A refractory high-entropy alloy that simultaneously achieves friction reduction and wear resistance at high temperatures, its preparation method, and its applications.
By using a refractory high-entropy alloy composed of Nb, Ta, V and W, and adding elements such as Zr, Mo and Si, a continuous and dense composite oxide layer is formed, which solves the problem of simultaneously achieving friction reduction and wear resistance at high temperatures. This results in a significant reduction in the coefficient of friction and wear rate, making it suitable for high-temperature self-lubricating wear-resistant components in aerospace and other fields.
Patent Information
- Application Number
- CN202410181491.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-18
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-02-18
AI Technical Summary
Existing metal alloys cannot simultaneously achieve friction reduction and wear resistance at high temperatures. The addition of traditional solid lubricants will deteriorate the mechanical properties of the material and have poor adhesion to the matrix. The oxide layer promotes friction and wear at high temperatures.
Refractory high-entropy alloys with Nb, Ta, V and W as the main components are prepared by adding elements such as Zr, Mo and Si through vacuum arc melting or sintering. The resulting continuous and dense composite oxide layer forms at high temperature, which plays a role in solid lubrication and anti-wear.
It achieves excellent friction reduction and wear resistance with a friction coefficient ≤0.3 and a wear rate ≤1×10-5mm3·N-1·m-1 at high temperatures, making it suitable for high-temperature self-lubricating wear-resistant parts in aerospace and other fields.
Smart Images

Figure CN118007002B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of refractory high-entropy alloy technology, and in particular to a refractory high-entropy alloy that simultaneously achieves friction reduction and wear resistance at high temperatures, its preparation method, and its application. Background Technology
[0002] Key hot-end components in aerospace and other fields operate under high-temperature conditions, making friction and wear one of the main failure modes. Developing high-temperature friction-reducing and wear-resistant materials is crucial for reducing energy dissipation and extending component service life. It has been reported that most metal alloys exhibit high friction coefficients (0.6–1.2) due to plastic deformation and microstructural changes in the friction sub-surface under dry friction. In actual production, solid lubricants are commonly used to reduce the friction coefficient of metal alloys. However, the addition of traditional solid lubricants (such as graphite, molybdenum disulfide, and metallic silver) often deteriorates the mechanical properties of the material and has poor adhesion to the matrix, making it difficult for most self-lubricating composite materials to meet service requirements. Furthermore, under high-temperature and oxygen-containing conditions, ambient temperature and the heat generated by friction jointly promote material oxidation; therefore, the oxide layer dominates the interfacial friction and wear behavior. Studies have shown that some metal oxides have low shear strength at high temperatures and can also be used as high-temperature solid lubricants.
[0003] As a novel class of alloy materials, high-entropy alloys (HEAs) have attracted widespread attention due to their unique structural and performance characteristics. Refractory high-entropy alloys (RHEAs) refer to high-entropy alloys mainly composed of high-melting-point refractory metal elements in equimolar or near-equimolar ratios. Furthermore, the large compositional space and unique "cocktail" effect provide more opportunities for the design and development of refractory high-entropy alloys. Refractory high-entropy alloys possess high-temperature strength and hardness unmatched by traditional high-temperature alloys, thus holding promise for achieving excellent high-temperature tribological properties. However, to date, there have been no reports of refractory high-entropy alloys simultaneously achieving friction reduction and wear resistance at high temperatures. Summary of the Invention
[0004] The purpose of this invention is to provide a refractory high-entropy alloy that simultaneously achieves friction reduction and wear resistance at high temperatures, as well as its preparation method and applications. The refractory high-entropy alloy can simultaneously achieve friction reduction and wear resistance at high temperatures.
[0005] To achieve the above-mentioned objectives, the present invention provides the following technical solution:
[0006] This invention provides a refractory high-entropy alloy that simultaneously achieves friction reduction and wear resistance at high temperatures, comprising Nb, Ta, V, and W;
[0007] The molar ratio of Nb, Ta, V and W is (21-35):(24-36):(32-44):(4-8).
[0008] Preferably, it also includes adding elements;
[0009] The added elements include one or more of Zr, Mo and Si.
[0010] Preferably, the molar ratio of Nb to the added element is (21-35):(0-4);
[0011] Furthermore, the molar quantity of the added element is not zero.
[0012] This invention also provides a method for preparing the refractory high-entropy alloy described above, comprising the following steps:
[0013] The refractory high-entropy alloy is prepared by mixing the raw materials of the refractory high-entropy alloy using vacuum arc melting or sintering.
[0014] Preferably, when the preparation method uses vacuum arc melting, the number of times the ingot is flipped and remelted is ≥5, the melting current of each remelting is ≥500A independently, and the remelting time of each remelting is ≥2min independently.
[0015] Preferably, before the vacuum arc melting, the vacuum arc melting furnace is first evacuated to a vacuum level of 8.5 × 10⁻⁶. -4 Pa, then fill with argon gas to -0.06 MPa.
[0016] Preferably, the sintering method includes spark plasma sintering or vacuum hot pressing sintering.
[0017] Preferably, the sintering temperature is ≥1600℃ and the time is ≥20min.
[0018] Preferably, the sintering process is carried out in a vacuum environment, and the sintering pressure is ≥20MPa.
[0019] The present invention also provides the application of the refractory high-entropy alloy described in the above technical solution or the refractory high-entropy alloy prepared by the preparation method described in the above technical solution in the field of high-temperature friction reduction and wear resistance.
[0020] This invention provides a refractory high-entropy alloy that simultaneously achieves friction reduction and wear resistance at high temperatures, comprising Nb, Ta, V, and W; wherein the molar ratio of Nb, Ta, V, and W is (21–35):(24–36):(32–44):(4–8). During high-temperature friction, the refractory high-entropy alloy of this invention undergoes a tribochemical reaction, forming a continuous and dense composite oxide layer on the wear surface. On one hand, this composite oxide layer has low shear strength, acting as a solid lubricant; on the other hand, this composite oxide layer prevents direct contact between friction pairs, providing excellent wear resistance. Compared with most metal-based self-lubricating composite materials and wear-resistant materials, the refractory high-entropy alloy of this invention exhibits superior friction reduction and wear resistance at high temperatures (around 800°C), and its chemical composition and preparation process are simple, making it promising for application in high-temperature self-lubricating wear-resistant components in aerospace and other fields. According to the embodiments, the refractory high-entropy alloy of this invention has a friction coefficient ≤0.3 and a wear rate ≤1×10⁻⁶ at a high temperature of around 800°C. -5 mm 3 ·N -1 ·m -1 . Attached Figure Description
[0021] Figure 1 The friction coefficient curve and two-dimensional profile of the wear track cross section of the refractory high-entropy alloy in Example 1 at 800℃ are shown.
[0022] Figure 2 The friction coefficient curve and two-dimensional profile of the wear track cross section of the refractory high-entropy alloy in Example 2 at 850°C are shown.
[0023] Figure 3 The friction coefficient curve and two-dimensional profile of the wear track cross section of the refractory high-entropy alloy in Example 3 at 800℃ are shown. Detailed Implementation
[0024] This invention provides a refractory high-entropy alloy that simultaneously achieves friction reduction and wear resistance at high temperatures, comprising Nb, Ta, V, and W;
[0025] The molar ratio of Nb, Ta, V and W is (21-35):(24-36):(32-44):(4-8).
[0026] In this invention, the molar ratio of Nb, Ta, V and W is (21-35):(24-36):(32-44):(4-8), preferably (25-30):(28-32):(35-40):(5-7).
[0027] In this invention, the refractory high-entropy alloy preferably includes additive elements; the additive elements preferably include one or more of Zr, Mo and Si. When the additive elements are two or more of the above-mentioned specific selections, this invention does not impose any special limitation on the proportion of the above-mentioned specific substances, and they can be mixed in any proportion.
[0028] In this invention, the molar ratio of Nb to the added element is preferably (21-35):(0-4), more preferably (25-30):(1-3); and the molar amount of the added element is not 0.
[0029] This invention also provides a method for preparing the refractory high-entropy alloy described above, comprising the following steps:
[0030] The refractory high-entropy alloy is prepared by mixing the raw materials of the refractory high-entropy alloy using vacuum arc melting or sintering.
[0031] In this invention, unless otherwise specified, all raw materials used in the preparation are commercially available products well known to those skilled in the art.
[0032] In this invention, when the preparation method employs vacuum arc melting, the refractory high-entropy alloy raw material is preferably a metallic element corresponding to a refractory metal. Before mixing, the refractory high-entropy alloy raw material is preferably subjected to mechanical grinding and ultrasonic cleaning sequentially; the purity of the refractory high-entropy alloy raw material is preferably ≥99.9 wt%; the mechanical grinding process is not particularly limited in this invention, and a process well-known to those skilled in the art is used to ensure the removal of oxide scale from the surface of the raw material particles. In this invention, the ultrasonic cleaning is preferably performed in anhydrous ethanol.
[0033] The present invention does not impose any special limitations on the mixing process; any process known to those skilled in the art can be used.
[0034] In this invention, the preferred process of vacuum arc melting is as follows: the refractory high-entropy alloy raw materials are mixed and placed in a water-cooled copper crucible; the vacuum arc melting furnace is then evacuated sequentially using a mechanical pump and a molecular pump, followed by the introduction of high-purity argon gas for vacuum arc melting. In this invention, the pressure after evacuation is preferably ≤8.5×10⁻⁶. -4 Pa; the furnace pressure after being filled with high-purity argon is preferably -0.06 MPa.
[0035] In this invention, the number of times the ingot is flipped and remelted is preferably ≥5, more preferably 7 to 10 times; the melting current for each remelting is preferably ≥500A, more preferably 600 to 800A; and the remelting time for each remelting is preferably ≥2 minutes, more preferably 2.5 to 4 minutes. After each remelting is completed, this invention also preferably includes reducing the current to 0 before flipping the ingot for the next remelting.
[0036] In this invention, the process of melting and absorbing oxygen in titanium ingots is preferably performed before vacuum arc melting; there are no special limitations on the process of melting and absorbing oxygen in this invention, and any process known to those skilled in the art can be used.
[0037] In this invention, when the preparation method employs sintering, the sintering method preferably includes spark plasma sintering or vacuum hot pressing sintering.
[0038] In this invention, when the sintering method is spark plasma sintering, the raw material of the refractory high-entropy alloy is preferably ball-milled before mixing; the purity of the raw material of the refractory high-entropy alloy is preferably ≥99.5wt%, and the particle size is ≤50μm; this invention does not impose any special limitations on the ball milling process, and any process well known to those skilled in the art can be used. In an embodiment of this invention, the grinding media used in the ball milling are agate balls with a diameter of 3-10mm, the ball-to-material ratio is 3:1, the ball milling time is 24h, and the rotation speed is 150r / min.
[0039] In this invention, when the sintering method is vacuum hot pressing sintering, the refractory high-entropy alloy raw material is preferably ball-milled before mixing; the purity of the refractory high-entropy alloy raw material is preferably ≥99.5wt%, and the particle size is ≤50μm; this invention does not impose any special limitations on the ball milling process, and any process well known to those skilled in the art can be used. In an embodiment of this invention, the grinding media used in the ball milling are agate balls with a diameter of 3-10mm, the ball-to-material ratio is 3:1, the ball milling time is 24h, and the rotation speed is 150r / min.
[0040] In this invention, the sintering temperature is preferably ≥1600℃, more preferably 1650~1800℃; the time is preferably ≥20min, more preferably 25~35min; the sintering is preferably carried out in a vacuum environment, and the sintering pressure is preferably ≥20MPa, more preferably 25~30MPa. In this invention, the furnace body is preferably evacuated to below 5Pa before sintering.
[0041] After the vacuum arc melting or sintering is completed, the present invention preferably includes processing the obtained ingot with electrical discharge wire cutting to obtain a sample with a size of Φ25×2mm, grinding and polishing the sample surface with SiC sandpaper of specifications of 80#, 240#, 400#, 800#, 1200# and 1500# in sequence, and then ultrasonically cleaning it in anhydrous ethanol.
[0042] This invention also provides the application of the refractory high-entropy alloy described in the above-described technical solutions or the refractory high-entropy alloy prepared by the preparation method described in the above-described technical solutions in the field of high-temperature friction reduction and wear resistance. This invention does not impose any special limitations on the methods for these applications; methods well-known to those skilled in the art can be used.
[0043] The following detailed description, in conjunction with embodiments, illustrates the refractory high-entropy alloy that simultaneously achieves friction reduction and wear resistance at high temperatures, its preparation method, and its applications. However, these descriptions should not be construed as limiting the scope of protection of this invention.
[0044] Example 1
[0045] The elemental composition of the refractory high-entropy alloy is: Nb 30 at.%, Ta 30 at.%, V 35 at.% and W 5 at.%.
[0046] Preparation methods of refractory high-entropy alloys:
[0047] Raw material particles with a purity greater than 99.9 wt% (niobium particles, tantalum particles, vanadium particles, and tungsten particles, respectively) were taken. The oxide scale on the surface of the raw material particles was removed by mechanical grinding, and ultrasonic cleaning was performed in anhydrous ethanol. The raw material particles with a total mass of 100g were weighed according to the formula using an electronic analytical balance, with an accuracy of 0.01g.
[0048] After weighing and mixing the raw materials, place them into a water-cooled copper crucible. Then, sequentially use a mechanical pump and a molecular pump to evacuate the vacuum in the vacuum arc melting process to 8.5 × 10⁻⁶. -4 Pa, then high-purity argon gas was introduced into the furnace to a pressure of -0.06 MPa. After igniting the electric arc, the melting current was slowly increased to 650 A and maintained for 3 minutes before being reduced to 0, completing one melting cycle. Each sample was flipped and remelted 8 times. The ingot was then processed using wire EDM to obtain a sample with dimensions of Φ25×2 mm. The sample surface was polished sequentially using SiC sandpaper of specifications 80#, 240#, 400#, 800#, 1200#, and 1500#. Then, it was ultrasonically cleaned in anhydrous ethanol to obtain a refractory high-entropy alloy (Nb). 30 Ta 30 V 35 W5);
[0049] The high-temperature tribological properties of the refractory high-entropy alloy were tested using an HT-1000 high-temperature friction and wear testing machine. The mating material used was silicon nitride spheres with a diameter of 6 mm. The test load was 5 N, the sliding speed was 0.2 m / s, the test time was 1800 s, and the test temperatures were 25℃, 300℃, 600℃, 700℃, 750℃, 800℃, 850℃, and 900℃. Figure 1 The friction coefficient curve and two-dimensional profile of the wear track cross-section of the refractory high-entropy alloy at 800℃ are shown below. Figure 1 It can be seen that after the frictional running stage, the friction coefficient stabilizes at around 0.13, and the width and depth of the wear tracks are relatively small. The average friction coefficient and wear rate at various temperatures are shown in Table 1.
[0050] Table 1. Tribological property parameters of the refractory high-entropy alloy described in Example 1
[0051] Test temperature (°C) coefficient of friction <![CDATA[Wear rate (mm 3 ·N -1 ·m -1 )]]> 25 0.72 <![CDATA[2.5×10 -4 ]]> 300 0.74 <![CDATA[1.8×10 -4 ]]> 600 0.68 <![CDATA[7.6×10 -5 ]]> 700 0.52 <![CDATA[7.2×10 -6 ]]> 750 0.21 <![CDATA[5.4×10 -6 ]]> 800 0.13 (e.g.) Figure 1 (As shown) <![CDATA[3.9×10 -6 ]]> 850 0.15 <![CDATA[6.5×10 -6 ]]> 900 0.27 <![CDATA[1.7×10 -4 ]]>
[0052] As shown in Table 1, the refractory high-entropy alloy exhibits a low coefficient of friction (≤0.3) at temperatures above 750°C, particularly as low as 0.13 at 800°C. Furthermore, within the temperature range of 700–850°C, the wear rate of the refractory high-entropy alloy is consistently as low as 10%. -6 The order of magnitude; therefore, the refractory high-entropy alloy exhibits excellent friction reduction and wear resistance within the temperature range of 700–850°C.
[0053] Example 2
[0054] The elemental composition of the refractory high-entropy alloy is: Nb 25 at.%, Ta 29 at.%, V 36 at.%, W 7 at.% and Si 3 at%.
[0055] Preparation methods of refractory high-entropy alloys:
[0056] Raw material particles (niobium, tantalum, vanadium, tungsten, and silicon particles) with a purity greater than 99.5 wt% and a particle size less than 50 μm were selected. Using an electronic analytical balance, 100 g of each powder was weighed according to the specified proportions, accurate to 0.01 g. The raw material particles were then mixed and placed in a planetary ball mill for ball milling. Agate balls with a diameter of 3–10 mm were used as the grinding media, with a ball-to-material ratio of 3:1. The milling time was 24 hours, and the rotation speed was 150 r / min. 40 g of the milled powder was then loaded into a 25 μm diameter... A graphite mold of size m was sintered in a spark plasma sintering furnace at a temperature of 1700℃ for 30 minutes and a pressure of 25MPa. The vacuum level inside the furnace was maintained at approximately 3Pa during the sintering process. The ingot was then machined using wire electrical discharge machining to obtain a sample with dimensions Φ25×2mm. The sample surface was successively polished using SiC abrasive paper of grades 80#, 240#, 400#, 800#, 1200#, and 1500#. Finally, the sample was ultrasonically cleaned in anhydrous ethanol to obtain a refractory high-entropy alloy (Nb). 25 Ta 29 V 36 W7Si3);
[0057] The high-temperature tribological properties of the refractory high-entropy alloy were tested using an HT-1000 high-temperature friction and wear testing machine. The mating material used was silicon nitride spheres with a diameter of 6 mm. The test load was 5 N, the sliding speed was 0.2 m / s, the test time was 1800 s, and the test temperatures were 25℃, 300℃, 600℃, 700℃, 750℃, 800℃, 850℃, and 900℃. Figure 2 The friction coefficient curve and two-dimensional profile of the wear track cross-section of the refractory high-entropy alloy at 850℃ are shown below. Figure 2 It can be seen that after the frictional running stage, the friction coefficient eventually stabilizes at around 0.19, and the width and depth of the wear tracks are relatively small. The average friction coefficient and wear rate at various temperatures are shown in Table 2.
[0058] Table 2. Tribological property parameters of the refractory high-entropy alloy described in Example 2.
[0059] Test temperature (°C) coefficient of friction <![CDATA[Wear rate (mm 3 ·N -1 ·m -1 )]]> 25 0.67 <![CDATA[1.7×10 -4 ]]> 300 0.64 <![CDATA[2.8×10 -4 ]]> 600 0.59 <![CDATA[5.3×10 -5 ]]> 700 0.61 <![CDATA[9.7×10 -6 ]]> 750 0.38 <![CDATA[4.9×10 -6 ]]> 800 0.23 <![CDATA[7.1×10 -6 ]]> 850 0.19 (e.g.) Figure 2 (As shown) <![CDATA[3.5×10 -6 ]]> 900 0.35 <![CDATA[6.3×10 -5 ]]>
[0060] As shown in Table 2, the refractory high-entropy alloy exhibits a low coefficient of friction (≤0.3) at temperatures greater than or equal to 800–850°C, especially at 850°C where the coefficient of friction is as low as 0.19. Furthermore, within the temperature range of 700–850°C, the wear rate of the refractory high-entropy alloy is consistently as low as 10%. -6 The order of magnitude; therefore, the refractory high-entropy alloy exhibits both excellent friction reduction and wear resistance within the range of 800–850°C.
[0061] Example 3
[0062] The elemental composition of the refractory high-entropy alloy is: Nb 26 at.%, Ta 28 at.%, V 40 at.%, W 5 at.% and Mo 1 at.%.
[0063] Preparation methods of refractory high-entropy alloys:
[0064] Raw material particles with a purity greater than 99.9 wt% (niobium particles, tantalum particles, vanadium particles, tungsten particles, and molybdenum particles, respectively) were taken. The oxide scale on the surface of the raw material particles was removed by mechanical grinding, and ultrasonic cleaning was performed in anhydrous ethanol. 100g of raw material particles were weighed according to the proportions using an electronic analytical balance, with an accuracy of 0.01g.
[0065] After weighing and mixing the raw materials, place them into a water-cooled copper crucible. Then, sequentially use a mechanical pump and a molecular pump to evacuate the vacuum in the vacuum arc melting process to 8.5 × 10⁻⁶. -4 Pa, then high-purity argon gas was introduced into the furnace to a pressure of -0.06 MPa. After igniting the electric arc, the melting current was slowly increased to 650 A and maintained for 3 minutes before being reduced to 0, completing one melting cycle. Each sample was flipped and remelted 8 times. The ingot was then processed using wire EDM to obtain a sample with dimensions of Φ25×2 mm. The sample surface was polished sequentially using SiC sandpaper of specifications 80#, 240#, 400#, 800#, 1200#, and 1500#. Then, it was ultrasonically cleaned in anhydrous ethanol to obtain a refractory high-entropy alloy (Nb). 30 Ta 30 V 35 W5);
[0066] The high-temperature tribological properties of the refractory high-entropy alloy were tested using an HT-1000 high-temperature friction and wear testing machine. The mating material used was silicon nitride spheres with a diameter of 6 mm. The test load was 5 N, the sliding speed was 0.2 m / s, the test time was 1800 s, and the test temperatures were 25℃, 300℃, 600℃, 700℃, 750℃, 800℃, 850℃, and 900℃. Figure 3 The friction coefficient curve and two-dimensional profile of the wear track cross-section of the refractory high-entropy alloy at 800℃ are shown below. Figure 3 It can be seen that the coefficient of friction fluctuated significantly throughout the testing phase, but remained relatively low, between 0.15 and 0.25, and the width and depth of the wear tracks were also small. The average coefficient of friction and wear rate at each temperature are shown in Table 3.
[0067] Table 3. Tribological property parameters of the refractory high-entropy alloy described in Example 3.
[0068]
[0069]
[0070] As shown in Table 3, the refractory high-entropy alloy exhibits a low coefficient of friction (≤0.3) at 800–850°C, especially as low as 0.21 at 800°C; furthermore, the wear rate of the refractory high-entropy alloy is as low as 10% within the temperature range of 700–850°C. -6 The order of magnitude; therefore, the refractory high-entropy alloy exhibits excellent friction reduction and wear resistance within the temperature range of 700–850°C.
[0071] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A refractory high-entropy alloy that simultaneously achieves friction reduction and wear resistance at high temperatures, characterized in that, The elemental composition is Nb, Ta, V, and W; The molar ratio of Nb, Ta, V and W is (21~35):(24~36):(32~44):(4~8); This also includes adding elements; The added elements include one or more of Zr, Mo, and Si; The molar ratio of Nb to the added element is (21~35):(0~4); And the molar quantity of the added element is not zero; The preparation method of the refractory high-entropy alloy includes the following steps: The refractory high-entropy alloy is prepared by mixing the raw materials of the refractory high-entropy alloy using vacuum arc melting or sintering. When the preparation method uses vacuum arc melting, the number of times the ingot is flipped and remelted is ≥5, the melting current of each remelting is ≥500A independently, and the remelting time of each remelting is ≥2min independently. Before the vacuum arc melting process, the vacuum arc melting furnace is first evacuated to a vacuum level of 8.5 × 10⁻⁶. -4 Pa, then argon gas is introduced to -0.06 MPa; The sintering method includes spark plasma sintering or vacuum hot pressing sintering. The sintering temperature is ≥1600℃ and the time is ≥20min; The sintering is carried out in a vacuum environment at a pressure ≥20MPa.
2. The method for preparing the refractory high-entropy alloy according to claim 1, characterized in that, The steps are as follows: The refractory high-entropy alloy is prepared by mixing the raw materials of the refractory high-entropy alloy using vacuum arc melting or sintering. When the preparation method uses vacuum arc melting, the number of times the ingot is flipped and remelted is ≥5, the melting current of each remelting is ≥500A independently, and the remelting time of each remelting is ≥2min independently. Before the vacuum arc melting process, the vacuum arc melting furnace is first evacuated to a vacuum level of 8.5 × 10⁻⁶. -4 Pa, then argon gas is introduced to -0.06 MPa; The sintering method includes spark plasma sintering or vacuum hot pressing sintering. The sintering temperature is ≥1600℃ and the time is ≥20min; The sintering is carried out in a vacuum environment at a pressure ≥20MPa.
3. The application of the refractory high-entropy alloy of claim 1 or the refractory high-entropy alloy prepared by the preparation method of claim 2 in the field of high-temperature friction reduction and wear resistance.
Citation Information
Patent Citations
WNbMoTaVZr series refractory high-entropy alloy and preparation method thereof
CN113088786A
Preparation process of refractory high-entropy alloy coating resistant to high-temperature friction and wear
CN114657550A
High-strength and high-hardness W-Ta-V-Zr series refractory high-entropy alloy and preparation method thereof
CN114941099A
Hight-entropy multioelement alloy with single phase and process for preparing the same