A composite electrode sheet for a battery, its fabrication process, and a solid-state battery
By employing a concave-convex embedded structure for the battery electrode design in all-solid-state batteries, the problems of high interface impedance and electrode expansion and detachment during charging and discharging are solved, thereby improving the cycle performance and safety of the battery.
Patent Information
- Application Number
- CN202410352431.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-26
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-03-26
AI Technical Summary
Existing all-solid-state batteries suffer from problems such as high electrode interfacial impedance and electrode volume expansion during charging and discharging, which leads to the shedding of the positive electrode material layer, electrolyte layer, and negative electrode layer, resulting in short cycle life and poor rate performance.
The battery electrode design with a concave-convex embedded structure involves spreading a solid electrolyte on the positive electrode and setting a positive current collector, pressing it into a positive electrode composite sheet with a concave-convex structure, and then filling the groove with negative electrode material and setting a negative current collector to form a concave-convex embedded battery composite electrode sheet.
It enhances the contact tightness between the positive electrode material layer, the solid electrolyte layer and the negative electrode material layer, reduces interface resistance, improves the cycle performance, rate performance and safety of the battery, and overcomes the problem of electrode expansion and shedding during charging and discharging.
Smart Images

Figure CN118016809B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery manufacturing technology, specifically to a composite electrode sheet for a battery, a manufacturing process, and a solid-state battery. Background Technology
[0002] With the large-scale use of fossil fuels, the concentration of greenhouse gases in the atmosphere has been increasing year by year. Simultaneously, the widespread use of internal combustion engines has further exacerbated this process, leading to global warming, frequent extreme weather events, and threatening humanity's future living environment. Therefore, humanity is actively developing cleaner new energy sources, such as wind, solar, and tidal energy. However, the acquisition methods of these new energy sources are not stable enough, fluctuating significantly due to external environmental factors such as weather, climate, and seasons. Therefore, they are not suitable for direct supply and require appropriate energy storage equipment to ensure a stable supply to end users. Lithium-ion and sodium-ion liquid rechargeable batteries, with their advantages of high cycle life, high power, no memory effect, and high energy density, have been widely used in energy storage and electric vehicle fields.
[0003] However, organic electrolytes in liquid batteries have drawbacks such as volatility, toxicity, leakage, susceptibility to short circuits and fires, and high cost. Furthermore, the energy density of liquid batteries has almost reached its limit, leaving little room for improvement, thus hindering the continued development of the new energy industry. To further improve the energy density, safety, and economy of batteries, researchers have developed all-solid-state batteries with higher energy density, better safety, and no electrolyte. However, current all-solid-state batteries still suffer from drawbacks such as high solid-solid interface impedance, poor conductivity, low rate performance, and large volume deformation during charge and discharge. This is because there is no electrolyte filling between particles within the active material of solid-state batteries, or between the foil and the active material interface. The gaps between various solid particles lack a transport medium, resulting in poor electronic and ionic conductivity within the battery. In addition, some positive electrode active materials (such as sulfur positive electrode materials) exhibit an expansion rate as high as 79% during lithium-ion insertion / extraction, severely impacting the cycle life and rate performance of solid-state batteries, making large-scale commercialization of all-solid-state batteries difficult.
[0004] For example, CN 110265707 A discloses a method for manufacturing an all-solid-state battery and an all-solid-state battery. The method involves stacking a negative electrode foil, a negative electrode layer, a solid electrolyte layer, and a positive electrode layer in this order, with the areas of the solid electrolyte layer and the negative electrode layer being larger than the area of the positive electrode layer. The method includes a first pressing step, where, for a laminate containing a negative electrode foil and a negative electrode layer, or a laminate containing a negative electrode foil, a negative electrode layer, and a solid electrolyte layer (i.e., a first laminate), the adhesion force between the negative electrode foil and the negative electrode layer is set to 30 N / cm. 2The above method is used for rolling to form the second laminate; in the laminate formation process, the second laminate is used to form a third laminate containing a negative electrode foil, a negative electrode layer, a solid electrolyte layer, and a positive electrode layer; in the second pressing process, the third laminate is rolled at a linear pressure of 1.0 t / cm or higher to form a fourth laminate. Clearly, this all-solid-state battery manufacturing method uses conventional pressing to combine the positive electrode, separator, and negative electrode together, which cannot overcome the problems of expansion and excessive interfacial impedance during charge and discharge of solid-state batteries. Therefore, with the increase of cycle number, the electrochemical performance of the solid-state battery will decrease, thus affecting the user experience. Summary of the Invention
[0005] The purpose of this invention is to provide a composite electrode sheet for a battery, a preparation process, and a solid-state battery, so as to solve the problem of high interfacial impedance of the electrode sheet in existing all-solid-state batteries. It can also solve the defects of short cycle life and poor rate performance of solid-state batteries caused by the volume expansion of the electrode sheet during charging and discharging, which leads to the shedding of the positive electrode material layer, electrolyte layer and negative electrode layer.
[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows: A process for fabricating a composite electrode sheet for a battery includes the following steps: S1. Spread a solid electrolyte on the upper surface of the positive electrode sheet, set a positive current collector on the lower surface of the positive electrode sheet, and then press it into a positive electrode composite sheet with an uneven structure. S2. Fill the groove of the positive electrode composite sheet with negative electrode material and make the negative electrode material extend beyond the edge of the groove. Place a negative electrode current collector on the negative electrode material and then press it into a composite electrode sheet for the battery.
[0007] Based on the aforementioned technical means, by simultaneously pressing the solid electrolyte, positive electrode sheet, and positive current collector, the fusion of the solid electrolyte and positive electrode sheet interface can be effectively promoted during the pressing process. Additionally, some solid electrolyte can infiltrate the positive electrode material, increasing the tightness of the connection between the electrolyte layer and the positive electrode material, reducing interfacial impedance, and improving conductivity. This also effectively simplifies the pressing process and improves the manufacturing efficiency of the battery cell. Simultaneously, by filling the grooves of the positive electrode composite sheet with negative electrode material, extending the negative electrode material beyond the edge of the groove, and then pressing it, a concave-convex interlocking structure is created between the negative electrode material and the positive electrode composite sheet. This effectively increases the contact area between the negative electrode material layer and the positive electrode composite sheet, thereby increasing the lithium-ion transport area, improving the electronic and ionic conductivity at the battery electrode interface, further reducing interfacial impedance. Furthermore, the concave-convex interlocking structure effectively overcomes the hazards of positive electrode material peeling off from the positive current collector and negative electrode material peeling off from the negative current collector, mitigating electrode volume changes during charging and discharging and reducing the problem of expansion, detachment, and material loss. Therefore, the concave-convex embedded battery electrode structure not only effectively enhances the contact tightness between the positive electrode material layer, the solid electrolyte layer and the negative electrode material layer and reduces the interface resistance, but also effectively overcomes the problem of battery electrode expansion and detachment during the charging and discharging process of ordinary solid battery electrodes, thereby improving the overall cycle performance, rate performance and safety of the battery.
[0008] Preferably, the uneven structure of the positive electrode composite sheet has a smooth transition.
[0009] By designing the concave-convex structure of the positive electrode composite sheet into a smooth transition, the tight contact between the positive electrode sheet, solid electrolyte, and negative electrode sheet is ensured, further reducing interface impedance. This reduces current obstruction and loss in the concave-convex structure during battery operation, improving current transmission efficiency. At the same time, the smooth transition also helps avoid stress concentration during battery charging and discharging, thereby reducing damage to the internal battery structure and performance degradation, thus ensuring the stability of the battery's cycle performance, rate performance, and service life.
[0010] Preferably, the depth of the groove in the positive electrode composite sheet is between 5 and 30 μm.
[0011] Since excessive groove depth can damage the solid electrolyte layer, while insufficient groove depth can lead to insignificant effects, experimental verification has shown that the groove depth of the positive electrode composite sheet should be controlled between 5 and 30 μm.
[0012] Preferably, the spread thickness of the solid electrolyte is between 15 μm and 50 μm.
[0013] By properly controlling the spreading thickness of the solid electrolyte, tearing or porosity problems can be effectively avoided during the subsequent pressing process.
[0014] Preferably, the height of the negative electrode material extending beyond the edge of the groove is 140um to 200um.
[0015] Preferably, in step S1, a positive electrode composite sheet with an uneven structure is formed by roller pressing, and the roller pressing temperature for forming the positive electrode composite sheet is 80~180℃.
[0016] By using a roll forming method to create a positive electrode composite sheet with a concave-convex structure, the contact area between the positive electrode sheet and the solid electrolyte is effectively increased, reducing the interfacial resistance. At the same time, by reasonably controlling the roll forming temperature, the solid electrolyte is kept in a molten state. When the solid electrolyte is combined with the positive electrode sheet, some electrolyte is immersed in the positive electrode material, which further increases the tightness of the connection between the electrolyte layer and the positive electrode active material, reducing the interfacial resistance. Moreover, the solid electrolyte and the positive electrode sheet are simultaneously composited with a concave-convex structure, which effectively simplifies the roll forming process and improves the cell manufacturing efficiency.
[0017] Preferably, in step S2, the composite electrode sheet for the battery is formed by rolling, and the rolling temperature for forming the composite electrode sheet for the battery is 80~180℃.
[0018] Preferably, before S1, the process further includes: premixing, coating, fiberizing and rolling of the positive electrode material, and premixing, coating and fiberizing of the negative electrode material.
[0019] Preferably, the premixing of the positive electrode material includes: mixing the positive electrode active material, conductive agent and binder in a reactor at a temperature of 5℃~15℃ to obtain a positive electrode premixed mixture; wherein, during premixing, the rotation speed of the dispersion disc in the reactor is between 100~200 rpm, and the rotation speed of the inner wall of the reactor is between 10~50 rpm.
[0020] By premixing the positive electrode active material, conductive agent, and binder, the surface of the positive electrode active material is uniformly covered with conductive agent and binder, which effectively improves the ionic conductivity and adhesion performance of the positive electrode active material, lays a solid foundation for subsequent process steps, and effectively ensures the smooth progress of the entire production process and the stable improvement of product quality.
[0021] Preferably, the premixing of the negative electrode material includes: mixing the negative electrode active material, conductive agent and binder in a reactor at a temperature of 5℃~15℃ to obtain a negative electrode premixed mixture; wherein, during premixing, the rotation speed of the dispersion disc in the reactor is between 100~200 rpm, and the rotation speed of the inner wall of the reactor is between 10~50 rpm.
[0022] By premixing the negative electrode active material, conductive agent, and binder, the surface of the negative electrode active material is uniformly covered with conductive agent and binder, which effectively improves the ionic conductivity and adhesion performance of the negative electrode active material, laying a solid foundation for subsequent process steps and effectively ensuring the smooth progress of the entire production process and the stable improvement of product quality.
[0023] Preferably, the coating of the positive electrode material includes: raising the temperature to 18°C~25°C, mixing the positive electrode premixed mixture in a reactor, and obtaining a positive electrode premixed mixture with a conductive agent coated on the surface; wherein, during coating, the rotation speed of the dispersion disk in the reactor is between 1000~2500 rpm, and the rotation speed of the inner wall of the reactor is between 20~45 rpm.
[0024] By adjusting the temperature and reactor speed to further mix the positive electrode premix, a high specific surface area conductive agent can be coated on the surface of the positive electrode premix, effectively increasing the electronic conductivity of the positive electrode material. At the same time, it can also constrain the volume stress of the positive electrode material during the charging and discharging process to a certain extent, and the coating can be achieved without adding any new additives.
[0025] Preferably, the coating of the negative electrode material includes: raising the temperature to 18°C~25°C, mixing the negative electrode premixed mixture in a reactor, and obtaining a negative electrode premixed mixture with a conductive agent coated on the surface; wherein, during coating, the rotation speed of the dispersion disk in the reactor is between 1000~2500 rpm, and the rotation speed of the inner cylinder wall of the reactor is between 10~50 rpm.
[0026] By adjusting the temperature and reactor speed to further mix the negative electrode premix, a high specific surface area conductive agent can be coated on the surface of the negative electrode premix, effectively increasing the electronic conductivity of the negative electrode material. At the same time, it can also constrain the volume stress of the negative electrode material during the charging and discharging process to a certain extent, and the coating can be achieved without adding any new additives.
[0027] Preferably, the fiberization of the positive electrode material includes: raising the temperature to 60°C~70°C, so that the positive electrode premixed mixture with the conductive agent coated on the surface continues to react in the reactor to obtain the positive electrode material; wherein, during fiberization, the dispersion disk of the reactor rotates at 3000~5000 rpm, and the inner cylinder wall of the reactor rotates at 10~50 rpm.
[0028] Since the binder in the cathode material is generally in the initial state of granules, it can only bond point-to-point, resulting in poor bonding effect. After fiberization, the granular binder will form long fibrous strips. The fiberized binders are connected to each other to form a network structure, which makes the binder not only sticky, but also able to constrain the volume expansion of the cathode active material during the charging and discharging process, effectively improving the cycle performance of the cathode material.
[0029] Preferably, the fiberization of the negative electrode material includes: raising the temperature to 60°C~70°C, so that the negative electrode premixed mixture with the conductive agent coated on the surface continues to react in the reactor to obtain the negative electrode material; wherein, during fiberization, the dispersion disk of the reactor rotates at 3000~5000 rpm, and the inner cylinder wall of the reactor rotates at 10~50 rpm.
[0030] Since the binder in the negative electrode material is generally in the initial state of granules, it can only bond point-to-point, resulting in poor bonding effect. After fiberization, the granular binder will form long fibrous strips. The fiberized binders are connected to each other to form a network structure, which makes the binder not only sticky, but also able to constrain the volume expansion of the negative electrode active material during the charging and discharging process, effectively improving the cycle performance of the negative electrode material.
[0031] Preferably, the rolling of the positive electrode material includes: pressing the positive electrode material into the positive electrode sheet by rolling at a temperature of 80~180℃.
[0032] Preferably, the positive electrode active material is selected from at least one of ternary positive electrode materials, lithium iron phosphate, lithium cobalt oxide, lithium manganese oxide, elemental sulfur, and lithium sulfide.
[0033] Preferably, the negative electrode active material is selected from at least one of graphite, silicon carbide, silicon, and silicon oxide.
[0034] Preferably, the solid electrolyte is selected from at least one of polymer electrolytes, oxide electrolytes, and sulfide electrolytes.
[0035] Preferably, the polymer electrolyte comprises at least one of polyethylene oxide (PEO), polyvinylidene fluoride (PVDF), and polyether carbonate (PEC).
[0036] Preferably, the oxide electrolyte includes perovskite oxides and / or garnet oxides.
[0037] Preferably, the sulfide electrolyte includes at least one of glassy sulfides, crystalline sulfides, and ceramic sulfides.
[0038] Preferably, the conductive agent is selected from at least one of conductive carbon black, carbon nanotubes, carbon nanofibers, and graphene.
[0039] Preferably, the adhesive is selected from polytetrafluoroethylene (PTFE) and / or polyvinylidene fluoride (PVDF).
[0040] The present invention also provides a composite electrode sheet for a battery, wherein the composite electrode sheet is manufactured using the preparation process described in the present invention.
[0041] The present invention also provides a solid-state battery, wherein the composite electrode sheet of the solid-state battery is fabricated using the preparation process described in the present invention.
[0042] The beneficial effects of this invention are: The composite electrode sheet fabrication process of the battery of the present invention involves simultaneously pressing a solid electrolyte, a positive electrode sheet, and a positive current collector into shape. This not only effectively promotes the fusion of the solid electrolyte and the positive electrode sheet interface during the pressing process, but also allows some solid electrolyte to infiltrate into the positive electrode material, thereby increasing the tightness of the connection between the electrolyte layer and the positive electrode material, reducing interfacial impedance, and improving conductivity. It also effectively simplifies the pressing process and improves the manufacturing efficiency of the battery cell. Simultaneously, a filling method is used to fill the grooves of the positive electrode composite sheet with negative electrode material, extending the negative electrode material beyond the edge of the groove, before pressing. This results in a concave-convex interlocking structure between the negative electrode material and the positive electrode composite sheet, effectively increasing the contact area between the negative electrode material layer and the positive electrode composite sheet. This increases the lithium-ion transport area, improves the electronic and ionic conductivity at the battery electrode interface, further reduces interfacial impedance, and the concave-convex interlocking structure effectively overcomes the hazards of positive electrode material peeling off from the positive current collector and negative electrode material peeling off from the negative current collector, mitigating electrode volume changes during charging and discharging and the problem of expansion, detachment, and material loss. Therefore, the concave-convex embedded battery electrode structure not only effectively enhances the contact tightness between the positive electrode material layer, the solid electrolyte layer, and the negative electrode material layer, and reduces the interface impedance, but also effectively overcomes the problem of battery electrode expansion and detachment during charging and discharging of ordinary solid-state batteries. This improves the overall cycle performance, rate performance, and safety of the battery, and effectively solves the defects of existing all-solid-state batteries, such as high electrode interface impedance and the detachment of the positive electrode material layer, electrolyte layer, and negative electrode layer caused by electrode volume expansion during charging and discharging, resulting in short cycle life and poor rate performance of solid-state batteries. It has promotion and application value in the field of battery manufacturing technology. Attached Figure Description
[0043] Figure 1 This is a process flow diagram of the fabrication process of the composite electrode sheet of the battery of the present invention; Figure 2 A schematic diagram of the protrusion structure on the outer side wall of the first upper roller; Figure 3 This is a schematic diagram of the positive electrode composite sheet; Figure 4 This is a schematic diagram of the composite electrode sheet. Figure 5 This is a schematic diagram of the stress analysis structure of the composite electrode sheet during the charging and discharging process; Among them, 1-positive electrode feeding port; 2-positive electrode reactor; 3-negative electrode feeding port; 4-negative electrode reactor; 5-solid electrode film forming equipment; 6-roller shaft; 7-positive electrode sheet; 8-solid electrolyte feeding port; 9-positive electrode current collector (aluminum foil); 10-positive electrode current collector unwinding shaft; 11-first upper roller shaft; 111-protruding structure; 12-first lower roller shaft; 13-positive electrode composite sheet; 131-solid electrolyte layer; 132-positive electrode material layer; 133-solid electrolyte; 14-negative electrode material feeding port; 15-negative current collector unwinding shaft; 16-negative electrode current collector (copper foil); 17-second lower roller shaft; 18-second upper roller shaft; 19-composite electrode sheet; 191-negative electrode material layer. Detailed Implementation
[0044] The embodiments of the present invention will be described below with reference to the accompanying drawings and preferred embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and various details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention. It should be understood that the preferred embodiments are only for illustrating the present invention and not for limiting the scope of protection of the present invention.
[0045] It should be noted that the illustrations provided in the following embodiments are only schematic representations of the basic concept of the present invention. Therefore, the drawings only show the components related to the present invention and are not drawn according to the actual number, shape and size of the components in the actual implementation. In the actual implementation, the form, quantity and proportion of each component can be arbitrarily changed, and the layout of the components may also be more complex.
[0046] Numerous details are explored in the following description to provide a more thorough explanation of embodiments of this application; however, it will be apparent to those skilled in the art that embodiments of this application may be implemented without these specific details.
[0047] This invention aims to disclose a composite electrode sheet, a manufacturing process, and a solid-state battery, in order to effectively solve the problem of high interfacial impedance of the electrode sheet in existing all-solid-state batteries. It can also solve the problem of short cycle life and poor rate performance of solid-state batteries caused by the volume expansion of the electrode sheet during charging and discharging, which leads to the shedding of the positive electrode material layer, electrolyte layer, and negative electrode layer.
[0048] One method for preparing a composite electrode sheet for a battery includes the following steps: S1. Spread a solid electrolyte on the upper surface of the positive electrode sheet, set a positive current collector on the lower surface of the positive electrode sheet, and then press it into a positive electrode composite sheet with an uneven structure. S2. Fill the groove of the positive electrode composite sheet with negative electrode material, and make the negative electrode material extend beyond the edge of the groove. Place the negative electrode current collector on the negative electrode material, and then press it into a composite electrode sheet for the battery.
[0049] By simultaneously pressing the solid electrolyte, positive electrode sheet, and positive current collector, the fusion of the solid electrolyte and positive electrode sheet interface is effectively promoted during the pressing process. Additionally, some solid electrolyte infiltrates the positive electrode material, increasing the tightness of the connection between the electrolyte layer and the positive electrode material, reducing interfacial impedance, and improving conductivity. This also simplifies the pressing process and improves the cell manufacturing efficiency. Simultaneously, by filling the grooves of the positive electrode composite sheet with negative electrode material extending beyond the edge of the groove before pressing, a concave-convex interlocking structure is created between the negative electrode material and the positive electrode composite sheet. This effectively increases the contact area between the negative electrode material layer and the positive electrode composite sheet, thereby increasing the lithium-ion transport area and improving the electronic and ionic conductivity at the battery electrode interface. This further reduces interfacial impedance. Furthermore, the concave-convex interlocking structure effectively overcomes the hazards of positive electrode material peeling off from the positive current collector and negative electrode material peeling off from the negative current collector, mitigating electrode volume changes during charging and discharging and reducing the problem of expansion, detachment, and material loss. Therefore, the concave-convex embedded battery electrode structure not only effectively enhances the contact tightness between the positive electrode material layer, the solid electrolyte layer and the negative electrode material layer and reduces the interface resistance, but also effectively overcomes the problem of battery electrode expansion and detachment during the charging and discharging process of ordinary solid battery electrodes, thereby improving the overall cycle performance, rate performance and safety of the battery.
[0050] In some embodiments, the negative electrode material can be filled into the grooves of the positive electrode composite sheet by electrostatic deposition, magnetron sputtering, blade coating, and extrusion coating.
[0051] In some embodiments, to ensure tight contact between the positive electrode, solid electrolyte, and negative electrode, and to further reduce interfacial impedance, the uneven structure of the positive electrode composite is designed with a smooth transition. This can also be understood as designing the uneven structure of the positive electrode composite with rounded corners. A smoothly transitioning positive electrode composite reduces current obstruction and loss in the uneven structure during battery operation, improving current transmission efficiency. Simultaneously, a smooth transition helps avoid stress concentration during battery charging and discharging, thereby reducing damage to the internal battery structure and performance degradation, ultimately ensuring the stability of the battery's cycle performance, rate performance, and lifespan.
[0052] The radius of the rounded corner transition can be adjusted according to actual needs.
[0053] In some embodiments, since excessive groove depth can damage the solid electrolyte layer, while insufficient groove depth can result in insignificant effects, the groove depth of the positive electrode composite sheet is controlled between 5 and 30 μm. This can also be understood as the height of the protrusions on the positive electrode composite sheet being between 5 and 30 μm.
[0054] In some embodiments, the protrusion or groove shape of the positive electrode composite sheet can be rectangular, cylindrical, etc.
[0055] In some embodiments, to avoid tearing or porosity problems during subsequent embossing, the spreading thickness of the solid electrolyte is controlled between 15µm and 50µm.
[0056] In some embodiments, the height of the negative electrode material extending beyond the edge of the groove is 140µm to 200µm.
[0057] In some embodiments, in order to increase the contact area between the positive electrode and the solid electrolyte and reduce the interfacial impedance, in S1, a positive electrode composite sheet with a concave-convex structure is formed by roll pressing. At the same time, in order to keep the solid electrolyte in a molten state so that some electrolyte can be immersed in the positive electrode material when the solid electrolyte is combined with the positive electrode, the roll pressing temperature for forming the positive electrode composite sheet is controlled at 80~180°C. Within this temperature range, the solid electrolyte can be in a molten state and no other side reactions will occur. When the molten solid electrolyte is combined with the positive electrode, some electrolyte is immersed in the positive electrode material, which can further increase the tight connection strength between the electrolyte layer and the positive electrode active material, reduce the interfacial impedance, and the solid electrolyte and the positive electrode simultaneously complete the concave-convex composite, which effectively simplifies the roll pressing process and improves the cell manufacturing efficiency.
[0058] In some embodiments, in S2, the composite electrode sheet of the battery is pressed by a rolling method, and the rolling temperature of the composite electrode sheet of the battery is 80~180°C.
[0059] In some embodiments, since the positive electrode active material itself has poor ionic conductivity and no adhesive properties, in order to improve the ionic conductivity and adhesive properties of the positive electrode active material, thereby laying a solid foundation for subsequent process steps and ensuring the smooth progress of the entire production process and the stable improvement of product quality, it is necessary to premix the positive electrode material first. The premixing operation of the positive electrode material includes: mixing the positive electrode active material, conductive agent and adhesive in a reactor at a temperature of 5℃~15℃ to obtain a positive electrode premixed mixture; wherein, during premixing, the dispersion disk of the reactor rotates at a speed of 100~200 rpm, and the inner cylinder wall of the reactor rotates at a speed of 10~50 rpm.
[0060] In some embodiments, since the negative electrode active material itself has poor ionic conductivity and no adhesive properties, in order to improve the ionic conductivity and adhesive properties of the negative electrode active material, thereby laying a solid foundation for subsequent process steps and ensuring the smooth progress of the entire production process and the stable improvement of product quality, it is necessary to premix the negative electrode material first. The premixing operation of the negative electrode material includes: mixing the negative electrode active material, conductive agent and adhesive in a reactor at a temperature of 5℃~15℃ to obtain a negative electrode premixed mixture; wherein, during premixing, the dispersion disc of the reactor rotates at a speed of 100~200 rpm, and the inner cylinder wall of the reactor rotates at a speed of 10~50 rpm.
[0061] In some embodiments, to increase the electronic conductivity of the positive electrode material, a material with a high specific surface area is coated onto the surface of the positive electrode premix. Specifically, the coating operation involves raising the temperature to 18°C~25°C and further mixing the positive electrode premix in a reactor to obtain a positive electrode premix coated with a conductive agent. During coating, the dispersion disc in the reactor rotates at 1000~2500 rpm, and the inner cylinder wall rotates at 20~45 rpm. By adjusting the temperature and reactor rotation speed, a conductive agent can be coated onto the surface of the positive electrode premix, and the volume stress of the positive electrode material during charging and discharging can be constrained to a certain extent.
[0062] In some embodiments, to increase the electronic conductivity of the negative electrode material, a material with a high specific surface area is coated onto the surface of the negative electrode premix. Specifically, the coating process involves raising the temperature to 18°C–25°C and further mixing the negative electrode premix in a reactor to obtain a negative electrode premix coated with a conductive agent. During coating, the dispersion disc in the reactor rotates at 1000–2500 rpm, and the inner cylinder wall rotates at 10–50 rpm. By adjusting the temperature and reactor rotation speed, a conductive agent can be coated onto the surface of the negative electrode premix, and the volumetric stress of the negative electrode material during charging and discharging can be constrained to a certain extent.
[0063] In some embodiments, since the binder in the positive electrode material is generally in a particulate state initially, it can only bond point-to-point, resulting in poor bonding. Therefore, the positive electrode material is subjected to a fiberization process. The specific operation of the fiberization process is as follows: the temperature in the reactor is raised to 60°C~70°C, allowing the positive electrode premixed mixture coated with conductive agent to continue reacting in the reactor to obtain the positive electrode material. During fiberization, the dispersion disc in the reactor rotates at 3000~5000 rpm, and the inner cylinder wall of the reactor rotates at 10~50 rpm. After fiberization, the particulate binder forms long fibers, and the fiberized binders connect with each other to form a network structure. In this way, the binder has both adhesiveness and can restrain the volume expansion of the positive electrode active material during charge and discharge, thereby improving the cycle performance of the positive electrode material.
[0064] For example, the fiberization temperature of the cathode material can be selected from 60℃, 62℃, 64℃, 66℃, 68℃ and 70℃. Among them, the optimal fiberization temperature of the cathode material is 64℃.
[0065] The cathode material obtained after fibrosis is cathode material powder.
[0066] In some embodiments, since the binder in the negative electrode material is generally in a particulate state initially, it can only bond point-to-point, resulting in poor bonding. Therefore, the negative electrode material is subjected to a fiberization treatment. The specific operation of the fiberization treatment is as follows: the temperature in the reactor is raised to 60°C~70°C, allowing the negative electrode premixed mixture coated with conductive agent to continue reacting in the reactor to obtain the negative electrode material. During fiberization, the dispersion disc of the reactor rotates at 3000~5000 rpm, and the inner cylinder wall of the reactor rotates at 10~50 rpm. After fiberization, the particulate binder forms long fibers, and the fiberized binders connect with each other to form a network structure. In this way, the binder has both adhesiveness and can restrain the volume expansion of the negative electrode active material during charge and discharge, improving the cycle performance of the negative electrode material.
[0067] For example, the fiberization temperature of the negative electrode material can be selected from 60℃, 63℃, 65℃, 69℃ and 70℃. Among them, the optimal fiberization temperature of the negative electrode material is 60℃.
[0068] The negative electrode material obtained after fibrosis treatment is negative electrode material powder.
[0069] In some embodiments, the rolling of the positive electrode material includes: pressing the positive electrode material into a positive electrode sheet by rolling at a temperature of 80~180°C.
[0070] In some embodiments, the positive electrode active material is selected from at least one of ternary positive electrode materials, lithium iron phosphate, lithium cobalt oxide, lithium manganese oxide, elemental sulfur, and lithium sulfide.
[0071] In some embodiments, the negative electrode active material is selected from at least one of graphite, silicon carbide, silicon, and silicon oxide.
[0072] In some embodiments, the solid electrolyte is selected from at least one of polymer electrolytes, oxide electrolytes, and sulfide electrolytes.
[0073] For example, the polymer electrolyte includes at least one of polyethylene oxide (PEO), polyvinylidene fluoride (PVDF), and polyether carbonate (PEC); the oxide electrolyte includes perovskite oxides and / or garnet oxides; and the sulfide electrolyte includes at least one of glassy sulfides, crystalline sulfides, and ceramic sulfides.
[0074] In some embodiments, the conductive agent is selected from at least one of conductive carbon black, carbon nanotubes, carbon nanofibers, and graphene.
[0075] In some embodiments, the adhesive is selected from polytetrafluoroethylene (PTFE) and / or polyvinylidene fluoride (PVDF).
[0076] In some embodiments, a composite electrode sheet for a battery is also provided, which is manufactured using any of the above-described preparation processes.
[0077] In some embodiments, a solid-state battery is also provided, wherein the composite electrode sheet of the solid-state battery is fabricated using any of the above-described fabrication processes.
[0078] To make the technical problems, technical solutions, and beneficial effects solved by this application clearer, the following will provide a more detailed description in conjunction with specific embodiments and accompanying drawings. Obviously, the specific embodiments described are merely some embodiments of this application, and not all embodiments. The following description of at least one exemplary embodiment is merely illustrative and is in no way intended to limit this application or its applications. Based on the specific embodiments in this application, all other embodiments obtained by those skilled in the art without inventive effort are within the scope of protection of this application.
[0079] Where specific techniques or conditions are not specified in the detailed embodiments, they shall be performed in accordance with the techniques or conditions described in the literature in this field or in accordance with the product instructions. Reagents or instruments whose manufacturers are not specified are all commercially available conventional products.
[0080] Example 1 like Figure 1 As shown, a process for fabricating a composite electrode sheet for a battery includes the following steps: S1, Premixed: Premixing of cathode materials: Lithium iron phosphate, polytetrafluoroethylene (PTFE), and conductive carbon black are weighed in a mass percentage ratio of 80:10:10 and added into cathode reactor 2 through cathode feed port 1. The mixture is then mixed in cathode reactor 2 for 1 to 3 minutes at a temperature of 8℃~12℃. The rotation speed of the dispersion disc in cathode reactor 2 is between 100 and 200 rpm, and the rotation speed of the inner cylinder wall in cathode reactor 2 is 40 rpm. A uniformly mixed cathode premixed mixture is obtained. Premixing of negative electrode materials: The negative electrode active material (graphite), polytetrafluoroethylene (PTFE) and conductive carbon black are weighed according to a mass fraction of 92:4:2 and fed into the negative electrode reactor 4 through the negative electrode feeding port 3. The mixture is then mixed in the negative electrode reactor 4 for 1 to 3 minutes at a temperature of 8℃~12℃ to obtain a negative electrode premixed mixture. During premixing, the speed of the dispersion disc in the negative electrode reactor 4 is between 100 and 200 rpm, and the speed of the inner cylinder wall of the negative electrode reactor 4 is 40 rpm. S2, Covering: Coating of positive electrode material: The temperature is raised to 18℃~25℃, and the mixture is further mixed in positive electrode reactor 2 for 5~10 minutes to obtain a positive electrode premixed mixture with conductive carbon black coated on the surface; wherein, during coating, the speed of the dispersion disk in positive electrode reactor 2 is between 1000~2500 rpm, and the speed of the inner cylinder wall of positive electrode reactor 2 is 20~45 rpm; Coating of negative electrode material: The temperature is raised to 18℃~25℃, and the mixture is further mixed for 5~10 minutes in negative electrode reactor 4 to obtain a negative electrode premixed mixture with conductive carbon black on the surface; wherein, during coating, the speed of the dispersion disk in negative electrode reactor 4 is between 1000~2500 rpm, and the speed of the inner cylinder wall of negative electrode reactor 4 is 10~50 rpm. S3, fibrosis: Fiberization of cathode material: The temperature of cathode reactor 2 containing cathode premixed mixture with conductive carbon black surface is raised to 60℃~70℃, so that cathode premixed mixture with conductive carbon black surface continues to react in cathode reactor 2 for 40~50min to obtain cathode material powder; wherein, during fiberization, the dispersion disk of cathode reactor 2 rotates at 4500rpm, and the inner cylinder wall of cathode reactor 2 rotates at 45rpm; Fiberization of negative electrode material: The temperature of negative electrode reactor 4, which contains a negative electrode premixed mixture with a surface coated with conductive carbon black, is raised to 60℃~70℃, so that the negative electrode premixed mixture with a surface coated with conductive carbon black continues to react in negative electrode reactor 4 for 40~50 minutes to obtain negative electrode material powder; wherein, during fiberization, the dispersion disk of negative electrode reactor 4 rotates at 4500 rpm, and the inner cylinder wall of negative electrode reactor 4 rotates at 45 rpm; S4. Positive electrode sheet rolling: The positive electrode material powder obtained in S3 is transferred to the solid electrode film forming equipment 5 and rolled into positive electrode sheet 7 by rollers 6. The number of rollers 6 in the solid electrode film forming equipment 5 can be adjusted according to actual needs. Each roller 6 can independently adjust the rolling gap. The rolling temperature is about 100℃. S5. Positive electrode composite sheet rolling: Polyethylene oxide (PEO) solid electrolyte is spread onto the upper surface of the positive electrode sheet 7 through the solid electrolyte feeding port 8, with a spreading thickness of 40 μm. Simultaneously, the positive electrode current collector (aluminum foil) 9 is introduced into the lower surface of the positive electrode sheet 7 through the positive electrode current collector unwinding shaft 10, so that the polyethylene oxide (PEO) solid electrolyte, the positive electrode sheet 7, and the positive electrode current collector (aluminum foil) 9 are located between the first upper roller shaft 11 and the first lower roller shaft 12, and then rolled to form the positive electrode composite sheet 13; wherein, as shown... Figure 2 As shown, the outer side wall of the first upper roller 11 has a protruding structure 111, which makes the solid electrolyte side of the positive electrode composite sheet 13 formed by roller pressing have a concave-convex structure. The height of the protruding structure is 5~30um, and the roller pressing temperature is 100℃. A schematic diagram of the positive electrode composite sheet 13 with an uneven structure is shown below. Figure 3 As shown, the solid electrolyte layer 131 and the positive electrode material layer 132 of the positive electrode composite sheet 13 together form a concave-convex composite structure, and some polyethylene oxide (PEO) solid electrolyte 133 penetrates into the positive electrode sheet 7. S6. Rolling of composite electrode sheet: Using the positive electrode composite sheet 13 with concave and convex structure as a carrier, the negative electrode material powder obtained in S3 is deposited on the solid electrolyte layer 131 of the positive electrode composite sheet 13 through the negative electrode material feeding port 14 by electrostatic deposition, so that the negative electrode material powder completely fills the groove of the positive electrode composite sheet 13 and extends about 140um beyond the edge of the groove. At the same time, the negative electrode current collector (copper foil) 16 is introduced onto the negative electrode material powder through the negative current collector unwinding shaft 15, so that the positive electrode composite sheet 13, the negative electrode material powder and the negative electrode current collector (copper foil) 16 are located between the second lower roller shaft 17 and the second upper roller shaft 18, and then rolled to form the composite electrode sheet 19 of the battery.
[0081] A schematic diagram of the composite electrode sheet 19 of the fabricated battery is shown below. Figure 4 As shown, the negative electrode material layer 191 and the positive electrode composite sheet 13 form a concave-convex mosaic structure, which can increase the contact area between the negative electrode material layer 191 and the positive electrode composite sheet 13.
[0082] When this composite electrode sheet is used to manufacture batteries, it can effectively increase the electronic conductivity and ionic conductivity at the battery electrode interface. Simultaneously, as... Figure 5As shown, during battery charging and discharging, when the electrode expands, a force F1 is generated on the electrode surface located at the concave-convex area, moving away from the foil and perpendicular to the electrode. This is the electrode front peeling force F1. Simultaneously, due to material expansion, a force F2 parallel to the electrode is generated on the side of the protruding position, i.e., the side force F2. The presence of force F2 prevents the electrode from expanding away from the foil force F1, thereby increasing the frictional force between the positive electrode and the negative electrode during the re-expansion process. This overcomes the harm of positive electrode material peeling off the positive current collector, effectively mitigating the electrode volume change during battery charging and discharging, and the problem of electrode expansion and material shedding. Therefore, the concave-convex interlocking structure of the composite electrode sheet further enhances the contact tightness between the positive electrode material layer, the solid electrolyte layer, and the negative electrode material layer, overcoming the defect of battery electrode detachment during long-term charging and discharging of ordinary solid-state battery electrodes, and improving the overall cycle performance and safety of the battery.
[0083] In summary, through multiple experiments, it has been found that the composite electrode sheet preparation process of the battery of the present invention, by simultaneously pressing the solid electrolyte, positive electrode sheet, and positive current collector, not only effectively promotes the fusion of the solid electrolyte and positive electrode sheet interface during the pressing process, but also allows some solid electrolyte to penetrate into the positive electrode material, thereby increasing the tight connection strength between the electrolyte layer and the positive electrode material, reducing interface impedance, and improving conductivity. It also effectively simplifies the pressing process and improves the manufacturing efficiency of the battery cell. Simultaneously, by using a filling method to fill the grooves of the positive electrode composite sheet with negative electrode material, extending the negative electrode material beyond the edge of the groove, and then pressing it, the negative electrode material and the positive electrode composite sheet form a concave-convex interlocking structure. This effectively increases the contact area between the negative electrode material layer and the positive electrode composite sheet, thereby increasing the lithium-ion transport area, improving the electronic and ionic conductivity at the battery electrode interface, reducing interface impedance, and effectively overcoming the hazards of positive electrode material peeling off the positive current collector and negative electrode material peeling off the negative current collector. This alleviates the problems of electrode volume changes and expansion / material shedding during battery charging and discharging. Therefore, the concave-convex embedded battery electrode structure effectively enhances the contact tightness between the positive electrode material layer, the solid electrolyte, and the negative electrode material layer, overcoming the problem of electrode detachment during long-term charge and discharge of ordinary solid-state batteries. This improves the overall cycle performance and safety of the battery and effectively solves the defects of existing all-solid-state batteries, such as high electrode interface impedance and electrode volume expansion during charge and discharge causing the positive electrode material layer, electrolyte layer, and negative electrode layer to detach, resulting in short cycle life and poor rate performance. It has application value in the field of battery manufacturing technology.
[0084] The above embodiments are merely illustrative of the principles and effects of the present invention and are not intended to limit this application. Any person skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of this application. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in this application should still be covered by the claims of this application.
Claims
1. A process for preparing a composite electrode sheet for a battery, characterized in that, Includes the following steps: S1. A solid electrolyte is spread on the upper surface of the positive electrode sheet, and a positive current collector is set on the lower surface of the positive electrode sheet. The positive electrode composite sheet with a concave-convex structure is formed by rolling. The rolling temperature for forming the positive electrode composite sheet is 80~180℃. The first upper roller shaft with a raised structure on the outer side wall and the first lower roller shaft are used for one rolling forming. The rolling temperature makes the solid electrolyte molten and part of the solid electrolyte is immersed in the positive electrode material. S2. The negative electrode material is deposited on the solid electrolyte layer of the positive electrode composite sheet by electrostatic deposition, so that the negative electrode material completely fills the groove of the positive electrode composite sheet and the negative electrode material powder extends beyond the edge of the groove. The height of the negative electrode material extending beyond the edge of the groove is 140um~200um. A negative electrode current collector is set on the negative electrode material, and then the composite electrode sheet of the battery is pressed by rolling. The rolling temperature of the composite electrode sheet of the battery is 80~180℃.
2. The fabrication process of the composite electrode sheet for the battery according to claim 1, characterized in that, The uneven structure of the positive electrode composite sheet has a smooth transition.
3. The fabrication process of the composite electrode sheet for the battery according to claim 1, characterized in that, The depth of the groove in the positive electrode composite sheet is between 5 and 30 μm; And / or, the spread thickness of the solid electrolyte is between 15 μm and 50 μm.
4. The fabrication process of the composite electrode sheet for the battery according to claim 1, characterized in that, Before S1, it also includes: premixing, coating, fiberization and rolling of positive electrode materials, and premixing, coating and fiberization of negative electrode materials; The premixing of the positive electrode material includes: mixing the positive electrode active material, conductive agent and binder in a reactor at a temperature of 5℃~15℃ to obtain a positive electrode premixed mixture; wherein, during premixing, the rotation speed of the dispersion disc in the reactor is between 100~200 rpm, and the rotation speed of the inner cylinder wall of the reactor is between 10~50 rpm. The premixing of the negative electrode material includes: mixing the negative electrode active material, conductive agent and binder in a reactor at a temperature of 5℃~15℃ to obtain a negative electrode premixed mixture; wherein, during premixing, the rotation speed of the dispersion disc in the reactor is between 100~200 rpm, and the rotation speed of the inner cylinder wall of the reactor is between 10~50 rpm.
5. The fabrication process of the composite electrode sheet for the battery according to claim 4, characterized in that, The coating of the positive electrode material includes: raising the temperature to 18℃~25℃, mixing the positive electrode premixed mixture in a reactor to obtain a positive electrode premixed mixture with a conductive agent coated on the surface; wherein, during coating, the rotation speed of the dispersion disk in the reactor is between 1000~2500 rpm, and the rotation speed of the inner cylinder wall of the reactor is between 20~45 rpm. And / or, the coating of the negative electrode material includes: raising the temperature to 18°C~25°C, mixing the negative electrode premixed mixture in a reactor to obtain a negative electrode premixed mixture with a conductive agent coated on the surface; wherein, during coating, the rotation speed of the dispersion disk in the reactor is between 1000~2500 rpm, and the rotation speed of the inner wall of the reactor is between 10~50 rpm.
6. The fabrication process of the composite electrode sheet for the battery according to claim 5, characterized in that, The fiberization of the positive electrode material includes: raising the temperature to 60°C~70°C, so that the positive electrode premixed mixture with the conductive agent coated on the surface continues to react in the reactor to obtain the positive electrode material; wherein, during fiberization, the dispersion disk of the reactor rotates at 3000~5000 rpm, and the inner cylinder wall of the reactor rotates at 10~50 rpm. And / or, the fiberization of the negative electrode material includes: raising the temperature to 60°C~70°C, so that the negative electrode premixed mixture with the conductive agent coated on the surface continues to react in the reactor to obtain the negative electrode material; wherein, during fiberization, the rotation speed of the dispersion disk in the reactor is 3000~5000 rpm, and the rotation speed of the inner cylinder wall of the reactor is 10~50 rpm. And / or, the rolling of the positive electrode material includes: pressing the positive electrode material into the positive electrode sheet by rolling at a temperature of 80~180℃.
7. The fabrication process of the composite electrode sheet for the battery according to claim 5, characterized in that, The positive electrode active material is selected from at least one of ternary positive electrode materials, lithium iron phosphate, lithium cobalt oxide, lithium manganese oxide, elemental sulfur, and lithium sulfide. And / or, the negative electrode active material is selected from at least one of graphite, silicon carbide, silicon, and silicon oxide; And / or, the solid electrolyte is selected from at least one of polymer electrolytes, oxide electrolytes, and sulfide electrolytes; And / or, the conductive agent is selected from at least one of conductive carbon black, carbon nanotubes, carbon nanofibers and graphene; And / or, the adhesive is selected from polytetrafluoroethylene and / or polyvinylidene fluoride.
8. A composite electrode sheet for a battery, characterized in that, It is prepared using the preparation process described in any one of claims 1 to 7.
9. A solid-state battery, characterized in that, The composite electrode sheet of the solid-state battery is manufactured using the preparation process described in any one of claims 1 to 7.
Citation Information
Patent Citations
Method for producing all solid state battery, and all solid battery
CN110265707A
All-solid-state battery with low interface impedance and high interface compatibility
CN111092254A
Method for preparing electrode membrane of lithium ion battery by dry method
CN115579458A
Multi-layer all-solid-state battery coating
CN117638236A
Lithium ion secondary battery manufacturing method
JP2013229315A