A high-strength crack-resistant concrete and its preparation method
By using phosphogypsum coarse aggregate and phosphogypsum gel material to replace traditional materials, combined with reinforcing fibers, the problems of uneven strength and easy cracking of phosphogypsum concrete were solved, achieving improved high strength and crack resistance.
Patent Information
- Application Number
- CN202410029848.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-09
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-01-09
AI Technical Summary
Phosphogypsum contains impurities such as phosphorus and fluorine in concrete, which leads to uneven local strength and easy cracking, a problem that is difficult to solve effectively with existing technologies.
High-strength, crack-resistant concrete was prepared by replacing basalt aggregate with phosphogypsum coarse aggregate and using phosphogypsum gel material and cement as gel material, combined with reinforcing fibers, and by controlling the calcination temperature and particle size to improve the bonding strength and uniformity.
It improves the compressive strength and splitting tensile strength of concrete, reduces the total crack area per unit area, and improves the overall performance of phosphogypsum concrete.
Smart Images

Figure BDA0004655723530000041 
Figure BDA0004655723530000051 
Figure BDA0004655723530000061
Abstract
Description
Technical Field
[0001] This application relates to the field of concrete, and in particular to a high-strength crack-resistant concrete and a method for preparing the same. Background Technology
[0002] Concrete is a composite material made by mixing coarse aggregate, fine aggregate and water with cement as a gelling material, and it is widely used in engineering construction.
[0003] Currently, phosphogypsum is a solid waste material with a large stockpile. To utilize phosphogypsum, it can be used as building gypsum, cement retarder, gypsum bricks, etc. There are also proposals to use phosphogypsum to replace part of the gel in the preparation of concrete, so that phosphogypsum can be recycled.
[0004] However, because phosphogypsum contains impurities such as phosphorus and fluorine, it hinders the dissolution and hydration of phosphogypsum during concrete preparation, reduces the local strength of concrete, and leads to uneven overall strength of concrete, making it prone to cracking. Summary of the Invention
[0005] To address the problem of uneven strength distribution in concrete leading to cracking, this application provides a high-strength, crack-resistant concrete and its preparation method.
[0006] On the one hand, the high-strength crack-resistant concrete provided in this application adopts the following technical solution: A high-strength, crack-resistant concrete is prepared from the following components in parts by weight: 50-70 parts of phosphogypsum coarse aggregate; 1-5 parts of phosphogypsum gel material; 7.5-12 parts cement; 3-5 parts water; Fine aggregate 25-40; Water-reducing agent 0.4-1 part; 0.5-1.5 parts of reinforcing fiber; The phosphogypsum coarse aggregate was prepared by the following method: Phosphogypsum, magnesium oxide, silicon oxide, clay and water are mixed, granulated, dried and sieved to obtain pretreated granules. The pretreated granules are then calcined and carbonized to obtain phosphogypsum coarse aggregate.
[0007] By adopting the above technical solution, using phosphogypsum coarse aggregate to replace commonly used basalt aggregate, and using phosphogypsum gel material and cement as a gel material to bond the phosphogypsum coarse aggregate, reinforcing fibers, and fine aggregate, the proportion of reusable phosphogypsum is increased, and the bonding strength between coarse aggregate and gel material is improved. This results in increased compressive strength and splitting tensile strength of the high-strength crack-resistant concrete, while reducing the total crack area per unit area, thus improving the problem of easy cracking in concrete using phosphogypsum.
[0008] Optionally, the calcination temperature during the preparation of the phosphogypsum coarse aggregate is 1100-1500℃.
[0009] Preferably, the calcination temperature during the preparation of the phosphogypsum coarse aggregate is 1200-1300℃.
[0010] By adopting the above technical solution, the pretreated particles are calcined at a temperature of not less than 1200℃ during the preparation of phosphogypsum coarse aggregate, thereby removing impurities from the phosphogypsum in the pretreated particles, which is beneficial to improving the strength of the phosphogypsum coarse aggregate.
[0011] Optionally, the particle size of the pretreated particles is 10-20 mm.
[0012] Preferably, the pretreated particles have a particle size of 13-16 mm.
[0013] By adopting the above technical solution, in the process of preparing phosphogypsum coarse aggregate, under the condition that the composition is basically similar, the loss on ignition during calcination is relatively fixed. Therefore, by controlling the particle size of the pretreated particles, the particle size of the obtained phosphogypsum coarse aggregate can be controlled. Compared with sieving to control the particle size of phosphogypsum coarse aggregate, the production process is simplified and the utilization rate of raw materials is improved.
[0014] Optionally, the phosphogypsum gel material is prepared by the following method: phosphogypsum, limestone powder, silicate cement and water are added to a ball mill and ball-milled, then dried in an inert gas environment and ground to obtain the phosphogypsum gel material.
[0015] Preferably, in the preparation process of the phosphogypsum gel material, the weight ratio of phosphogypsum, limestone powder, silicate cement and water is (40-60):(1.6-4.8):(6.4-7.2):25.
[0016] By adopting the above technical solution, in the process of preparing phosphogypsum gel material, on the one hand, by controlling the ratio of phosphogypsum, limestone powder and silicate cement, harmful elements such as fluorine and phosphorus in phosphogypsum are fixed, reducing their hindering effect on the solidification of the high-strength crack-resistant concrete. On the other hand, the ball milling method combined with other particulate components not only helps to improve the particle morphology of phosphogypsum, but also improves the uniformity of mixing between various components.
[0017] Optionally, the weight ratio of the phosphogypsum gel material to the cement is 0.3-0.625:1.
[0018] By adopting the above technical solution and controlling the weight ratio of phosphogypsum gel material to cement, phosphogypsum is recycled on the one hand, and the bonding effect on other components is improved on the other hand.
[0019] Optionally, the reinforcing fiber includes one or more of steel fiber, polypropylene fiber, and glass fiber.
[0020] Preferably, the average length of the reinforcing fiber is 8-16 mm.
[0021] Preferably, the reinforcing fiber has an average length of 12 mm and a cross-sectional diameter of 0.2 mm.
[0022] By adopting the above technical solution and controlling the average length of the reinforcing fiber, the compatibility of the reinforcing fiber with other components is improved, and its average length is matched with the particle size of the phosphogypsum coarse aggregate, which further improves the compressive strength and splitting tensile strength of the high-strength crack-resistant concrete and reduces the total crack area per unit area.
[0023] On the other hand, this application also provides a method for preparing high-strength crack-resistant concrete, which adopts the following technical solution: A method for preparing high-strength crack-resistant concrete includes the following steps: High-strength, crack-resistant concrete is obtained by mixing reinforcing fibers, phosphogypsum gel material, cement, phosphogypsum coarse aggregate, fine aggregate, water, and water-reducing agent.
[0024] Preferably, the mixing includes the following steps: Reinforcing fibers, cement, phosphogypsum coarse aggregate and fine aggregate are mixed to obtain a solid mixture. Then, the uniformly mixed phosphogypsum gel material, water and water-reducing agent are added to the solid mixture and stirring is continued.
[0025] By adopting the above technical solution, the solid mixture is prepared by mixing reinforcing fibers, cement, phosphogypsum coarse aggregate and fine aggregate, which improves the uniformity of dispersion of the main solid components. The uniform mixing of phosphogypsum gel material, water and water-reducing agent improves the uniformity of mixing of the relatively small amount of phosphogypsum gel material with water and water-reducing agent, which facilitates the dispersion effect of phosphogypsum gel material in high-strength crack-resistant concrete. Under the combined effect, the crack resistance and compressive strength of concrete are improved.
[0026] In summary, this application includes at least one of the following beneficial technical effects: 1. By using phosphogypsum coarse aggregate to replace commonly used basalt aggregate, and using phosphogypsum gel material and cement as gel materials to bond phosphogypsum coarse aggregate, reinforcing fiber, and fine aggregate, the proportion of reusable phosphogypsum is increased, and the bond strength between coarse aggregate and gel material is improved. This results in increased compressive strength and splitting tensile strength of the high-strength crack-resistant concrete, and reduced total crack area per unit area. 2. In the process of preparing phosphogypsum gel material, on the one hand, by controlling the ratio of phosphogypsum, limestone powder and silicate cement, harmful elements such as fluorine and phosphorus in phosphogypsum are fixed, reducing their hindering effect on the solidification of the high-strength crack-resistant concrete. On the other hand, the ball milling method combined with other particulate components not only helps to improve the particle morphology of phosphogypsum, but also improves the uniformity of mixing between various components. 3. The preparation of a solid mixture by mixing reinforcing fibers, cement, phosphogypsum coarse aggregate and fine aggregate improves the uniformity of dispersion of the main solid components. The uniform mixing of phosphogypsum gel material, water and water-reducing agent improves the uniformity of mixing of the relatively small amount of phosphogypsum gel material with water and water-reducing agent, which facilitates the dispersion effect of phosphogypsum gel material in high-strength crack-resistant concrete. Under the combined effect, the crack resistance and compressive strength of concrete are improved. Detailed Implementation
[0027] The present application will be further described in detail below with reference to the embodiments. The following embodiments are for illustrative purposes only and should not be considered as limiting the scope of the invention. Unless otherwise specified, specific conditions in the following embodiments were performed under conventional conditions or conditions recommended by the manufacturer. Unless otherwise specified, the methods used are conventional methods known in the art, and the consumables and reagents used are commercially available. Unless otherwise stated, the technical and scientific terms used herein have the same meaning as those familiar to those skilled in the art. Furthermore, any methods or materials similar to or equivalent to those described herein may also be applied to the present invention.
[0028] All raw materials used in the examples are commercially available. The fine aggregate is river sand, the water-reducing agent is polycarboxylate superplasticizer, and the cement is ordinary Portland cement with a strength of 42.5.
[0029] Examples 1-11 Examples 1-11 provide a high-strength crack-resistant concrete and its preparation method, the composition and proportions of which are shown in Table 1.
[0030] The preparation method of phosphogypsum coarse aggregate in Examples 1-11 is as follows: Phosphogypsum, magnesium oxide, silicon dioxide, clay, and water were mixed evenly in a weight ratio of 40:13:27:11:9 and then added to a drum granulator for granulation, drying, and sieving to obtain pretreated particles with a particle size of 13-16 mm. The pretreated particles were then calcined at 1200℃ for 20 min, and then the temperature was raised to 1300℃ for another 1 h. After cooling, the particles were cured in a carbonization curing chamber at normal pressure, temperature of 25℃, relative humidity of 75%, and carbon dioxide concentration of 75% for 15 h to obtain phosphogypsum coarse aggregate.
[0031] The preparation methods of the phosphogypsum gel materials in Examples 1-11 are as follows: Phosphogypsum, limestone powder, silicate cement and water were added to a ball mill in a weight ratio of 50:3:7:25 and ball-milled for 20 minutes. Then the mixture was dried in a nitrogen atmosphere at 50°C and ground to obtain phosphogypsum gel material.
[0032] The preparation methods of high-strength crack-resistant concrete in Examples 1-11 are as follows: Reinforcing fibers, phosphogypsum gel material, cement, phosphogypsum coarse aggregate, fine aggregate, water and water-reducing agent are added to a concrete mixer and mixed evenly to obtain high-strength crack-resistant concrete.
[0033] In Examples 1-11, the reinforcing fiber is steel fiber with an average length of 12 mm and a cross-sectional diameter of 0.2 mm.
[0034] Table 1: Composition and mix proportions of high-strength crack-resistant concrete Example 12 Example 12 provides a high-strength crack-resistant concrete and its preparation method. The difference between Example 12 and Example 8 is that the particle size of the pretreated particles in Example 12 when preparing phosphogypsum coarse aggregate is 10-12 mm.
[0035] Example 13 Example 13 provides a high-strength crack-resistant concrete and its preparation method. The difference between Example 13 and Example 8 is that the particle size of the pretreated particles in Example 13 when preparing phosphogypsum coarse aggregate is 17-20 mm.
[0036] Example 14 Example 14 provides a high-strength crack-resistant concrete and its preparation method. The difference between Example 14 and Example 8 is that when preparing the phosphogypsum gel material in Example 14, the weight ratio of phosphogypsum, limestone powder, silicate cement and water is 40:1.6:6.4:25.
[0037] Example 15 Example 15 provides a high-strength crack-resistant concrete and its preparation method. The difference between Example 15 and Example 8 is that when preparing the phosphogypsum gel material in Example 15, the weight ratio of phosphogypsum, limestone powder, silicate cement and water is 60:4.8:7.2:25.
[0038] Example 16 Example 16 provides a high-strength crack-resistant concrete and its preparation method. The difference between Example 16 and Example 8 is that the average length of the steel fiber in Example 16 is 8 mm and the cross-sectional diameter is 0.2 mm.
[0039] Example 17 Example 17 provides a high-strength crack-resistant concrete and its preparation method. The difference between Example 17 and Example 8 is that the average length of the steel fiber in Example 17 is 16 mm and the cross-sectional diameter is 0.2 mm.
[0040] Example 18 Example 18 provides a high-strength crack-resistant concrete and its preparation method. The difference between Example 18 and Example 8 is that the preparation method of the high-strength crack-resistant concrete in Example 18 is as follows: Reinforcing fibers, cement, phosphogypsum coarse aggregate and fine aggregate are added to a concrete mixer and mixed evenly to obtain a solid mixture. Then, phosphogypsum gel material, water and water-reducing agent are mixed evenly and added to the concrete mixer. The mixture is then stirred evenly to obtain high-strength crack-resistant concrete.
[0041] Comparative Example 1 Comparative Example 1 provides a high-strength crack-resistant concrete and its preparation method. The difference between Comparative Example 1 and Example 2 is that basalt aggregate with a particle size of 12-15 mm is used to replace phosphogypsum coarse aggregate in Comparative Example 1.
[0042] Comparative Example 2 Comparative Example 2 provides a high-strength crack-resistant concrete and its preparation method. The difference between Comparative Example 2 and Example 2 is that cement is used to replace phosphogypsum gel material in Comparative Example 2.
[0043] Comparative Example 3 Comparative Example 3 provides a high-strength crack-resistant concrete and its preparation method. The difference between Comparative Example 3 and Example 2 is that basalt aggregate with a particle size of 12-15mm is used to replace phosphogypsum coarse aggregate in Comparative Example 3, and cement is used to replace phosphogypsum gel material.
[0044] Testing and Inspection The high-strength crack-resistant concrete prepared according to Examples 1-18 and Comparative Examples 1-3 were subjected to the following tests: (1) Test the 28-day compressive strength (MPa) and 28-day splitting tensile strength (MPa) of high-strength crack-resistant concrete in accordance with GB / T 50081-2019.
[0045] (2) The total crack area per unit area (mm²) of high-strength crack-resistant concrete was tested according to GB / T 50082-2009. 2 / m 2 ).
[0046] The test data are shown in Table 2.
[0047] Table 2: Compressive strength, splitting tensile strength, and total crack area per unit area of high-strength crack-resistant concrete The following detailed description of this application is based on the experimental data provided in Table 1-2.
[0048] The high-strength permeable concrete obtained in Examples 1-3 achieved a 28-day compressive strength of over 37 MPa, a 28-day splitting tensile strength of over 2.6 MPa, and a total crack area per unit area of less than 18 mm. 2 / m 2 This demonstrates that the high-strength permeable concrete obtained from the construction of Examples 1-3 has good compressive strength and crack resistance.
[0049] Using Example 2 as a control, Examples 4-7 investigated the effects of the content of phosphogypsum coarse aggregate and phosphogypsum gel material on the compressive strength and crack resistance of the prepared high-strength crack-resistant concrete. The 28-day compressive strength and 28-day splitting tensile strength of the high-strength crack-resistant concrete prepared in Example 2 were greater than those prepared in Examples 4-7. The total crack area per unit area of the high-strength crack-resistant concrete prepared in Example 2 was smaller than that of the high-strength crack-resistant concrete prepared in Examples 4-7. This indicates that the content of phosphogypsum coarse aggregate and phosphogypsum gel material affects the compressive strength and crack resistance of the prepared high-strength crack-resistant concrete.
[0050] Using Example 2 as a control, Examples 8 and 9 investigated the effect of the ratio of phosphogypsum gel material to cement on the compressive strength and crack resistance of the prepared high-strength crack-resistant concrete. The 28-day compressive strength and 28-day splitting tensile strength of the high-strength crack-resistant concrete prepared in Example 8 were greater than those prepared in Examples 2 and 9. The total crack area per unit area of the high-strength crack-resistant concrete prepared in Example 8 was smaller than that of the high-strength crack-resistant concrete prepared in Examples 2 and 9. This indicates that when the weight ratio of phosphogypsum gel material to cement is 4:9, the prepared high-strength crack-resistant concrete exhibits high compressive strength and good crack resistance.
[0051] Using Example 8 as a control, Examples 10 and 11 investigated the effect of the amount of reinforcing fiber added on the compressive strength and crack resistance of the prepared high-strength crack-resistant concrete. The 28-day compressive strength and 28-day splitting tensile strength of the high-strength crack-resistant concrete prepared in Example 5 were greater than those of the high-strength crack-resistant concrete prepared in Examples 10 and 11. The total crack area per unit area of the high-strength crack-resistant concrete prepared in Example 8 was smaller than that of the high-strength crack-resistant concrete prepared in Examples 10 and 11. This indicates that the amount of reinforcing fiber added affects the compressive strength and crack resistance of the prepared high-strength crack-resistant concrete.
[0052] Using Example 8 as a control, Examples 12 and 13 investigated the effect of the particle size of the pretreated particles during the preparation of phosphogypsum coarse aggregate on the compressive strength and crack resistance of the resulting high-strength crack-resistant concrete. The 28-day compressive strength and 28-day splitting tensile strength of the high-strength crack-resistant concrete prepared in Example 8 were greater than those prepared in Examples 12 and 13. The total crack area per unit area of the high-strength crack-resistant concrete prepared in Example 8 was also smaller than that of the high-strength crack-resistant concrete prepared in Examples 12 and 13. This indicates that when the particle size of the pretreated particles during the preparation of phosphogypsum coarse aggregate is 13-16 mm, the resulting high-strength crack-resistant concrete exhibits high compressive strength and good crack resistance.
[0053] Using Example 8 as a control, Examples 14 and 15 investigated the effect of the weight ratio of phosphogypsum, limestone powder, silicate cement, and water on the compressive strength and crack resistance of the high-strength crack-resistant concrete prepared when using phosphogypsum gel material. The 28-day compressive strength and 28-day splitting tensile strength of the high-strength crack-resistant concrete prepared in Example 8 were greater than those prepared in Examples 14 and 15. The total crack area per unit area of the high-strength crack-resistant concrete prepared in Example 8 was also smaller than that of the high-strength crack-resistant concrete prepared in Examples 14 and 15. This indicates that when the weight ratio of phosphogypsum, limestone powder, silicate cement, and water is 50:3:7:25, the resulting high-strength crack-resistant concrete exhibits higher compressive strength and better crack resistance.
[0054] Compared with Example 8, Examples 16 and 17 investigated the effect of the average length of the reinforcing fibers on the compressive strength and crack resistance of the high-strength crack-resistant concrete. The 28-day compressive strength and 28-day splitting tensile strength of the high-strength crack-resistant concrete prepared in Example 8 were greater than those prepared in Examples 16 and 17. The total crack area per unit area of the high-strength crack-resistant concrete prepared in Example 8 was smaller than that of the high-strength crack-resistant concrete prepared in Examples 16 and 17. This indicates that when steel fibers with an average length of 12 mm and a cross-sectional diameter of 0.2 mm are used as reinforcing fibers, the resulting high-strength crack-resistant concrete exhibits higher compressive strength and better crack resistance.
[0055] Compared with Example 8, Example 18 investigated the effect of the preparation steps of high-strength crack-resistant concrete on the compressive strength and crack resistance of the obtained high-strength crack-resistant concrete. The 28-day compressive strength and 28-day splitting tensile strength of the high-strength crack-resistant concrete prepared in Example 18 were greater than those of the high-strength crack-resistant concrete prepared in Example 8. The total crack area per unit area of the high-strength crack-resistant concrete prepared in Example 18 was smaller than that of the high-strength crack-resistant concrete prepared in Example 8. This indicates that dispersing the phosphogypsum gel material in water and water-reducing agent before mixing it with other solid materials is beneficial to improving the compressive strength and crack resistance of the obtained high-strength crack-resistant concrete.
[0056] Using Example 2 as a control, Comparative Examples 1-3 investigated the effects of phosphogypsum coarse aggregate and phosphogypsum gel on the compressive strength and crack resistance of the prepared high-strength crack-resistant concrete. The 28-day compressive strength and 28-day splitting tensile strength of the high-strength crack-resistant concrete prepared using Example 2 were significantly greater than those of the high-strength crack-resistant concrete prepared using Comparative Examples 1-3. Furthermore, the total crack area per unit area of the high-strength crack-resistant concrete prepared using Example 2 was significantly smaller than that of the high-strength crack-resistant concrete prepared using Comparative Examples 1-3. This indicates that, compared to using basalt aggregate and cement, the simultaneous use of phosphogypsum coarse aggregate and phosphogypsum gel has a synergistic effect in improving the compressive strength and crack resistance of the prepared high-strength crack-resistant concrete.
[0057] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.
Claims
1. A method for preparing high-strength, crack-resistant concrete, characterized in that, Includes the following steps: Phosphogypsum, magnesium oxide, silicon dioxide, clay and water were mixed evenly in a weight ratio of 40:13:27:11:9 and then added to a drum granulator for granulation, drying and sieving to obtain pretreated particles with a particle size of 13-16 mm. The pretreated particles were then calcined at 1200℃ for 20 min, and then the temperature was raised to 1300℃ for another 1 h. After cooling, the particles were cured in a carbonization curing chamber at normal pressure, temperature of 25℃, relative humidity of 75% and carbon dioxide concentration of 75% for 15 h to obtain phosphogypsum coarse aggregate. Phosphogypsum, limestone powder, silicate cement and water were added to a ball mill in a weight ratio of 50:3:7:25 and ball-milled for 20 minutes. Then the mixture was dried in a nitrogen atmosphere at 50°C and ground to obtain phosphogypsum gel material. 1 kg of steel fiber with an average length of 12 mm and a cross-sectional diameter of 0.2 mm, 9 kg of cement, 60 kg of phosphogypsum coarse aggregate and 32 kg of fine aggregate were added to a concrete mixer and mixed evenly to obtain a solid mixture. Then, 4 kg of phosphogypsum gel material, 4 kg of water and 0.8 kg of water-reducing agent were mixed evenly and added to the concrete mixer. The mixture was then mixed evenly to obtain concrete.
Citation Information
Patent Citations
Phosphogypsum fly coal ash ceramsite and preparation method thereof
CN107686334A
Phosphogypsum-based cement concrete mortar and preparation process thereof
CN109851308A
Phosphogypsum lightweight aggregate concrete and preparation method thereof
CN116041026A