A mixing method for PVC raw materials and its application in preparing related products
By adopting the automatic dispersion and mixing process in the production of PVC pipes, the problems of difficulty in uniform mixing of formula materials and easy clogging of equipment are solved, improving production efficiency and environmental safety, and reducing costs.
Patent Information
- Application Number
- CN202410151596.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-02
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-02-02
AI Technical Summary
In the existing technology, it is difficult to mix the formula materials evenly in the production of PVC pipes, the materials are easy to stick, and the equipment is easy to block, resulting in low production efficiency, high costs, difficult equipment maintenance, and the dust environment affects the health of operators.
Using a new automatic dispersion and mixing process of PVC raw materials, the main material and the auxiliary materials containing viscous components are premixed in a specific ratio to form a premix, which is then mixed with the supplementary main material to achieve overall uniform mixing of the material and avoid adhesion and adhesion. clogged.
It significantly improves the uniformity and production efficiency of formula materials, reduces equipment failures and maintenance costs, improves the working environment, and reduces material loss and production costs.
Smart Images

Figure BDA0004695875550000081 
Figure BDA0004695875550000101 
Figure BDA0004695875550000111
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of material manufacturing, and in particular to a mixing method of PVC raw materials and application thereof in preparing related products. Background Art
[0002] The key process of mixing and processing PVC plastic pipe products is the weighing and mixing of the formula. Technical personnel in this industry usually use micro-formula automatic metering scales or screw-type quantitative feeding weighing methods to mix ingredients. However, due to poor sealing of weighing instruments, various powder or granular formula materials are prone to scattering and leaking, or materials clump and get stuck, which causes great interference to the weighing accuracy of each formula material and cannot meet the high-precision weighing requirements, resulting in large deviations in the formula materials, and ultimately unstable product quality. In addition, powder or granular formula materials are prone to generate dust during the process of mixing, feeding and unloading, which can easily lead to equipment failures and require regular calibration and maintenance. The operation and transportation process is cumbersome, increasing production costs.
[0003] In the actual industrial production of PVC pipes, it is usually necessary to mix a large amount of raw materials. The usage ratio of the main material and the auxiliary material varies greatly. For some auxiliary materials with less usage, it is impossible to mix them evenly or according to the precise usage, and it is difficult to mix them evenly with the main material, resulting in low overall uniformity of the raw materials and large fluctuations in production performance. In the prior art, the process mode of quantitatively weighing the main materials and auxiliary materials one by one with separate screws is usually adopted. There are many problems such as unstable feeding, stuck agglomerated materials, and unsmooth bridging feeding. The process is cumbersome, the labor intensity is high, the production efficiency is low, and the dust in the working area is large, which affects the health of the operator. Although the uniformity of raw material mixing can be improved to a certain extent by regularly calibrating the formula auxiliary material weighing equipment and extending the mixing time, the problem of pipeline blockage and material jamming caused by material adhesion and agglomeration can only be alleviated by clearing and unblocking the conveying pipeline and setting up a pipe cleaning procedure, which cannot reduce the difficulty of equipment maintenance and maintenance costs. Summary of the invention
[0004] In order to solve the problems in the prior art of large-scale industrial production of PVC pipes that the formulated materials are difficult to mix evenly, the materials are easy to stick together, and the equipment is easy to be blocked, the present invention provides a mixing method for PVC raw materials and its application in the preparation of related products.
[0005] The first object of the present invention is to provide a method for mixing PVC raw materials.
[0006] The second object of the present invention is to provide the application of the compounding method in the preparation of PVC pipes and related products.
[0007] The third object of the present invention is to provide a method for preparing a PVC pipe.
[0008] The fourth object of the present invention is to provide a PVC pipe obtained by the preparation method.
[0009] In order to achieve the above object, the present invention is implemented by the following scheme:
[0010] The invention provides a novel automatic dispersing and mixing process for PVC formula. The main material and the auxiliary material containing viscous components are mixed in a specific ratio to obtain a premix, and then part of the premix is taken and fully mixed with the main material that makes up the amount of the formula, so that all the materials can be stirred, mixed and dispersed uniformly as a whole without adhesion and without clogging the equipment.
[0011] A method for mixing raw materials for preparing PVC pipes, wherein the PVC raw materials are composed of a main material and an auxiliary material, wherein the main material includes polyvinyl chloride and a filler, and the auxiliary material includes wax; according to the formula dosage, the mass of the auxiliary material is M x , the mass of the main material is M y , the mass ratio of auxiliary materials to main materials in conventional PVC raw materials is 1:10;
[0012] The mixing method comprises the following steps:
[0013] S1. The mass is N×M x The auxiliary materials and quality are M y The main ingredients are mixed evenly to obtain a premix, and the mass of the premix is M x+y =N×M x +M y , where 20≤N≤50; the N×M x The auxiliary materials are the amount of the formula magnified N times, where the mass of each auxiliary material is N times the amount of its own formula;
[0014] S2. Then (M x+y / N) parts of premix and (M y -M x+y / N) parts of main ingredients are mixed evenly.
[0015] Preferably, the M x :M y =(1~1.5):10.
[0016] More preferably, the M x :M y =1.1:10.
[0017] Preferably, 25≤N≤50.
[0018] More preferably, 35≤N≤40.
[0019] More preferably, N=35.
[0020] Preferably, the polyvinyl chloride is a powder.
[0021] Preferably, the filler comprises calcium carbonate.
[0022] More preferably, the calcium carbonate is a powder.
[0023] Preferably, the wax is in the form of granules.
[0024] Preferably, the wax comprises mineral wax and / or synthetic wax.
[0025] More preferably, the mineral wax comprises paraffin wax.
[0026] More preferably, the synthetic wax comprises polyethylene wax.
[0027] Preferably, the auxiliary materials further include stabilizers, processing aids and anti-impact agents.
[0028] More preferably, the stabilizer comprises a calcium zinc stabilizer.
[0029] More preferably, the processing aid comprises an ACR processing aid.
[0030] More preferably, the impact resistant agent comprises chlorinated polyethylene.
[0031] More preferably, the auxiliary materials further include lubricant and titanium dioxide.
[0032] Further preferably, the lubricant comprises glyceryl monostearate.
[0033] Further preferably, the formula of the PVC raw material is as follows by weight:
[0034] The main ingredients include: 90 to 110 parts of polyvinyl chloride powder and 90 to 110 parts of calcium carbonate powder;
[0035] The auxiliary materials include: 4 to 6 parts of calcium zinc stabilizer, 0.5 to 1 part of ACR processing aid, 1 to 2 parts of polyethylene wax, 8 to 12 parts of chlorinated polyethylene, 0.5 to 1 part of glyceryl monostearate, 1 to 1.5 parts of paraffin wax, and 2 to 4 parts of titanium dioxide.
[0036] More preferably, the formula of the PVC raw material is as follows, in parts by weight:
[0037] The main ingredients include: 100 parts of polyvinyl chloride powder and 100 parts of calcium carbonate powder;
[0038] The auxiliary materials include: 5 parts of calcium zinc stabilizer, 0.7 parts of ACR processing aid, 1.4 parts of polyethylene wax, 10 parts of chlorinated polyethylene, 0.7 parts of glyceryl monostearate, 1.1 parts of paraffin wax, and 3 parts of titanium dioxide.
[0039] Specifically, the formula of the PVC raw material is as follows:
[0040] The main ingredients are: 100kg polyvinyl chloride powder (brand: SG-5), 100kg calcium carbonate powder (brand: JD-200);
[0041] Auxiliary materials are: 5kg calcium zinc stabilizer (brand: 108A), 0.7kg ACR processing aid (brand: LPA-40), 1.4kg polyethylene wax (brand: YT-95), 10kg chlorinated polyethylene (brand: CPE-135A), 0.7kg glyceryl monostearate (brand: GMS-90), 1.1kg paraffin (brand: YT-60), 3kg titanium dioxide (brand: NR-950).
[0042] Preferably, in step S1, the mixing method is cold mixing.
[0043] More preferably, in step S1, the temperature of the cold mix is 25°C to 35°C.
[0044] Preferably, in step S1, the mixing speed is 20 r / min to 30 r / min.
[0045] More preferably, in step S1, the mixing speed is 27 r / min.
[0046] Preferably, in step S1, the mixing time is 20 min to 40 min.
[0047] More preferably, in step S1, the mixing time is 30 minutes.
[0048] Preferably, in step S2, the mixing method is hot mixing and / or cold mixing.
[0049] More preferably, in step S2, the mixing method is hot mixing first and then cold mixing.
[0050] More preferably, in step S2, the temperature of the hot mixing is 120°C to 130°C.
[0051] Further preferably, in step S2, the temperature of the hot mixing is 120°C.
[0052] More preferably, in step S2, the rotation speed of the hot mixing is 600 r / min to 700 r / min.
[0053] Further preferably, in step S2, the rotation speed of the hot mix is 650 r / min.
[0054] More preferably, in step S2, the heat mixing time is 5 min to 10 min.
[0055] Further preferably, in step S2, the hot mixing time is 8 minutes.
[0056] More preferably, in step S2, the temperature of the cold mix is 60°C to 75°C.
[0057] Further preferably, in step S2, the temperature of the cold mix is 75°C.
[0058] More preferably, in step S2, the rotation speed of the cold mix is 80 r / min to 100 r / min.
[0059] Further preferably, in step S2, the rotation speed of the cold mixer is 90 r / min.
[0060] More preferably, in step S2, the cold mixing time is 1 min to 5 min.
[0061] Further preferably, in step S2, the mixing time is 2 minutes.
[0062] Preferably, in step S2, the premix is first transported for 50 to 200 meters, and then (M x+y / N) parts of premix and (M y -M x+y / N) parts of main ingredients are mixed evenly.
[0063] More preferably, in step S2, the premix is first transported for 100 meters and then (M x+y / N) parts of premix and (M y -M x+y / N) parts of main ingredients are mixed evenly.
[0064] Specifically, the premix is first transported from the sending tank to the storage bin through a pipeline with a distance of 100 meters, and then weighed by the system to obtain (M x+y / N) parts of premix and (M y -M x+y / N) parts of main ingredients, then (M x+y / N) parts of premix and (M y -M x+y / N) parts of main ingredients are mixed evenly.
[0065] The application of any of the above methods in the preparation of PVC pipes and related products should also be within the scope of protection of the present invention.
[0066] After the PVC raw materials are processed according to the mixing method provided by the present invention, they are transported to a silo over a long distance for mixing and use, and subsequent preparation processes such as extrusion are performed to finally obtain a PVC pipe.
[0067] A method for preparing a PVC pipe comprises the following steps: firstly treating a PVC raw material by a mixing method to obtain a mixed raw material, and then extruding the mixed raw material to obtain a PVC pipe;
[0068] The PVC raw material is composed of a main material and an auxiliary material, wherein the main material includes polyvinyl chloride and filler, and the auxiliary material includes wax; according to the formula dosage, the mass of the auxiliary material is M x , the mass of the main material is M y ;
[0069] The mixing method comprises the following steps:
[0070] S1. The mass is N×M x The auxiliary materials and quality are M y The main ingredients are mixed evenly to obtain a premix, and the mass of the premix is M x+y =N×M x +M y , where 20≤N≤50; the N×M x The auxiliary materials are the amount of the formula magnified N times, where the mass of each auxiliary material is N times the amount of its own formula;
[0071] S2. Then (M x+y / N) parts of premix and (M y -M x+y / N) parts of main ingredients are mixed evenly.
[0072] Preferably, the M x :M y =(1~1.5):10.
[0073] More preferably, the M x :M y =1.1:10.
[0074] Preferably, 25≤N≤50.
[0075] More preferably, 35≤N≤40.
[0076] More preferably, N=35.
[0077] Preferably, the polyvinyl chloride is a powder.
[0078] Preferably, the filler comprises calcium carbonate.
[0079] More preferably, the calcium carbonate is a powder.
[0080] Preferably, the wax is in the form of granules.
[0081] Preferably, the wax comprises mineral wax and / or synthetic wax.
[0082] More preferably, the mineral wax comprises paraffin wax.
[0083] More preferably, the synthetic wax comprises polyethylene wax.
[0084] Preferably, the auxiliary materials further include stabilizers, processing aids and anti-impact agents.
[0085] More preferably, the stabilizer comprises a calcium zinc stabilizer.
[0086] More preferably, the processing aid comprises an ACR processing aid.
[0087] More preferably, the impact resistant agent comprises chlorinated polyethylene.
[0088] More preferably, the auxiliary materials further include lubricant and titanium dioxide.
[0089] Further preferably, the lubricant comprises glyceryl monostearate.
[0090] Further preferably, the formula of the PVC raw material is as follows by weight:
[0091] The main ingredients include: 90 to 110 parts of polyvinyl chloride powder and 90 to 110 parts of calcium carbonate powder;
[0092] The auxiliary materials include: 4 to 6 parts of calcium zinc stabilizer, 0.5 to 1 part of ACR processing aid, 1 to 2 parts of polyethylene wax, 8 to 12 parts of chlorinated polyethylene, 0.5 to 1 part of glyceryl monostearate, 1 to 1.5 parts of paraffin wax, and 2 to 4 parts of titanium dioxide.
[0093] More preferably, the formula of the PVC raw material is as follows, in parts by weight:
[0094] The main ingredients include: 100 parts of polyvinyl chloride powder and 100 parts of calcium carbonate powder;
[0095] The auxiliary materials include: 5 parts of calcium zinc stabilizer, 0.7 parts of ACR processing aid, 1.4 parts of polyethylene wax, 10 parts of chlorinated polyethylene, 0.7 parts of glyceryl monostearate, 1.1 parts of paraffin wax, and 3 parts of titanium dioxide.
[0096] Specifically, the formula of the PVC raw material is as follows:
[0097] The main ingredients are: 100kg polyvinyl chloride powder (brand: SG-5), 100kg calcium carbonate powder (brand: JD-200);
[0098] Auxiliary materials are: 5kg calcium zinc stabilizer (brand: 108A), 0.7kg ACR processing aid (brand: LPA-40), 1.4kg polyethylene wax (brand: YT-95), 10kg chlorinated polyethylene (brand: CPE-135A), 0.7kg glyceryl monostearate (brand: GMS-90), 1.1kg paraffin (brand: YT-60), 3kg titanium dioxide (brand: NR-950).
[0099] Preferably, in step S1, the mixing method is cold mixing.
[0100] More preferably, in step S1, the temperature of the cold mix is 25°C to 35°C.
[0101] Preferably, in step S1, the mixing speed is 20 r / min to 30 r / min.
[0102] More preferably, in step S1, the mixing speed is 27 r / min.
[0103] Preferably, in step S1, the mixing time is 20 min to 40 min.
[0104] More preferably, in step S1, the mixing time is 30 minutes.
[0105] Preferably, in step S2, the mixing method is hot mixing and / or cold mixing.
[0106] More preferably, in step S2, the mixing method is hot mixing first and then cold mixing.
[0107] More preferably, in step S2, the temperature of the hot mixing is 120°C to 130°C.
[0108] Further preferably, in step S2, the temperature of the hot mixing is 120°C.
[0109] More preferably, in step S2, the rotation speed of the hot mixing is 600 r / min to 700 r / min.
[0110] Further preferably, in step S2, the rotation speed of the hot mix is 650 r / min.
[0111] More preferably, in step S2, the heat mixing time is 5 min to 10 min.
[0112] Further preferably, in step S2, the hot mixing time is 8 minutes.
[0113] More preferably, in step S2, the temperature of the cold mix is 60°C to 75°C.
[0114] Further preferably, in step S2, the temperature of the cold mix is 75°C.
[0115] More preferably, in step S2, the rotation speed of the cold mix is 80 r / min to 100 r / min.
[0116] Further preferably, in step S2, the rotation speed of the cold mixer is 90 r / min.
[0117] More preferably, in step S2, the cold mixing time is 1 min to 5 min.
[0118] Further preferably, in step S2, the mixing time is 2 minutes.
[0119] Preferably, in step S2, the premix is first transported for 50 to 200 meters, and then (M x+y / N) parts of premix and (M y -M x+y / N) parts of main ingredients are mixed evenly.
[0120] More preferably, in step S2, the premix is first transported for 100 meters and then (M x+y / N) parts of premix and (M y -M x+y / N) parts of main ingredients are mixed evenly.
[0121] Specifically, the premix is first transported from the sending tank to the storage bin through a pipeline with a distance of 100 meters, and then weighed by the system to obtain (M x+y / N) parts of premix and (M y -M x+y / N) parts of main ingredients, then (M x+y / N) parts of premix and (M y -M x+y / N) parts of main ingredients are mixed evenly.
[0122] Preferably, during the preparation process, the mixed raw material is first transported over a distance of 10 to 50 meters and then extruded.
[0123] More preferably, during the preparation process, the mixed raw material is first transported over a distance of 20 meters and then extruded.
[0124] Specifically, the mixed raw material is first transported from the mixer to the extruder through a pipeline or a pipe chain with a distance of 20 meters, and then extruded.
[0125] Preferably, the extrusion conditions include: a temperature of 165° C. to 185° C. and a rotation speed of 20 r / min to 40 r / min.
[0126] More preferably, the temperature decreases gradually from the feed inlet to the outlet of the extruder.
[0127] Further preferably, the temperatures from the feed port to the sample outlet of the extruder are 185°C, 180°C, 175°C, 170°C and 165°C, respectively.
[0128] More preferably, the rotation speed is 30 r / min.
[0129] More preferably, the extrusion conditions further include: the outlet temperature of the extruder is 180°C to 185°C.
[0130] Further preferably, the outlet temperature of the extruder is 185°C.
[0131] More preferably, the extrusion conditions further include: a feeding speed of 20 r / min to 30 r / min.
[0132] Further preferably, the feeding speed is 27 r / min.
[0133] More preferably, the extrusion conditions further include: a torque of 60% to 70%.
[0134] Further preferably, the torque is 65%.
[0135] More preferably, the preparation method further comprises the following steps: the mixed raw materials are extruded, cooled, and shaped to obtain the product.
[0136] The PVC pipe obtained by any of the preparation methods should also be within the protection scope of the present invention.
[0137] Compared with the prior art, the present invention has the following beneficial effects:
[0138] The invention provides a PVC formula dispersion mixing process, simplifies the original formula weighing mode, is more flexible and simple to operate, realizes the whole package of formula delivery or enlarged integer multiple delivery, is suitable for ingredients and feeding with different equal amounts, and the overall mixing amount of each pot of formula can be adjusted to 35 times the original amount. Especially for the demand for special material dosage, it can be directly delivered according to the enlarged ratio without dilution treatment, completes batch preparation and mixing at one time, and greatly improves the formula weighing efficiency.
[0139] In addition, the present invention also significantly reduces the adhesion of the formulated materials, avoids agglomeration and adhesion, improves the smoothness of long-distance transportation, and the mixed materials do not stratify, block pipes, or raise dust during transportation, thereby reducing material loss, improving the on-site working environment and operator health, reducing the cost of formula equipment failure maintenance, saving energy and reducing consumption, greatly improving the efficiency of industrial production of PVC pipes, and significantly reducing production costs. DETAILED DESCRIPTION
[0140] The present invention is further elaborated in detail below in conjunction with specific examples. The examples are only used to explain the present invention and are not used to limit the scope of the present invention. The test methods used in the following examples are all conventional methods unless otherwise specified; the materials, reagents, etc. used are reagents and materials that can be obtained from commercial channels unless otherwise specified. The following examples are all carried out in a 4-story PVC pipe workshop unless otherwise specified. The production area on the first floor is 120 meters long and 102 meters wide, covering an area of 12,240 square meters. The daily output of PVC pipes in the workshop is 400 tons / day to 450 tons / day.
[0141] Example 1 Mixing Process Comparison
[0142] 1. Formula materials
[0143] This embodiment provides a formula for preparing PVC plastic pipes, and the specific information is shown in Table 1.
[0144] Table 1 Standard process formula dosage
[0145]
[0146] 2. Weighing and mixing methods
[0147] (1) Method 1
[0148] According to the formula shown in Table 1, each auxiliary material was weighed and magnified 20 times (ie, mass (kg)×20), and the total mass of the auxiliary materials was 438 kg.
[0149] Directly put all the auxiliary materials magnified 20 times into a mixer (Sixing Mechanical Mixing Equipment, 3200L) at once, and stir and mix at a speed of 27 r / min for 30 minutes at room temperature (25°C to 35°C) to obtain mixture 1. Repeat 5 times in parallel to obtain mixtures 1-1 to 1-5 in turn.
[0150] (2) Method 2
[0151] According to the formula shown in Table 1, each auxiliary material was weighed to obtain a 20-fold increase in weight, and the total weight of the auxiliary materials was 438 kg; the main material was not magnified, and was directly weighed to obtain 100 kg of resin powder.
[0152] Each auxiliary material magnified 20 times and 100 kg of resin powder were put into a mixer (Sixing Mechanical Mixing Equipment, 3200L), and stirred and mixed at a speed of 27 r / min for 30 minutes at room temperature (25°C to 35°C) to obtain Mix 2. Repeat 5 times in parallel to obtain Mix 2-1 to Mix 2-5 in turn.
[0153] (3) Method 3
[0154] First, each auxiliary material magnified 20 times and 100 kg of calcium carbonate powder were put into a mixer (Sixing Mechanical Mixing Equipment, 3200L), and stirred and mixed at a speed of 27 r / min for 30 minutes at room temperature (25°C to 35°C) to obtain mixture 3. Repeat 5 times in parallel to obtain mixtures 3-1 to 3-5 in turn.
[0155] (4) Method 4
[0156] According to the formula shown in Table 1, each auxiliary material magnified 20 times was weighed, and the total mass of the auxiliary materials was 438 kg; the main material was not magnified, and 100 kg of resin powder and 100 kg of calcium carbonate powder were directly weighed.
[0157] Each auxiliary material magnified 20 times, 100 kg of resin powder and 100 kg of calcium carbonate powder were put into a mixer (Sixing Mechanical Mixing Equipment, 3200L), and stirred and mixed at a speed of 27 r / min for 30 minutes at room temperature (25°C to 35°C) to obtain Mix 4. Repeat 5 times in parallel to obtain Mix 4-1 to Mix 4-5 in turn.
[0158] (5) Method 5
[0159] According to the formula shown in Table 1, each auxiliary material magnified 50 times was weighed, and the total mass of the auxiliary materials was 1095 kg; the main material was not magnified, and 100 kg of resin powder and 100 kg of calcium carbonate powder were directly weighed.
[0160] Each auxiliary material magnified 50 times, 100 kg of resin powder and 100 kg of calcium carbonate powder were put into a mixer (Sixing Mechanical Mixing Equipment, 3200L), and stirred and mixed at a speed of 27 r / min for 30 minutes at room temperature (25°C to 35°C) to obtain Mixture 5. Repeat 5 times in parallel to obtain Mixtures 5-1 to 5-5 in turn.
[0161] 3. Stirring and adhesion
[0162] During low-speed stirring, when method 1 is used for mixing, paraffin wax and polyethylene wax often stick to the mixing blade or cylinder of the mixing equipment, and some materials stick together. When methods 2 to 5 are used for mixing, the frequency of the above-mentioned adhesion and sticking is significantly reduced, and the stirring is smoother.
[0163] 4. Pipeline transportation
[0164] Mixtures 1-1 to 1-5, 2-1 to 2-5, 3-1 to 3-5, 4-1 to 4-5 and 5-1 to 5-5 are respectively transported through sending tanks at a pressure of 250Mka through a 100m conveying pipeline to formula storage silos 1 to 6 on the 4th floor (the straight-line distance from the sending tank is 100m, and the relative height from the ground is 16m) (the interval between each formula storage silo is 15m).
[0165] 5. Blockage
[0166] (1) Detection method
[0167] When the monitoring devices of the conveying equipment and the silo equipment show: abnormal pressure, abnormal pressure relief, and the silo level meter does not detect that the material is transported to the corresponding silo, it is determined that the material causes equipment blockage during the process of being transported to the silo.
[0168] The number of times each mixing material causes equipment blockage and the blockage probability are counted. The calculation formula for the blockage probability is: Blockage probability (%) = number of blockages / total number of conveying times × 100%.
[0169] (2) Results
[0170] Table 2 The situation of equipment blockage caused by various mixing materials
[0171]
[0172]
[0173] As shown in Table 2, the mixture obtained by method 1 is transported through the sending tank, and a large amount of sticky agglomerate materials (mainly paraffin wax, PE wax and other viscous materials) are blocked in the conveying pipeline, and the blocking probability is as high as 80% to 100%; the mixture obtained by methods 2 and 3 significantly improves the phenomenon of blocking the transportation pipeline, with only occasional blockage, and the blocking probability of the mixture is as low as 0% to 33.3%; there is basically no blocking phenomenon when using methods 4 and 5, and the blocking probability is as low as 0% to 16.6%, indicating that methods 4 and 5 significantly improve the smoothness of conveying the mixture, improve transportation efficiency, and reduce material loss.
[0174] Example 2 Hot Mixing and Cold Mixing Process
[0175] 1. Weighing of formula materials
[0176] According to the formula shown in Table 1, the auxiliary materials were weighed and magnified by 20 times, 25 times, 30 times, 35 times, 40 times, 45 times and 50 times respectively, and the total mass of the auxiliary materials at each magnification was 438 kg, 547.5 kg, 657 kg, 766.5 kg, 876 kg, 985.5 kg and 1095 kg respectively; the main material was not magnified and was directly weighed.
[0177] 2. Hybrid Approach
[0178] Referring to method 4 and method 5 in Example 1, materials at different magnification ratios are mixed, and the specific operation is as follows:
[0179] (1) Magnification 20 times
[0180] First, put the auxiliary materials magnified 20 times, 100kg of resin powder polyvinyl chloride and 100kg of calcium carbonate powder into a color mixer (Sixing Mechanical Mixing Equipment, 3200L), stir and mix at room temperature (25℃~35℃) at a speed of 27r / min for 30 minutes to obtain a premix with a total mass of 638kg.
[0181] In addition, 95kg of resin powder polyvinyl chloride and 95kg of calcium carbonate powder were accurately weighed through the system, and put into the mixer (GRH1000 / LH3000B hot and cold mixing equipment) together with 31.9kg of premix, and hot mixed in the hot mixing tank, and stirred and mixed at a high speed of 650r / min for 8 minutes to make the temperature of the mixed material reach the process requirement of 120°C; then discharged to the cold mixing tank, stirred and mixed at a speed of 90r / min for 2 minutes to make the mixed material cool to 75°C.
[0182] (2) Magnification 25 times
[0183] First, put the auxiliary materials magnified 25 times, 100kg of resin powder polyvinyl chloride and 100kg of calcium carbonate powder into a color mixer (Sixing Mechanical Mixing Equipment, 3200L), stir and mix at room temperature (25℃~35℃) at a speed of 27r / min for 30 minutes to obtain a premix with a total mass of 747.5kg.
[0184] Weigh 96 kg of resin powder polyvinyl chloride and 96 kg of calcium carbonate powder together with 29.9 kg of premix and put them into a mixer (GRH1000 / LH3000B hot and cold mixing equipment), mix them in a hot mixing tank, stir and mix them at 120°C and a speed of 650 r / min for 8 minutes; then cool them to 75°C for cold mixing, and stir and mix them at a speed of 90 r / min for 2 minutes.
[0185] (3) Magnification 30 times
[0186] First, put the auxiliary materials magnified 30 times, 100kg of resin powder polyvinyl chloride and 100kg of calcium carbonate powder into a color mixer (Sixing Mechanical Mixing Equipment, 3200L), stir and mix at room temperature (25℃~35℃) at a speed of 27r / min for 30 minutes to obtain a premix with a total mass of 857kg.
[0187] Weigh 96.65kg of resin powder polyvinyl chloride and 96.65kg of calcium carbonate powder together with 28.6kg of premix and put them into a mixer (GRH1000 / LH3000B hot and cold mixing equipment), hot mix them in a hot mixing tank, stir and mix at a high speed of 650r / min for 8 minutes, so that the temperature of the mixed material reaches the process requirement of 120°C; then discharge them to a cold mixing tank, stir and mix at a speed of 90r / min for 2 minutes, so that the mixed material drops to 75°C.
[0188] (4) Magnification 35 times
[0189] First, put the auxiliary materials magnified 35 times, 100kg of resin powder polyvinyl chloride and 100kg of calcium carbonate powder into a color mixer (Sixing Mechanical Mixing Equipment, 3200L), stir and mix at room temperature (25℃~35℃) at a speed of 27r / min for 30 minutes to obtain a premix with a total mass of 966.5kg.
[0190] Weigh 97.15kg of resin powder polyvinyl chloride and 97.15kg of calcium carbonate powder together with 27.6kg of premix and put them into a mixer (GRH1000 / LH3000B hot and cold mixing equipment), hot mix them in a hot mixing tank, stir and mix at a high speed of 650r / min for 8 minutes, so that the temperature of the mixed material reaches the process requirement of 120°C; then discharge them to a cold mixing tank, stir and mix at a speed of 90r / min for 2 minutes, so that the mixed material drops to 75°C.
[0191] (5) Magnification 40 times
[0192] First, put the auxiliary materials magnified 40 times, 100kg of resin powder polyvinyl chloride and 100kg of calcium carbonate powder into a color mixer (Sixing Mechanical Mixing Equipment, 3200L), stir and mix at room temperature (25℃~35℃) at a speed of 27r / min for 30 minutes to obtain a premix with a total mass of 1076kg.
[0193] Weigh 97.5kg of resin powder polyvinyl chloride and 97.5kg of calcium carbonate powder together with 26.9kg of premix and put them into a mixer (GRH1000 / LH3000B hot and cold mixing equipment), hot mix them in a hot mixing tank, stir and mix at a high speed of 650r / min for 8 minutes, so that the temperature of the mixed material reaches the process requirement of 120°C; then discharge them to a cold mixing tank, stir and mix at a speed of 90r / min for 2 minutes, so that the mixed material drops to 75°C.
[0194] (6) Magnification 45 times
[0195] First, put the auxiliary materials magnified 45 times, 100kg of resin powder polyvinyl chloride and 100kg of calcium carbonate powder into a color mixer (Sixing Mechanical Mixing Equipment, 3200L), stir and mix at room temperature (25℃~35℃) at a speed of 27r / min for 30 minutes to obtain a premix with a total mass of 1185.5kg.
[0196] Weigh 97.8kg of resin powder polyvinyl chloride and 97.8kg of calcium carbonate powder together with 26.3kg of premix and put them into a mixer (GRH1000 / LH3000B hot and cold mixing equipment), hot mix them in a hot mixing tank, stir and mix at a high speed of 650r / min for 8 minutes, so that the temperature of the mixed material reaches the process requirement of 120°C; then discharge them to a cold mixing tank, stir and mix at a speed of 90r / min for 2 minutes, so that the mixed material drops to 75°C.
[0197] (7) Magnification 50 times
[0198] First, put the auxiliary materials magnified 50 times, 100kg of resin powder polyvinyl chloride and 100kg of calcium carbonate powder into a color mixer (Sixing Mechanical Mixing Equipment, 3200L), stir and mix at room temperature (25℃~35℃) at a speed of 27r / min for 30 minutes to obtain a premix with a total mass of 1295kg.
[0199] Weigh 98kg of resin powder polyvinyl chloride and 98kg of calcium carbonate powder together with 25.9kg of premix and put them into a mixer (GRH1000 / LH3000B hot and cold mixing equipment), hot mix them in a hot mixing tank, stir and mix them at a high speed of 650r / min for 8 minutes, so that the temperature of the mixed material reaches the process requirement of 120°C; then discharge them to a cold mixing tank, stir and mix them at a speed of 90r / min for 2 minutes, so that the mixed material drops to 75°C.
[0200] Example 3 Preparation and performance evaluation of PVC pipe
[0201] 1. Mix
[0202] The processing was carried out according to Example 2, and the magnifications were 20 times, 25 times, 30 times, 35 times, 40 times, 45 times and 50 times corresponding to tests 1 to 7, respectively, and each test was repeated 5 times in parallel.
[0203] 2. Extrusion
[0204] The mixed materials of tests 1 to 7 were transported from the mixer to the conical twin-screw extruder (the pipe chain conveying distance was 20 meters). In the barrel segmented heating temperature zone, there were 5 screw shearing and plasticizing zones from the material inlet to the mold, recorded as zones 1 to 5, with temperatures of 185°C in zone 1, 180°C in zone 2, 175°C in zone 3, 170°C in zone 4, and 165°C in zone 5. The sample outlet temperature of the extruder was 180°C to 185°C. The screw speed of the extruder was 30r / min, the feeding speed was 27r / min, the current was 80A, and the torque of the screw rotation power motor was 65%.
[0205] After extrusion, the sizing sleeve is used for cooling water tank shaping to reach the outer diameter of 110.2 mm required by G8806-2008 standard. After cooling, it is cut into lengths of 4010 mm to obtain PVC pipes of tests 1 to 7.
[0206] 3. Performance testing
[0207] The tensile strength (MPa) of the PVC pipes in tests 1 to 7 was measured using the standard method for tensile strength of thermoplastic pipes (GBT 8804.3-2003). The tensile strength value range required by the company's internal control standard (LS-QEO-NK.27.C01.2022 "Product Performance Acceptance Internal Control Standard") is 23MPa to 24MPa.
[0208] The impact performance of thermoplastic pipes (GBT 14152-2001) was used to measure the drop weight impact strength of PVC pipes from test 1 to 7. The drop weight impact strength qualification standard required by the company's internal control standard (LS-QEO-NK.27.C01.2022 "Internal Control Standard for Product Performance Acceptance") is: the number of broken pipes in 10 impact tests is ≤ 1. Further, according to the drop weight impact strength results, the proportion of qualified samples is calculated to obtain the qualified rate.
[0209] The flat test was used to determine the cracking conditions of the PVC pipes in tests 1 to 7. The cracking acceptance standard required by the company's internal control standard (LS-QEO-NK.27.C01.2022 "Product Performance Acceptance Internal Control Standard") is: the PVC pipe sample tested by the ring stiffness tester (WDT-H-100KN) is qualified if the downward compression deformation is 50% of the outer diameter of the corresponding product without cracking or rupture.
[0210] The density (kg / m2) of the PVC pipes in tests 1 to 7 was measured using a Sartorius Scientific Instruments BSA224S-CW electronic analytical balance. 3 ), the density value of the test sample is obtained by converting the data between the weight of air and the weight in the liquid. The density reference value required by the enterprise internal control standard (LS-QEO-NK.27.C01.2022 "Product Performance Acceptance Internal Control Standard") is: 1650kg / m 3~1780kg / m 3 .
[0211] The color of the PVC pipes in tests 1 to 7 was detected by using the X-Rite Gi7600 fully automatic colorimeter, and the L value (black and white phase value), a value (red and green phase value) and b value (yellow phase value) were measured. The difference between the test results of the test samples and the test results of the normal color sample products was used as the reference value of the color difference of the test samples. The qualified standard of the reference value required by the enterprise internal control standard (LS-QEO-NK.27.C01.2022 "Product Performance Acceptance Internal Control Standard") is: L value is in the range of 90 to 92, greater than 92 is white, less than 90 is black; a value is in the range of -0.65 to -0.35; b value is 4.5 to 6.0, and greater than 6.0 is yellowish.
[0212] From the PVC pipes of tests 1 to 7 obtained by repeating the test 5 times in parallel, one sample was randomly selected from each test and each repeat for the above-mentioned test.
[0213] 4. Performance evaluation results
[0214] Table 3 Performance evaluation results of PVC pipes
[0215]
[0216]
[0217] Note: “*” indicates the drop weight impact strength is unqualified.
[0218] As shown in Table 3, the tensile strength of the PVC pipes in test 1 (magnified 20 times) to test 3 (magnified 30 times) is between 20.9 MPa and 22.6 MPa, which is lower than the standard; the qualified rate of the drop weight impact strength is between 40% and 60%, which is lower than the standard; the flat test results are all free of breakage and cracking, which meets the standard; the density is 1771 kg / m 3 ~1780kg / m 3 , which meets the standards; the color test results show that the L value is 90.74~92.15, the a value is -0.65~-0.22, and the b value is 5.46~7.17, which are higher than the standard and the appearance color is slightly yellowish.
[0219] The overall performance of the PVC pipe in test 4 (magnified 35 times) is relatively stable, with a tensile strength of 23.4MPa~24.5MPa, which basically meets the standard; the qualified rate of the drop weight impact strength is as high as 100%, which meets the standard; the flat test results show no breakage or cracking, which meets the standard; the density is 1768kg / m 3 ~1774kg / m 3, which meets the standards; the color detection results show that the L value is 90.81~91.35, the a value is -0.54~-0.34, and the b value is 4.98~5.27. The color is normal and the color value is stable.
[0220] The tensile strength of the PVC pipe in test 5 (magnified 40 times) is 22.3MPa~23.2MPa, which basically meets the standard; the qualified rate of the drop weight impact strength is as high as 80%, which meets the standard; the flat test results show no breakage or cracking, which meets the standard; the density is 1771kg / m 3 ~1780kg / m 3 , in line with the standard; the color test results show that the L value is 91.24~92.22, the a value is -0.71~-0.39, and the b value is 5.02~5.47. The color is normal and the color value is stable. The overall performance of test 5 is similar to that of test 4.
[0221] The tensile strength of the PVC pipes in test 6 (magnified 45 times) and test 7 (magnified 50 times) is in the range of 21.6MPa to 23.1MPa, which is lower than the standard. The qualified rate of the drop weight impact strength is 60%, which is lower than the standard. The flat test results show no breakage or cracking, which meets the standard. The density is 1748kg / m 3 ~1780kg / m 3 , in line with the standards; color test results show that the L value is 92.03 ~ 92.72, the a value is -0.65 ~ -0.42, and the b value is 4.62 ~ 5.36. The color is whiter than normal products, and the color value is stable.
[0222] The test results above show that in the hot mixing and cold mixing processes provided in Example 2 of the present invention, the enlargement ratio of the auxiliary materials used to prepare the premix has a significant correlation with the performance of the final product, mainly affecting the strength performance, impact performance and color, and has little effect on the density of the product. Among them, the premix prepared by enlarging the auxiliary materials by 35 times according to the standard formula, and the finished product produced after mixing with the main materials according to the standard process has the best overall performance, is the most stable, and best meets the internal control standards.
[0223] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the protection scope of the present invention. For ordinary technicians in this field, other different forms of changes or modifications can be made based on the above descriptions and ideas. It is not necessary and impossible to list all the implementation methods here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A mixing method for PVC raw materials, characterized in that: The PVC raw material is composed of a main material and an auxiliary material, wherein the main material includes polyvinyl chloride and filler, and the auxiliary material includes wax; according to the formula dosage, the mass of the auxiliary material is M x , the mass of the main material is M y ; The mixing method comprises the following steps: S1. The mass is N×M x The auxiliary materials and quality are M y The main ingredients are mixed evenly to obtain a premix, and the mass of the premix is M x+y =N×M x +M y , where 25≤N≤50; S2. Then (M x+y / N) parts of premix and (M x +M y -M x+y / N) parts of main ingredients are mixed evenly.
2. The compounding method according to claim 1, characterized in that: The M x :M y =(1~1.5):
10.
3. The compounding method according to claim 1, characterized in that: Waxes include mineral waxes and / or synthetic waxes.
4. The compounding method according to claim 1, characterized in that: The filler includes calcium carbonate.
5. The compounding method according to claim 1, characterized in that: The auxiliary materials also include stabilizers, processing aids and anti-impact agents.
6. The compounding method according to claim 1, characterized in that: In step S2, the mixing method is hot mixing and / or cold mixing.
7. Use of the mixing method according to any one of claims 1 to 6 in the preparation of PVC pipes and related products.
8. A method for preparing a PVC pipe, characterized in that: The following steps are involved: The PVC raw material is first treated by the mixing method described in any one of claims 1 to 7 to obtain a mixed raw material, and then extruded to obtain the mixed raw material.