A kind of anti-clogging coated abrasive tool coating dispersion liquid with endothermic effect and its preparation method and application

By introducing phase change microcapsules and other additives into the coating of coated abrasive tools, the problems of clogging and low grinding efficiency of coated abrasive tools are solved, the life of the abrasive tools is extended and the surface quality is improved.

CN117986933BActive Publication Date: 2024-10-25SENCHUANGAN (SHANGHAI) MATERIAL TECH CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202410068322.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-17
Publication Date
2024-10-25
Estimated Expiration
2044-01-17

AI Technical Summary

Technical Problem

Existing coated abrasive tools are prone to clogging when processing oily or soft surfaces, resulting in low grinding efficiency and short grinding life. Moreover, anti-clogging coatings containing stearates can cause slippery phenomena and dust accumulation during long-term use. clogged.

Method used

The anti-clogging coated abrasive coating dispersion with endothermic effect contains stearate, dispersant, wetting agent, penetrant, adhesive, phase change microcapsules, defoaming agent and preservative. Phase change microcapsules reduce interface grinding heat and stearate melting, and improve dispersion and coating uniformity.

Benefits of technology

Delay the melting state of stearate, reduce debris clogging, increase tool life and surface quality, and improve grinding efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004668997300000151
    Figure BDA0004668997300000151
  • Figure BDA0004668997300000161
    Figure BDA0004668997300000161
Patent Text Reader

Abstract

The present invention provides an anti-clogging coated abrasive coating dispersion with heat absorption effect, a preparation method and application thereof, comprising the following raw materials in weight percentage: 15%-40% stearate, 0.1%-3% dispersant, 0.2%-3% wetting agent, 0.1%-3% penetrant, 5%-20% adhesive, 3%-15% phase change microcapsule, 0.1%-3% defoamer, 0.1%-3% preservative and 40%-65% water. When the anti-clogging coated abrasive coating dispersion with heat absorption effect of the present invention is used for coated abrasives, it helps to reduce the interfacial grinding heat generated by the coated abrasives during the grinding process, delays the time for the stearate molten state to be generated, reduces chip blockage, increases the life of the abrasives, and improves the surface quality of the ground workpiece.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of functional coatings for coated abrasives, and in particular relates to an anti-clogging coated abrasive coating dispersion with endothermic effect, and a preparation method and application thereof. Background Art

[0002] Coated abrasives are a vital and indispensable tool for grinding and polishing in modern industrial production. From rough grinding to fine grinding and sub-micron polishing, different coated abrasives can meet different processing requirements. Coated abrasives can process workpieces of different types, different hardness and different flatness.

[0003] Coated abrasives can clog the grinding surface of coated abrasives to varying degrees when machining oily or soft surfaces. The chip load caused by this clogging prevents the abrasive product from effectively grinding the work surface and reduces the material removal / "cutting" rate that the abrasive can provide.

[0004] A common method widely used in the abrasives industry to reduce chip load is to coat the abrasive particles with a layer of metal soap, such as calcium or zinc stearate. This stearate coating is often called an "anti-clogging coating" and can lubricate the chip contact surface and reduce chip load. Usually due to the hydrophobicity of the stearate itself, the coating can effectively reduce the accumulation and adhesion of grinding dust on the undulating sand surface, thereby increasing the grinding life of the coated abrasive.

[0005] However, during long-term continuous grinding, the anti-clogging coating containing stearate will cause the grinding contact surface to become slippery, aggravating the sliding phenomenon during grinding and reducing grinding efficiency. In addition, it will also cause rapid accumulation and adhesion of grinding dust, thereby clogging the sand surface of the coated abrasive and reducing the grinding life of the coated abrasive.

[0006] Therefore, it is necessary to provide an improved technical solution to address the above-mentioned deficiencies in the prior art. Summary of the invention

[0007] The object of the present invention is to provide an anti-clogging coated abrasive coating dispersion with endothermic effect and a preparation method and application thereof, so as to solve or improve at least one of the problems of low grinding efficiency, easy clogging of the coated abrasive sand surface and reduced grinding life of the coated abrasive in the use process of the coated abrasive in the prior art.

[0008] In order to achieve the above-mentioned purpose, the present invention provides the following technical scheme: an anti-clogging coated abrasive coating dispersion with endothermic effect, comprising the following raw materials in weight percentage: 15%-40% stearate, 0.1%-3% dispersant, 0.2%-3% wetting agent, 0.1%-3% penetrant, 5%-20% adhesive, 3%-15% phase change microcapsule, 0.1%-3% defoamer, 0.1%-3% preservative and 40%-65% water.

[0009] Preferably, the stearate is calcium stearate and / or zinc stearate; the dispersant is at least one of alkyl biphenyl ether sodium sulfonate, lignin sulfonate, alkylphenol polyoxyethylene ether formaldehyde condensate, fatty alcohol polyoxyethylene ether sodium sulfate, polyacrylate ammonium salt and polyacrylate sodium salt; the wetting agent is at least one of anionic surfactant fatty acid or / and fatty acid ester sulfate, polyol polyoxyethylene ether, sodium isopropyl naphthalene sulfonate and alkyl naphthalene sulfonate; the penetrant is ethanolamine, sodium sulfate, fatty alcohol polyoxyethylene ether and alkylphenol polyoxyethylene ether; the adhesive is at least one of acrylic emulsion, nitrile emulsion, styrene-butadiene emulsion, styrene-acrylic emulsion, styrene-butadiene emulsion and amino emulsion; the wall material of the phase change microcapsule is modified polyurethane; the defoamer is at least one of polysiloxane defoamers, fatty alcohol defoamers, mineral oil defoamers, silicone oil defoamers and natural plant extract defoamers; the preservative is at least one of benzoic acid, sodium benzoate, sorbic acid, potassium sorbate and isothiazolinone.

[0010] Preferably, the core material of the phase-change microcapsule is at least one of inorganic acid salts, aliphatic hydrocarbons, fatty acids, fatty acid esters, fatty acid salts and alcohols.

[0011] Preferably, the stearate is zinc stearate, the dispersant is sodium dodecylbenzene sulfonate, the wetting agent is polyol polyoxyethylene ether, the penetrant is alkylphenol polyoxyethylene ether, the adhesive is a neutral styrene-acrylic copolymer emulsion, the defoamer is a fatty alcohol defoamer, and the preservative is an isothiazolinone preservative.

[0012] Preferably, the particle size of the stearate is 180-1250 mesh.

[0013] The present invention also proposes a method for preparing an anti-clogging coated abrasive tool coating dispersion having an endothermic effect, which adopts the following technical scheme: The method for preparing an anti-clogging coated abrasive tool coating dispersion having an endothermic effect comprises the following steps: (1) firstly fully stirring 40%-50% by weight of water and 0.2%-3% by weight of a wetting agent; (2) adding 0.1%-3% by weight of a dispersant and fully stirring; (3) adding 0.1%-3% by weight of a penetrant and fully stirring; (4) then adding 15%-40% by weight of a stearate while continuing to stir and fully stirring; (5) pouring the material obtained by the treatment of step (4) into a grinder for grinding, so that the average particle size D50 of the ground slurry is less than 10 μm; (6) pouring the ground slurry into a container, adding 5%-20% by weight of a binder and 3%-15% by weight of water and stirring thoroughly; (7) then adding 3%-15% by weight of phase change microcapsules while continuing to stir, and stirring thoroughly; (8) then adding 0.1%-3% by weight of a defoamer and 0.1%-3% by weight of a preservative, and stirring thoroughly, to obtain the anti-clogging coated abrasive coating dispersion with endothermic effect.

[0014] The present invention also proposes an anti-clogging coated abrasive coating with endothermic effect, which adopts the following technical scheme: an anti-clogging coated abrasive coating with endothermic effect, the coating is prepared from the anti-clogging coated abrasive coating dispersion with endothermic effect as described above.

[0015] The present invention also proposes an anti-clogging coated abrasive with endothermic effect, which adopts the following technical scheme: an anti-clogging coated abrasive with endothermic effect, wherein the anti-clogging coated abrasive with endothermic effect has the coating as described above.

[0016] Beneficial effects:

[0017] The present invention introduces phase change microcapsules into the anti-clogging coated abrasive coating dispersion, so that when the anti-clogging coated abrasive coating dispersion with endothermic effect is used for coated abrasives, it helps to reduce the interfacial grinding heat generated by the coated abrasives during the grinding process, delay the time for the stearate to be in a molten state, reduce debris blockage, increase the life of the abrasive, and improve the surface quality of the ground workpiece.

[0018] In the anti-clogging coated abrasive coating dispersion with endothermic effect of the present invention, by introducing dispersants, wetting agents and penetration aids, the dispersion characteristics of stearate are effectively improved and the agglomeration phenomenon is reduced; by introducing defoaming agents, the bubbles generated during the stirring, transportation and coating processes are effectively reduced and the coating uniformity is improved; by introducing preservatives, the demulsification and corruption of the emulsion coating system are effectively avoided. DETAILED DESCRIPTION

[0019] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. All other embodiments obtained by ordinary technicians in this field based on the embodiments of the present invention belong to the scope of protection of the present invention.

[0020] The present invention will be described in detail below in conjunction with embodiments. It should be noted that the embodiments and features in the embodiments of the present invention can be combined with each other without conflict.

[0021] The inventors found in their research that the melting point of stearates used for coated abrasives affects the grinding efficiency and the grinding life of coated abrasives. Specifically, the melting point of stearates generally used for coated abrasives is between 100-150°C. During long-term continuous grinding, the accumulated grinding heat will cause the temperature of the contact interface between the abrasive and the workpiece to exceed the melting point of the stearate, causing the stearate to enter a molten state prematurely, thereby causing the grinding contact interface to enter a slippery state, aggravating the sliding phenomenon during the grinding process and reducing the grinding efficiency. In addition, the molten stearate will cause the rapid aggregation and adhesion of grinding dust, thereby blocking the sand surface of the coated abrasive and reducing the grinding life of the coated abrasive.

[0022] The present invention aims at at least one of the problems of low grinding efficiency, easy clogging of the sand surface of the coated abrasive and short grinding life of the coated abrasive, which exist in the current coated abrasives coated with stearate. The present invention provides a dispersion liquid for coating the coated abrasive with an endothermic effect and an anti-clogging coating, which comprises the following raw materials in weight percentage: 15%-40% of stearate (for example, 15%, 20%, 25%, 30%, 35% or 40%), 0.1%-3% of dispersant (for example, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5% or 3%), 0.2%-3% of wetting agent (for example, 0.2%, 0.8%, 1.2%, 1.9%, 2.2%, 2.8% or 3%), Agent 0.1%-3% (e.g., 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5% or 3%), binder 5%-20% (e.g., 5%, 10%, 15% or 20%), phase change microcapsules 3%-15% (e.g., 3%, 6%, 9%, 12% or 15%), defoaming agent 0.1%-3% (e.g., 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5% or 3%), preservative 0.1%-3% (e.g., 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5% or 3%) and water 40%-65% (e.g., 40%, 44%, 49%, 54%, 60% or 65%).

[0023] Among them, phase change materials refer to substances that absorb or release energy to undergo phase changes and provide a large amount of latent heat as the temperature of the external environment changes. At present, the classification of phase change materials can be divided into solid-solid, solid-liquid, solid-gas and gas-liquid according to the phase state. Among them, solid-liquid phase change materials have two processes of melting and crystallization during the phase change process. By absorbing and releasing a certain amount of heat, energy storage and release can be achieved. Phase change materials are mainly divided into organic phase change materials and inorganic phase change materials according to the chemical composition of the material. Organic phase change materials are mainly paraffin and fatty acids; inorganic phase change materials are mainly inorganic hydrated salts and metals. Phase change materials are divided into low-temperature phase change materials (below 80°C), medium-temperature phase change materials (80°C-180°C) and high-temperature phase change materials (180°C-2000°C) according to different phase change temperatures. However, the inventors found in their research that the use of inorganic phase change materials in the coating dispersion for coated abrasives will cause the uniformity of the coating dispersion for coated abrasives to deteriorate and become prone to sedimentation; while the use of organic phase change materials in the coating dispersion for coated abrasives will cause the phase change performance of the phase change material to deteriorate, thereby making it unable to play a good role in phase change endothermicity and making it difficult to inhibit the melting of stearate.

[0024] The present invention introduces phase change microcapsules into the coating dispersion for coated abrasives by utilizing the heat absorption characteristics of phase change materials, thereby helping to reduce the interfacial grinding heat generated by the coated abrasives during the grinding process, delay the time for the stearate to be in a molten state, reduce debris blockage, increase the life of the abrasives, and improve the surface quality of the ground workpiece. The use of phase change microcapsules not only helps to achieve uniform dispersion of the phase change microcapsules in the anti-blocking coated abrasive coating dispersion with heat absorption, but also helps to ensure that the core material (phase change material) inside the phase change microcapsules can better play the role of heat absorption. The wall material protects the inner layer of the phase change material (core material) and also helps to improve the stability and reuse rate of the phase change material. In addition, the dispersant, wetting agent and penetrant in the present invention help to improve the dispersibility of stearate and reduce agglomeration; the introduction of the defoamer helps to reduce the bubbles generated during the stirring, transportation and coating process and improve the coating uniformity; the introduction of the bactericide helps to avoid the demulsification and corruption of the emulsion coating system.

[0025] In a preferred embodiment of the anti-clogging coated abrasive coating dispersion with endothermic effect of the present invention, the stearate is calcium stearate and / or zinc stearate; the dispersant is at least one of alkyl biphenyl ether sodium sulfonate, lignin sulfonate, alkylphenol polyoxyethylene ether formaldehyde condensate, fatty alcohol polyoxyethylene ether sodium sulfate, polyacrylate ammonium salt and polyacrylate sodium salt; the wetting agent is at least one of anionic surfactant fatty acid or / and fatty acid ester sulfate, polyol polyoxyethylene ether, sodium isopropyl naphthalene sulfonate and alkyl naphthalene sulfonate; the penetrant is at least one of ethanolamine, sodium sulfate, fatty alcohol polyoxyethylene ether and alkylphenol polyoxyethylene ether; the adhesive is acrylic emulsion, nitrile emulsion, styrene butadiene emulsion, benzene At least one of acrylic emulsion, styrene-butadiene emulsion and amino emulsion; the adhesive used in the present invention may include aqueous emulsion and solvent-based emulsion, and the aqueous emulsion or solvent-based emulsion used in the present invention needs to be pH neutral or near-neutral emulsion, and the glass transition temperature (Tg) needs to be greater than 5°C; the wall material of the phase change microcapsule is modified polyurethane (preferably, the modified polyurethane is silicone diol or siloxane-modified polyurethane); the defoamer is at least one of polysiloxane defoamers, fatty alcohol defoamers, mineral oil defoamers, silicone oil defoamers and natural plant extract defoamers; the defoamer is at least one of benzoic acid, sodium benzoate, sorbic acid, potassium sorbate and isothiazolinone.

[0026] Among them, different types of stearates are suitable for different abrasive tool sizes and grinding occasions, which can mainly reduce the grinding load and inhibit the adhesion of grinding dust and debris; the addition of dispersants can be adsorbed on the surface of stearates (dispersants can also be adsorbed on the surface of phase change material microcapsules) to form a steric effect, avoid particle agglomeration, and improve the coating appearance and product performance stability; the addition of wetting agents, adsorbed on the surface of stearates, can reduce the surface tension of stearates and increase the solubility of stearates in water; adhesives can adhere stearates and phase change materials to the surface of coated abrasives. During grinding, The anti-clogging effect can be gradually released; bubbles will appear to varying degrees during the dispersion, stirring and grinding of the coating emulsion. The addition of defoaming agent can reduce the number of bubbles, inhibit the generation of new bubbles, and improve the subsequent coating quality; the addition of preservatives can inhibit the coating dispersion from corroding microorganisms and prevent the coating dispersion from demulsifying and deteriorating; phase change microcapsules with modified polyurethane as the wall material are helpful to form a uniform dispersed phase in the anti-clogging coated abrasive coating dispersion of the present invention, which helps to avoid the performance deterioration of the anti-clogging coated abrasive coating dispersion with endothermic effect caused by the sedimentation of the phase change material.

[0027] In a preferred embodiment of the anti-clogging coated abrasive coating dispersion with endothermic effect of the present invention, the core material of the phase change microcapsule is at least one of inorganic acid salts (for example, nitrates, phosphates, carbonates, etc.), aliphatic hydrocarbons (for example, paraffin, etc.), fatty acids, fatty acid esters, fatty acid salts (for example, acetates, etc.) and alcohols.

[0028] In a preferred embodiment of the anti-clogging coated abrasive coating dispersion with endothermic effect of the present invention, the stearate is zinc stearate, the dispersant is sodium dodecylbenzene sulfonate, the wetting agent is polyol polyoxyethylene ether, the penetrant is alkylphenol polyoxyethylene ether, the adhesive is a neutral styrene-acrylic acid copolymer emulsion, the defoamer is a fatty alcohol defoamer, and the preservative is an isothiazolinone preservative.

[0029] In the preferred embodiment of the anti-clogging coated abrasive coating dispersion with endothermic effect of the present invention, the particle size specification of stearate is 180-1250 mesh (for example, 180 mesh, 200 mesh, 300 mesh, 500 mesh, 800 mesh, 1000 mesh or 1250 mesh). Among them, large stearate powder particle size (particle size greater than 180 mesh) is not conducive to the loading and grinding of sand mill, and the particle size of general large particles will be crushed and ground by crusher, ball mill and other processes. Smaller particle size, such as powder less than 1250 mesh, on the one hand, the powder cost will be higher, on the other hand, it is not conducive to dispersed grinding, and the problem of powder agglomeration will occur easily, and the agglomerated powder will have a great impact on the subsequent coating uniformity. The requirement of the present invention is that when the average particle size specification of stearate reaches greater than or equal to 1250 mesh through grinding of the grinding machine, it can be well used in the anti-clogging coating.

[0030] More preferably, the particle size of the stearate is 400 mesh.

[0031] The present invention also provides a method for preparing a dispersion liquid of an anti-clogging coated abrasive tool with an endothermic effect. The method for preparing a dispersion liquid of an anti-clogging coated abrasive tool with an endothermic effect in an embodiment of the present invention comprises the following steps: (1) firstly, 40% to 50% by weight of water and 0.2% to 3% by weight of a wetting agent are fully stirred; (2) 0.1% to 3% by weight of a dispersant is added and fully stirred; (3) 0.1% to 3% by weight of a penetrant is added and fully stirred; (4) then, while continuing to stir, 15% to 40% by weight of a stearate is added and fully stirred; (5) The material obtained by the treatment in step (5) is poured into a grinder for grinding, so that the average particle size D50 of the ground slurry is less than 10 μm; (6) the ground slurry is poured into a container, and 5%-20% by weight of a binder and 3%-15% by weight of water are added and stirred thoroughly; (7) while continuing to stir, 3%-15% by weight of phase change microcapsules are added and stirred thoroughly; (8) 0.1%-3% by weight of a defoamer and 0.1%-3% by weight of a preservative are added and stirred thoroughly to obtain the anti-clogging coated abrasive tool coating dispersion with endothermic effect according to the embodiment of the present invention. In the preparation method of the anti-clogging coated abrasive coating dispersion with endothermic effect of the present invention: adding a wetting agent, a dispersant and a penetrant in the aqueous solution in advance will allow the three additives to be evenly dispersed in the aqueous solution. When the stearate powder is added for grinding, the three additives will evenly contact the surface of the stearate powder, thereby playing the role of wetting, dispersing and penetrating, thereby forming a uniform dispersed emulsion; after the uniform dispersed emulsion is obtained, the adhesive is added to effectively avoid the phenomenon of stearate agglomeration caused by the addition of the adhesive; the final addition of the defoamer and the preservative is to eliminate bubbles and microbial contamination generated in the previous processing process.

[0032] The present invention also proposes an anti-clogging coated abrasive coating with endothermic effect. The anti-clogging coated abrasive coating with endothermic effect of the embodiment of the present invention is prepared from the anti-clogging coated abrasive coating dispersion with endothermic effect as described above.

[0033] The present invention further provides an anti-clogging coated abrasive tool with heat absorption effect. The anti-clogging coated abrasive tool with heat absorption effect according to an embodiment of the present invention has the coating as described above.

[0034] The anti-clogging coated abrasive tool coating dispersion with endothermic effect and its preparation method and application are described in detail below through specific embodiments.

[0035] The materials and reagents used in the following examples are summarized as follows:

[0036] St-1: calcium stearate powder, fineness (400 mesh pass rate) greater than 99%.

[0037] St-2: zinc stearate powder, fineness (400 mesh pass rate) greater than 99%.

[0038] St-3: Calcium stearate and zinc stearate blended powder, fineness (400 mesh pass rate) greater than 99%; wherein the mass addition ratio of calcium stearate to zinc stearate is 1:1.

[0039] Dispersant: DS-1 sodium dodecylbenzene sulfonate.

[0040] Wetting agent: WT-1 polyol polyoxyethylene ether.

[0041] Penetrant: PT-1 alkylphenol polyoxyethylene ether.

[0042] Adhesive: BE-1 neutral styrene-acrylic copolymer emulsion, Tg>5℃.

[0043] Phase change microcapsule powder:

[0044] MCPCM-1: Model ZJ-PCM-M-37, shell material is organic material modified polyurethane, phase change temperature is 30℃, phase change latent heat is 180J / g, purchased from Guangzhou Zhongjia New Material Technology Co., Ltd.;

[0045] MCPCM-2: Model RX-193, shell material is organic material modified polyurethane, phase change temperature is 38.8℃, phase change latent heat is 193J / g, purchased from Hefei Ruixue New Material Technology Co., Ltd.;

[0046] MCPCM-3: It is an inorganic material coated phase change microcapsule dry powder prepared by emulsifying and drying the inorganic reaction precursor ethyl orthosilicate with aminopropyl trimethoxysilane and phenyl trimethoxysilane, and the shell material is the inorganic material SiO2 (MCPCM-3 is a high-grade pure GR silica-coated crystalline hydrated salt phase change material microcapsule purchased from Xi'an Qiyue Biotechnology Co., Ltd.). The phase change temperature of this inorganic material coated phase change microcapsule is 20.1°C, and the phase change latent heat is 133 J / g.

[0047] Phase change material powder:

[0048] PCM-1: Model: PCM-XR-78, containing crystalline water inorganic salt phase change material, phase change temperature 78 ° C, enthalpy value 230 J / g, purchased from Guangzhou Zhongjia New Material Technology Co., Ltd.;

[0049] Defoamer: DF-1 fatty alcohol defoamer (the main component is the polycondensate of fatty alcohol and ethylene oxide / propylene oxide; the fatty alcohol defoamer can quickly penetrate into the liquid and spread rapidly, and can stably defoam under different conditions);

[0050] Preservative: AB-1 isothiazolinone preservative.

[0051] Example 1

[0052] The anti-clogging coated abrasive coating dispersion with endothermic effect of this embodiment includes the following components in weight percentage: 25% stearate (ST-1), 1% dispersant (DS-1), 1.5% wetting agent (WT-1), 0.5% penetrant (PT-1), 10% binder (BE-1), 5% phase change microcapsule (MCPCM-1), 0.5% defoamer (DF-1), 0.5% preservative (AB-1) and 56% water (WT-1).

[0053] The preparation method of the anti-clogging coated abrasive coating dispersion with endothermic effect of the present embodiment comprises the following steps: (1) firstly, 50% by weight of water and 1.5% by weight of wetting agent are fully stirred; (2) 1% by weight of dispersant is added and fully stirred; (3) 0.5% by weight of penetrant is added and fully stirred; (4) then, while continuing to stir, 25% by weight of stearate is added and fully stirred; (5) the material obtained by the treatment of step (4) is poured into a grinder for grinding, so that the average particle size D50 of the slurry after grinding is less than 10 μm; (6) the ground slurry is poured into a container, and 10% by weight of binder and 6% by weight of water are added and fully stirred; (7) then, while continuing to stir, 5% by weight of phase change microcapsules are added and fully stirred; (8) 0.5% by weight of defoamer and 0.5% by weight of preservative are added and fully stirred to obtain the anti-clogging coated abrasive coating dispersion with endothermic effect of the present invention.

[0054] Example 2

[0055] The anti-clogging coated abrasive coating dispersion with endothermic effect of this embodiment includes the following components in weight percentage: 20% stearate (ST-2), 0.5% dispersant (DS-1), 1% wetting agent (WT-1), 0.5% penetrant (PT-1), 10% adhesive (BE-1), 10% phase change microcapsule (MCPCM-2), 0.5% defoaming agent (DF-1), 0.5% preservative (AB-1) and 57% water (WT-1).

[0056] The preparation method of the anti-clogging coated abrasive tool coating dispersion with endothermic effect in this embodiment is the same as that in Example 1, the only difference is that the amount of water added in step (1) is 50%, and the amount of water added in step (6) is 7%.

[0057] Example 3

[0058] The anti-clogging coated abrasive coating dispersion with endothermic effect of this embodiment includes the following components in weight percentage: 30% stearate (ST-3), 0.5% dispersant (DS-1), 1% wetting agent (WT-1), 0.5% penetrant (PT-1), 10% adhesive (BE-1), 8% phase change microcapsule (MCPCM-1), 0.5% defoaming agent (DF-1), 0.5% preservative (AB-1) and 49% water (WT-1).

[0059] The preparation method of the anti-clogging coated abrasive tool coating dispersion with endothermic effect in this embodiment is the same as that in Example 1, the only difference is that the amount of water added in step (1) is 45%, and the amount of water added in step (6) is 4%.

[0060] Example 4

[0061] The anti-clogging coated abrasive coating dispersion with endothermic effect of this embodiment includes the following components in weight percentage: 25% stearate (ST-1), 1% dispersant (DS-1), 1.5% wetting agent (WT-1), 0.5% penetrant (PT-1), 10% binder (BE-1), 5% phase change microcapsule (MCPCM-3), 0.5% defoamer (DF-1), 0.5% preservative (AB-1) and 56% water (WT-1).

[0062] The preparation method of the anti-clogging coated abrasive tool coating dispersion with endothermic effect in this embodiment is the same as that in Example 1, the only difference is that the amount of water added in step (1) is 50%, and the amount of water added in step (6) is 6%.

[0063] Example 5

[0064] The anti-clogging coated abrasive coating dispersion with endothermic effect of this embodiment includes the following components in weight percentage: 20% stearate (ST-2), 0.5% dispersant (DS-1), 1% wetting agent (WT-1), 0.5% penetrant (PT-1), 10% adhesive (BE-1), 10% phase change microcapsule (MCPCM-3), 0.5% defoaming agent (DF-1), 0.5% preservative (AB-1) and 57% water (WT-1).

[0065] The preparation method of the anti-clogging coated abrasive tool coating dispersion with endothermic effect in this embodiment is the same as that in Example 1, the only difference is that the amount of water added in step (1) is 50%, and the amount of water added in step (6) is 7%.

[0066] Example 6

[0067] The difference between the endothermic anti-clogging coated abrasive tool coating dispersion of this embodiment and that of embodiment 2 is that the phase change microcapsule used is MCPCM-1; the rest is consistent with embodiment 2.

[0068] Specifically, the anti-clogging coated abrasive coating dispersion with endothermic effect of this embodiment includes the following components in weight percentage: 20% stearate (ST-2), 0.5% dispersant (DS-1), 1% wetting agent (WT-1), 0.5% penetrant (PT-1), 10% adhesive (BE-1), 10% phase change microcapsule (MCPCM-1), 0.5% defoaming agent (DF-1), 0.5% preservative (AB-1) and 57% water (WT-1).

[0069] Comparative Example 1

[0070] The anti-clogging coated abrasive coating dispersion with endothermic effect in this comparative example includes the following components in weight percentage: 30% stearate (ST-1), 1% dispersant (DS-1), 1.5% wetting agent (WT-1), 0.5% penetrant (PT-1), 10% adhesive (BE-1), 0.5% defoaming agent (DF-1), 0.5% preservative (AB-1) and 56% water (WT-1).

[0071] The preparation method of the anti-clogging coated abrasive tool coating dispersion with endothermic effect in this comparative example refers to Example 1.

[0072] Comparative Example 2

[0073] The anti-clogging coated abrasive coating dispersion with endothermic effect in this comparative example includes the following components in weight percentage: 30% stearate (ST-2), 0.5% dispersant (DS-1), 1% wetting agent (WT-1), 0.5% penetrant (PT-1), 10% adhesive (BE-1), 0.5% defoamer (DF-1), 0.5% preservative (AB-1) and 57% water (WT-1).

[0074] The preparation method of the anti-clogging coated abrasive tool coating dispersion with endothermic effect in this comparative example refers to Example 1.

[0075] Comparative Example 3

[0076] The anti-clogging coated abrasive coating dispersion with endothermic effect in this comparative example includes the following components in weight percentage: 39% stearate (ST-3), 0.5% dispersant (DS-1), 1% wetting agent (WT-1), 0.5% penetrant (PT-1), 10% binder (BE-1) and 49% water (WT-1).

[0077] The preparation method of the anti-clogging coated abrasive tool coating dispersion with endothermic effect in this comparative example refers to Example 1.

[0078] Comparative Example 4

[0079] The anti-clogging coated abrasive coating dispersion with endothermic effect in this comparative example includes the following components in weight percentage: 30% stearate (ST-2), 1% wetting agent (WT-1), 0.5% penetrant (PT-1), 10% adhesive (BE-1), 0.5% defoaming agent (DF-1), 0.5% preservative (AB-1) and 57.5% water (WT-1).

[0080] The preparation method of the anti-clogging coated abrasive tool coating dispersion with endothermic effect in this comparative example refers to Example 1.

[0081] Comparative Example 5

[0082] The anti-clogging coated abrasive coating dispersion with endothermic effect in this comparative example includes the following components in weight percentage: 30% stearate (ST-2), 0.5% dispersant (DS-1), 0.5% penetrant (PT-1), 10% adhesive (BE-1), 0.5% defoamer (DF-1), 0.5% preservative (AB-1) and 58% water (WT-1).

[0083] The preparation method of the anti-clogging coated abrasive tool coating dispersion with endothermic effect in this comparative example refers to Example 1.

[0084] Comparative Example 6

[0085] The anti-clogging coated abrasive coating dispersion with endothermic effect in this comparative example includes the following components in weight percentage: 30% stearate (ST-2), 0.5% dispersant (DS-1), 1% wetting agent (WT-1), 10% adhesive (BE-1), 0.5% defoaming agent (DF-1), 0.5% preservative (AB-1) and 57.5% water (WT-1).

[0086] The preparation method of the anti-clogging coated abrasive tool coating dispersion with endothermic effect in this comparative example refers to Example 1.

[0087] Comparative Example 7

[0088] The anti-clogging coated abrasive coating dispersion with endothermic effect in this comparative example includes the following components in weight percentage: 25% stearate (ST-2), 0.5% dispersant (DS-1), 1% wetting agent (WT-1), 0.5% penetrant (PT-1), 10% adhesive (BE-1), 5% phase change material (PCM-1), 0.5% defoaming agent (DF-1), 0.5% preservative (AB-1) and 57% water (WT-1).

[0089] The preparation method of the anti-clogging coated abrasive tool coating dispersion with endothermic effect in this comparative example is the same as that in Example 1, the only difference is that the amount of water added in step (1) is 50%, and the amount of water added in step (6) is 7%.

[0090] Comparative Example 8

[0091] The anti-clogging coated abrasive coating dispersion with endothermic effect in this comparative example includes the following components in weight percentage: 20% stearate (ST-2), 0.5% dispersant (DS-1), 1% wetting agent (WT-1), 0.5% penetrant (PT-1), 10% adhesive (BE-1), 10% phase change material (PCM-1), 0.5% defoaming agent (DF-1), 0.5% preservative (AB-1) and 57% water (WT-1).

[0092] The preparation method of the anti-clogging coated abrasive tool coating dispersion with endothermic effect in this comparative example is the same as that in Example 1, the only difference is that the amount of water added in step (1) is 50%, and the amount of water added in step (6) is 7%.

[0093] Experimental example

[0094] 1. Dispersibility test: The anti-clogging coated abrasive coating dispersions with endothermic effect prepared in Examples 1-6 and Comparative Examples 1-8 were stirred and the dispersion was observed and recorded.

[0095] The dispersion grades and standards are as follows: completely dispersed without large agglomerated particles is grade A; partially dispersed with a small amount of agglomerated particles is grade B; a small amount of dispersed with a large amount of agglomerated particles is grade C, and particle sedimentation and stratification is grade D. The test results are shown in Table 1 below:

[0096] Table 1

[0097] sample Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Comparative Example 1 Dispersion level A-level A-level A-level A-level A-level A-level A-level sample Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 Comparative Example 7 Comparative Example 8 Dispersion level A-level A-level C-Class Class B Class B D-Class D-Class

[0098] From the above dispersibility test results, dispersants, wetting agents, and penetrants have a great influence on the dispersion characteristics of the anti-clogging coated abrasive coating dispersion with endothermic effect of the present invention, and the dispersant has the greatest influence. In addition, the phase change microcapsule material using polyurethane capsule wall is easier to form a uniform dispersed phase in the emulsion system. The uncoated inorganic phase change material, because of its large density, will gradually settle to the bottom of the emulsion after stopping stirring, resulting in stratification. In the use of anti-clogging coating products, particle agglomeration and stratification are generally not allowed to occur.

[0099] 2. Antibacterial and antifungal test:

[0100] Organic dispersed emulsion products often undergo microbial spoilage during storage due to the entry of different types of bacteria. For stearate dispersion coatings, preventing emulsion spoilage and demulsification is an important guarantee for ensuring product stability and extending product life.

[0101] The samples of Examples 1-6, Comparative Examples 1-3 and Comparative Examples 7-8 were taken out of a laboratory beaker and placed in a humid environment. After one month, the samples were observed for any decay.

[0102] If mildew, delamination, odor, etc. occur, it is marked as unqualified. If there is no obvious difference from the initial sample, it is marked as qualified. The test results are shown in Table 2 below:

[0103] Table 2

[0104] sample Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Antibacterial and anti-mildew qualified qualified qualified qualified qualified qualified sample Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 7 Comparative Example 8 / Antibacterial and anti-mildew qualified qualified Failure qualified qualified /

[0105] It can be seen from the above results that the use of isothiazolinone preservatives can effectively inhibit the corrosion of the endothermic anti-clogging coated abrasive coating dispersion of the present invention.

[0106] 3. Coatability test:

[0107] The dry sandpaper with a particle size of P320 produced by conventional methods and not coated with a plugging coating was selected as the material for the coatability verification test. The sandpaper substrate is 120g / m 2 Latex paper, base glue and surface glue are all urea-formaldehyde resin, and the abrasive is P320 ordinary brown corundum abrasive.

[0108] On the double-roll coating production line, the anti-clogging coated abrasive coating dispersions with endothermic effect of Examples 1-6 and Comparative Examples 1-3 and Comparative Examples 7-8 were selected and coated on P320 dry sandpaper respectively. Because in such coating production lines, bubbles are often generated by the introduction of air during the coating production stirring, transportation, and coating shearing process, and the generation of bubbles will greatly affect the uniformity and stability of the coating thickness. In addition, if the dispersed particles in the mixed coating have a certain sedimentation and stratification phenomenon, some solid sediments can be found in the slurry tray in the coating area during the coating process.

[0109] This test needs to observe whether there are many bubbles generated during the production process. For the situation of bubble generation, if there are no bubbles or a small number of bubbles, it is Class A, and if there are a large number of bubbles, it is Class B. After the coating is completed, the liquid in the slurry pan in the coating area can be drained, and it is often checked whether there is solid sediment in the slurry pan. The test results are shown in Table 3 below:

[0110] Table 3

[0111] sample Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Coatability A-level A-level A-level A-level A-level A-level Sedimentation results No sediment No sediment No sediment No sediment No sediment No sediment sample Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 7 Comparative Example 8 / Coatability A-level A-level Class B A-level A-level / Sedimentation results No sediment No sediment No sediment Small amount of sediment Large amount of sediment

[0112] From the above results, it can be seen that the addition of a suitable defoamer can effectively reduce the bubbles generated during stirring, transportation and coating shearing. In addition, the anti-clogging coated abrasive coating dispersion containing phase change microcapsules with endothermic effect basically does not have the phenomenon of particle sedimentation, while the anti-clogging coated abrasive coating dispersion with endothermic effect using inorganic phase change materials will have the phenomenon of particle sedimentation.

[0113] 4. Tests on anti-blocking performance, grinding temperature and grinding performance

[0114] Test method: The dry sandpaper with a particle size of P320 produced by conventional methods and not coated with blocking coating is selected as the material for the coatability verification test. The base material of the sandpaper is 120g / m 2 Latex paper, the base glue and the top glue are both urea-formaldehyde resin, and the abrasive is P320 common brown corundum abrasive. On the double-roll coating production line, the anti-clogging coated abrasive coating dispersion with endothermic effect of Examples 1-6, Comparative Examples 1-2 and Comparative Examples 7-8 are selected and coated on P320 dry sandpaper respectively, with a coating amount of 14g / m 2 The coated samples were dried in an oven at 70°C for 2 minutes.

[0115] The sandpaper prepared by the above method is used to make adhesive-backed sandpaper through double-sided tape, and then the sample is cut into 5-inch adhesive-backed sand discs.

[0116] A standard black metallic painted cold-rolled steel plate of 400 cm×60 cm was selected as the grinding workpiece, and a commercially available 5-inch eccentric vibration pneumatic grinder was selected as the grinder.

[0117] Put the sand disc on the plate of the grinder, increase the speed of the grinder to 12,000 rpm, and manually grind the paint board. The weight of the workpiece to be polished should be weighed before and after polishing. The difference is the amount of chips in a single polishing.

[0118] The environment of the grinding laboratory is 25℃ and 50% humidity. After every 1 minute of grinding, stop grinding, use an infrared temperature measuring gun to quickly test the temperature of the workpiece surface, record the grinding weight, and grind for a total of 5 minutes. After 5 minutes of grinding, check the blockage of the sand surface.

[0119] The blockage conditions are classified into the following categories:

[0120] A: Covered by dust, severely blocked; B: Dust particles agglomerated; C: Slightly blocked.

[0121] The test results of anti-blocking performance, grinding temperature and grinding performance are shown in Table 4 below:

[0122] Table 4

[0123]

[0124]

[0125] By comparing the grinding amount and the grinding interface temperature between Example 1 and Comparative Example 2, and between Example 2 and Comparative Example 2, it can be seen that the addition of phase change microcapsule material can effectively reduce the grinding interface temperature, reduce dust clogging on the sand surface, and increase the total grinding amount.

[0126] By comparing the test performance of Examples 1-6, Comparative Examples 1-2 and Comparative Examples 7-8 with the P320 uncoated sand disc, it can be seen that the grinding performance and anti-clogging performance of the coated product are significantly better than those of the uncoated product.

[0127] By comparing Example 1, Example 2 and Example 3, and by comparing Example 4 with Example 5, it can be seen that the coating performance of zinc stearate is better than that of calcium stearate or a mixture of calcium stearate and zinc stearate.

[0128] Through the comparison of Example 2, Comparative Example 7 and Comparative Example 8, it can be seen that the grinding performance and anti-clogging performance of the sandpaper prepared by adding the coating of phase change microcapsules are better than those directly adding the phase change material. Because the powder particles of the inorganic phase change material are directly added, the powder will gradually settle to the bottom of the emulsion after stirring and dispersing, affecting the amount of phase change material on the surface of the sandpaper finally coated. At the same time, after the inorganic phase change material coating is applied to the sandpaper, the inorganic powder particles will also settle to the bottom of the coating layer, affecting the uniformity of the dispersion of the inorganic phase change material in the coating layer and affecting the heat dissipation effect (through the previous dispersion experiment and coatability experiment, it can be seen that the direct use of uncoated phase change material in the process of dispersion and coating of the emulsion has different degrees of sedimentation and stratification problems, which will greatly affect the endothermic effect of the phase change material). In addition, although hydrated salt is an inorganic phase change material with excellent performance, most hydrated salts are unstable and are easily lost when exposed to air. Crystal water. This phenomenon will weaken the heat storage performance and stability of the phase change material, because after the heating-cooling cycle of the phase change material, the inorganic salt will be separated due to dehydration. Therefore, the hydrated salt not only needs to reduce the supercooling, but also needs a wrapping layer to protect it from the influence of the external environment in order to play a better effect.

[0129] Comparative Example 2 uses a higher stearate addition ratio (30%), while Comparative Examples 7 and 8 reduce the stearate addition ratio due to the introduction of inorganic phase change materials. However, the phase change material that can play a functional heat absorption role settles to the bottom of the emulsion in large quantities and cannot be evenly coated on the sandpaper surface. Therefore, compared with the sample of Comparative Example 2, the grinding temperature of the samples of Comparative Examples 7 and 8 is not significantly reduced, but the grinding amount is reduced more.

[0130] By comparing Example 2, Example 5 and Example 6, it can be seen that the grinding performance of the sandpaper prepared by adding the phase change microcapsules coated with modified polyurethane is better than the grinding performance of the sandpaper prepared by adding the phase change microcapsules coated with inorganic materials.

[0131] By comparing Example 1 with Example 6, it can be seen that increasing the proportion of phase change microcapsules can increase the heat absorption effect of the phase change microcapsules during the grinding process, slightly reduce the grinding temperature, and increase the grinding amount.

[0132] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. An anti-clogging coated abrasive coating dispersion having an endothermic effect, characterized in that: The invention comprises the following raw materials in weight percentage: Stearate 15%-40%, dispersant 0.1%-3%, wetting agent 0.2%-3%, penetrant 0.1%-3%, binder 5%-20%, phase change microcapsule 3%-15%, defoamer 0.1%-3%, preservative 0.1%-3% and water 40%-65%; The stearate is calcium stearate and / or zinc stearate; The dispersant is at least one of sodium alkyl biphenyl ether sulfonate, lignin sulfonate, alkylphenol polyoxyethylene ether formaldehyde condensate, sodium fatty alcohol polyoxyethylene ether sulfate, ammonium polyacrylate and sodium polyacrylate; The wetting agent is polyol polyoxyethylene ether and / or alkyl naphthalene sulfonate; The penetrant is at least one of ethanolamine, sodium sulfate, fatty alcohol polyoxyethylene ether and alkylphenol polyoxyethylene ether; The adhesive is at least one of acrylic emulsion, styrene-butadiene emulsion, styrene-acrylic emulsion and styrene-butadiene emulsion; The wall material of the phase change microcapsule is modified polyurethane; The defoamer is at least one of a fatty alcohol defoamer, a mineral oil defoamer, a silicone oil defoamer and a natural plant extract defoamer; The preservative is at least one of benzoic acid, sodium benzoate, sorbic acid, potassium sorbate and isothiazolinone.

2. The anti-clogging coated abrasive coating dispersion with endothermic effect as claimed in claim 1, characterized in that: The core material of the phase-change microcapsule is at least one of inorganic acid salts, aliphatic hydrocarbons, fatty acids, fatty acid esters and fatty acid salts.

3. The anti-clogging coated abrasive coating dispersion with endothermic effect as claimed in claim 1, characterized in that: The stearate is zinc stearate, the dispersant is sodium dodecylbenzene sulfonate, the wetting agent is polyol polyoxyethylene ether, the penetrant is alkylphenol polyoxyethylene ether, the adhesive is neutral styrene-acrylic acid copolymer emulsion, the defoamer is a fatty alcohol defoamer, and the preservative is an isothiazolinone preservative.

4. The anti-clogging coated abrasive coating dispersion with endothermic effect according to any one of claims 1 to 3, characterized in that: The particle size specification of the stearate is 180-1250 meshes.

5. The method for preparing the anti-clogging coated abrasive coating dispersion with endothermic effect according to any one of claims 1 to 4, characterized in that: The steps include: (1) First, fully stir 40%-50% by weight of water and 0.2%-3% by weight of a wetting agent; (2) Add 0.1%-3% by weight of dispersant and stir thoroughly; (3) Add 0.1%-3% by weight of penetrant and stir thoroughly; (4) Then, while continuing to stir, add 15% to 40% by weight of stearate and stir thoroughly; (5) pouring the material obtained in step (4) into a grinder for grinding, so that the average particle size D50 of the slurry after grinding is less than 10 μm; (6) Pour the ground slurry into a container, add 5% to 20% by weight of a binder and 3% to 15% by weight of water, and stir thoroughly; (7) Then, while continuing to stir, add 3% to 15% by weight of phase change microcapsules and stir thoroughly; (8) Add 0.1% to 3% by weight of a defoamer and 0.1% to 3% by weight of a preservative, and stir thoroughly to obtain the anti-clogging coated abrasive tool coating dispersion having an endothermic effect.

6. An anti-clogging coated abrasive coating with endothermic effect, characterized in that: The coating is prepared from the anti-clogging coated abrasive coating dispersion with endothermic effect as described in any one of claims 1 to 5.

7. An anti-clogging coated abrasive tool with heat absorption, characterized in that: The anti-clogging coated abrasive tool with endothermic effect has the coating as claimed in claim 6.

Citation Information

Patent Citations

  • Self-lubricating grinding tool and preparation method thereof

    CN101758463A

  • Phase-change microcapsule / UHMWPE (Ultrahigh Molecular Weight Polyethylene) wear-resistant material and preparation method thereof

    CN104004255A

  • Self-dressing ultra-hard micro grinding tool pellet containing soluble resin material and preparation method thereof

    CN106944939A

  • Preparation method of environment-friendly abrasive paper anti-blocking coating formula

    CN107778958A

  • Novel environment-friendly abrasive paper anti-blocking coating and preparation method thereof

    CN111021136A