microporous membrane is due to the physical entanglement of a hydrophilic three-dimensional network structure on the PTFE microporous membrane. The stable Si-O-Si bond structure in the hydrophilic three-dimensional network makes it difficult for the network to fall off during actual use, thus giving the modified PTFE microporous membrane excellent stability.
[0154] The hydrophilic polytetrafluoroethylene microporous membranes prepared by this invention have an initial water contact angle of less than 88°, with an optimal angle of 42°, and an optimal initial pure water flux of 2242 L / m. 2 After 14 days of continuous operation, the water contact angle remained at or below 95°, and the optimal pure water flux reached 2137 L / m. 2 Therefore, the hydrophilic polytetrafluoroethylene microporous membrane prepared by this invention has excellent hydrophilicity and stability, and has extremely high application value in water filtration equipment.
Claims
1. A method for preparing a hydrophilic polytetrafluoroethylene microporous membrane, characterized in that, It includes the following steps: S1. Polytetrafluoroethylene microporous membrane is mixed with an alkenylamide-containing hydrophilic agent, an alkenylsilane-containing crosslinking agent, a free radical initiator and an organic solvent to carry out a polymerization reaction to obtain a precursor. The alkenylamide-containing hydrophilic agent contains N,N-methylenebisacrylamide; S2. The precursor undergoes a hydrolysis-condensation reaction to obtain a hydrophilic polytetrafluoroethylene microporous membrane.
2. The method for preparing the hydrophilic polytetrafluoroethylene microporous membrane as described in claim 1, characterized in that, The alkenylamide-containing hydrophilic agent is N,N-methylenebisacrylamide; Alternatively, the alkenylamide-containing hydrophilic agent includes acrylamide and N,N-methylenebisacrylamide.
3. The method for preparing the hydrophilic polytetrafluoroethylene microporous membrane as described in claim 2, characterized in that, When the alkenylamide-containing hydrophilic agent includes acrylamide and N,N-methylenebisacrylamide, the mass ratio of the acrylamide to the N,N-methylenebisacrylamide is 1:(0.5~2).
4. The method for preparing the hydrophilic polytetrafluoroethylene microporous membrane as described in claim 3, characterized in that, When the alkenylamide-containing hydrophilic agent includes acrylamide and N,N-methylenebisacrylamide, the mass ratio of the acrylamide and the N,N-methylenebisacrylamide is 1:
1.
5. The method for preparing the hydrophilic polytetrafluoroethylene microporous membrane as described in claim 1, characterized in that, In step S1, the alkenyl silane-containing crosslinking agent is any one or more of vinyltrimethoxysilane, vinyltriethoxysilane, vinyltriisopropoxysilane, and methylvinyldimethoxysilane; And / or, in step S1, the free radical initiator is any one or more of azobisisobutyronitrile, dimethyl azobisisobutyrate, and azobisisoheptanenitrile; And / or, in step S1, the organic solvent is any one or more of acetone, ethyl acetate, and triethyl phosphate.
6. The method for preparing the hydrophilic polytetrafluoroethylene microporous membrane as described in claim 5, characterized in that, In step S1, the alkenylsilane-containing crosslinking agent is vinyltriethoxysilane; And / or, in step S1, the free radical initiator is azobisisobutyronitrile; And / or, in step S1, the organic solvent is triethyl phosphate.
7. The method for preparing the hydrophilic polytetrafluoroethylene microporous membrane as described in claim 5, characterized in that, In step S1, the alkenyl amide-containing hydrophilic agent is acrylamide and N,N-methylenebisacrylamide, and the alkenyl silane-containing crosslinking agent is vinyltriethoxysilane.
8. The method for preparing the hydrophilic polytetrafluoroethylene microporous membrane as described in claim 1, characterized in that, In step S1, the mass ratio of the amide hydrophilic agent, the silane crosslinking agent, the free radical initiator and the organic solvent is 1:(0.05~20):(0.001~0.1):(10~200).
9. The method for preparing the hydrophilic polytetrafluoroethylene microporous membrane as described in claim 8, characterized in that, In step S1, the mass ratio of the amide hydrophilic agent, the silane crosslinking agent, the free radical initiator and the organic solvent is 1:(2~20):(0.01~0.1):(50~100).
10. The method for preparing the hydrophilic polytetrafluoroethylene microporous membrane as described in claim 9, characterized in that, In step S1, the mass ratio of the amide hydrophilic agent, the silane crosslinking agent, the free radical initiator, and the organic solvent is 1.5:11.2:0.08:
100.
11. The method for preparing the hydrophilic polytetrafluoroethylene microporous membrane as described in claim 8, characterized in that, In step S1, the alkenylamide-containing hydrophilic agent is acrylamide and N,N-methylenebisacrylamide, the alkenylsilane-containing crosslinking agent is vinyltriethoxysilane, the free radical initiator is azobisisobutyronitrile, and the organic solvent is triethyl phosphate; wherein, the mass ratio of acrylamide, N,N-methylenebisacrylamide, vinyltriethoxysilane, azobisisobutyronitrile, and triethyl phosphate is 1:0.5:11.2:0.08:100; And / or, in step S1, the alkenylamide-containing hydrophilic agent is acrylamide and N,N-methylenebisacrylamide, the alkenylsilane-containing crosslinking agent is vinyltriethoxysilane, the free radical initiator is azobisisobutyronitrile, and the organic solvent is triethyl phosphate; wherein, the mass ratio of acrylamide, N,N-methylenebisacrylamide, vinyltriethoxysilane, azobisisobutyronitrile, and triethyl phosphate is 0.75:0.75:11.2:0.08:100; And / or, in step S1, the alkenyl amide-containing hydrophilic agent is acrylamide and N,N-methylenebisacrylamide, the alkenyl silane-containing crosslinking agent is vinyltriethoxysilane, the free radical initiator is azobisisobutyronitrile, and the organic solvent is triethyl phosphate; wherein, the mass ratio of acrylamide, N,N-methylenebisacrylamide, vinyltriethoxysilane, azobisisobutyronitrile, and triethyl phosphate is 0.5:1:11.2:0.08:100; And / or, in step S1, the alkenylamide-containing hydrophilic agent is N,N-methylenebisacrylamide, the alkenylsilane-containing crosslinking agent is vinyltriethoxysilane, the free radical initiator is azobisisobutyronitrile, and the organic solvent is triethyl phosphate; wherein, the mass ratio of N,N-methylenebisacrylamide, vinyltriethoxysilane, azobisisobutyronitrile, and triethyl phosphate is 1.5:11.2:0.08:
100.
12. The method for preparing the hydrophilic polytetrafluoroethylene microporous membrane as described in claim 1, characterized in that, In step S1, the mixing operation includes: first dissolving the alkenylamide-containing hydrophilic agent, the alkenylsilane-containing crosslinking agent, and the free radical initiator in the organic solvent, then adding the polytetrafluoroethylene microporous membrane, and stirring. And / or, in step S1, the temperature of the polymerization reaction is 60~100℃; And / or, in step S1, the polymerization reaction takes 4 to 12 hours.
13. The method for preparing the hydrophilic polytetrafluoroethylene microporous membrane as described in claim 12, characterized in that, In step S1, the stirring is carried out under nitrogen protection; And / or, in step S1, the stirring is carried out at room temperature; And / or, in step S1, the stirring time is 10~60 min; And / or, in step S1, the polymerization reaction temperature is 75~85℃; And / or, in step S1, the polymerization reaction takes 5 to 6 hours.
14. The method for preparing the hydrophilic polytetrafluoroethylene microporous membrane as described in claim 13, characterized in that, In step S1, the stirring time is 25~35 min; And / or, in step S1, the polymerization reaction is carried out at a temperature of 80°C; And / or, in step S1, the polymerization reaction takes 5 hours.
15. The method for preparing the hydrophilic polytetrafluoroethylene microporous membrane as described in claim 14, characterized in that, In step S1, the stirring time is 30 minutes.
16. The method for preparing the hydrophilic polytetrafluoroethylene microporous membrane as described in claim 12, characterized in that, In step S1, the polymerization reaction temperature is 80°C; the polymerization reaction time is 5 h.
17. The method for preparing the hydrophilic polytetrafluoroethylene microporous membrane as described in claim 1, characterized in that, In step S1, the polytetrafluoroethylene microporous membrane is a polytetrafluoroethylene flat sheet membrane, a polytetrafluoroethylene hollow fiber membrane, or a polytetrafluoroethylene capillary membrane. And / or, in step S1, the polymerization reaction is further preceded by pretreatment of the polytetrafluoroethylene microporous membrane.
18. The method for preparing the hydrophilic polytetrafluoroethylene microporous membrane as described in claim 17, characterized in that, In step S1, the surface pore size of the polytetrafluoroethylene capillary membrane is 0.1~10 μm; And / or, in step S1, the outer diameter of the polytetrafluoroethylene capillary membrane is 2.0~2.4 mm; And / or, in step S1, the inner diameter of the polytetrafluoroethylene capillary membrane is 1.0~1.2 mm; And / or, in step S1, the pretreatment operation includes washing, drying, and immersing the polytetrafluoroethylene microporous membrane in an immersion solution until it is transparent and colorless. The soaking solution is any one or more of methanol, ethanol, ethylene glycol, glycerol, isopropanol, acetone and ethyl acetate; The soaking time is 1 to 60 minutes. The washing operation is performed using deionized water; The drying temperature is 60~80℃; the drying time is 2~8 h.
19. The method for preparing the hydrophilic polytetrafluoroethylene microporous membrane as described in claim 18, characterized in that, In step S1, the outer diameter of the polytetrafluoroethylene capillary membrane is 2.2 mm; And / or, in step S1, the inner diameter of the polytetrafluoroethylene capillary membrane is 1.1 mm; And / or, in step S1, the soaking solution is ethanol; And / or, in step S1, the soaking time is 60 minutes; And / or, in step S1, the drying temperature is 70°C; And / or, in step S1, the drying time is 4 hours.
20. The method for preparing the hydrophilic polytetrafluoroethylene microporous membrane as described in claim 1, characterized in that, In step S2, the hydrolysis-condensation reaction is carried out under acidic conditions; And / or, in step S2, the temperature of the hydrolysis-condensation reaction is 40~80℃; And / or, in step S2, the hydrolysis-condensation reaction takes 1 to 12 hours; And / or, in step S2, the hydrolysis-condensation reaction further includes washing and drying operations.
21. The method for preparing the hydrophilic polytetrafluoroethylene microporous membrane as described in claim 20, characterized in that, In step S2, the substance providing the acidic conditions is any one or more of hydrochloric acid, acetic acid, and citric acid monohydrate aqueous solution; And / or, in step S2, the temperature of the hydrolysis-condensation reaction is 65~75℃; And / or, in step S2, the hydrolysis-condensation reaction takes 4-5 hours; And / or, in step S2, the washing operation is performed using deionized water; And / or, in step S2, the drying temperature is 60~80℃; And / or, in step S2, the drying time is 2 to 8 hours.
22. The method for preparing the hydrophilic polytetrafluoroethylene microporous membrane as described in claim 21, characterized in that, In step S2, the temperature of the hydrolysis-condensation reaction is 70°C; And / or, in step S2, the hydrolysis-condensation reaction takes 4 hours; And / or, in step S2, the drying temperature is 70°C; And / or, in step S2, the drying time is 4 hours.
23. The method for preparing the hydrophilic polytetrafluoroethylene microporous membrane as described in claim 21, characterized in that, In step S2, the hydrolysis-condensation reaction is carried out in an aqueous solution of citric acid monohydrate; Wherein, the mass fraction of the citric acid monohydrate aqueous solution is 0.1~10%; % is the mass percentage of citric acid monohydrate in the total mass of the citric acid monohydrate aqueous solution; The volume ratio of the citric acid monohydrate aqueous solution to the precursor is 1:(0.1~10).
24. The method for preparing the hydrophilic polytetrafluoroethylene microporous membrane as described in claim 23, characterized in that, In step S2, the mass fraction of the citric acid monohydrate aqueous solution is 1%~3%; % is the mass percentage of citric acid monohydrate in the total mass of the citric acid monohydrate aqueous solution; And / or, in step S2, the volume ratio of the citric acid monohydrate aqueous solution to the precursor is 1:(0.5~2).
25. The method for preparing the hydrophilic polytetrafluoroethylene microporous membrane as described in claim 24, characterized in that, In step S2, the mass fraction of the citric acid monohydrate aqueous solution is 2%; % is the mass percentage of citric acid monohydrate in the total mass of the citric acid monohydrate aqueous solution. And / or, in step S2, the volume ratio of the citric acid monohydrate aqueous solution to the precursor is 1:
1.
26. The method for preparing the hydrophilic polytetrafluoroethylene microporous membrane as described in claim 23, characterized in that, In step S2, the mass fraction of the citric acid monohydrate aqueous solution is 2%; the volume ratio of the citric acid monohydrate aqueous solution to the precursor is 1:1; the temperature of the hydrolysis-condensation reaction is 70°C; and the time of the hydrolysis-condensation reaction is 4 h.
27. A hydrophilic polytetrafluoroethylene microporous membrane, characterized in that, It is prepared using the method for preparing hydrophilic polytetrafluoroethylene microporous membranes as described in any one of claims 1-26.
28. The hydrophilic polytetrafluoroethylene microporous membrane as described in claim 27, characterized in that, It includes a polytetrafluoroethylene microporous membrane and a hydrophilic layer physically entangled on the polytetrafluoroethylene microporous membrane; the hydrophilic layer has a three-dimensional network structure; the hydrophilic layer includes a polymer containing amide groups and Si-O-Si bonds.
29. The hydrophilic polytetrafluoroethylene microporous membrane as described in claim 28, characterized in that, The initial water contact angle of the hydrophilic polytetrafluoroethylene microporous membrane is 42~88°; And / or, the initial pure water flux of the hydrophilic polytetrafluoroethylene microporous membrane is 1580~2242 L / m 2 ·h.
30. The application of a hydrophilic polytetrafluoroethylene microporous membrane as described in any one of claims 27-29 in a water filtration device.
Citation Information
Patent Citations
Heterogeneous interface hollow fiber membrane as well as preparation method and application thereof
CN117482756A