Environmentally friendly water-based paint
By adding composite damping reinforcement to the water-based coatings, the stability of existing water-based damping coatings in high temperature and corrosion environments is solved, and stable noise reduction and sound insulation effects are achieved. Improves the durability and flame retardancy of the coating.
Patent Information
- Application Number
- CN202410234275.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-01
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-03-01
AI Technical Summary
Existing water-based damping coatings have poor stability in high temperature and corrosion environments, and are susceptible to climate and temperature, making it difficult to maintain noise reduction and sound insulation effects for a long time.
Using a specific composite damping reinforcement, synergistically works with expanded graphite and expanded vermiculite, the spacing between graphite layers of expanded graphite is increased and the porous layered structure of expanded vermiculite is formed, and the damping performance of the coating is improved. The hollow pore structure of the composite damping reinforcement achieves a stable noise reduction effect.
It significantly improves the damping performance of water-based coatings, makes it stable noise reduction and sound insulation, and improves high temperature and corrosion resistance, enhancing the durability and flame retardancy of the coatings.
Smart Images

Figure BDA0004722093470000121
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of coating processing, and in particular relates to an environmentally friendly water-based coating. Background Art
[0002] In the field of modern transportation, in order to improve the operating efficiency of trains and provide passengers with a more comfortable riding experience, the use of advanced sound insulation and noise reduction technology has become an important research direction. Damping coatings have become an important choice for body interlayer spraying. Applying them to maglev trains and EMUs can achieve a quieter train operating environment. Water-based damping coatings use water-based formulas, which effectively reduce the use of organic solvents and reduce the emission of volatile organic compounds. They are environmentally friendly and do not contain harmful volatile substances, which is in line with the pursuit of environmentally friendly products in modern society. In high-speed rail transportation, reducing driving noise is crucial to ensure the peace of passengers' journey. By spraying water-based damping coatings on the body interlayer, the spread of external noise can be effectively isolated, the comfort of the riding environment can be improved, which helps to improve the overall operating efficiency of the train and reduce the impact of urban traffic noise on the surrounding environment. In short, water-based damping coatings play an important role in the interlayer spraying of high-speed railway vehicles such as maglev trains and EMUs, contributing to the sustainable development of urban transportation and the progress of modern railway transportation. Its environmental protection, sound insulation, noise reduction and other advantages make it one of the indispensable technologies in the future railway transportation field.
[0003] Chinese patent CN102408792B discloses a water-based damping coating for vehicles, comprising an emulsion base, an inorganic filler, a film-forming aid, a thickener, a heat-expandable organic hollow filling material, an organic foaming agent and water, wherein the emulsion base is a styrene-acrylic emulsion 1, a styrene-acrylic emulsion 3 and an epoxy resin emulsion used in combination, the inorganic filler is calcium carbonate and mica, the heat-expandable organic hollow filling material is polyacrylonitrile fiber, and the organic foaming agent is azobisisobutyronitrile; the damping coating has a microporous structure and can be coated into a film in one time, and can be used for coating vibration parts of various vehicles and motor products to suppress vibration and reduce noise. Chinese patent CN106566334B discloses a high-speed rail vehicle damping coating and its preparation method, the coating includes the following raw materials: waterproof emulsion, anti-rust emulsion, plasticized acrylic emulsion, pure acrylic emulsion, preservative, defoamer, thickener, composite flame retardant and functional enhancement material, the composite flame retardant is composed of antimony trioxide and aluminum hydroxide, and the functional enhancement material is selected from one or more of floating beads, mica powder, silica powder, anti-corrosion enhancement material and black slurry; the coating has good flame retardant effect and noise reduction effect, and can reduce the corrosion of substrate and coating film caused by bad media. Based on this, the present invention aims to develop an environmentally friendly water-based coating with stable noise reduction and sound insulation effect, and has strong resistance, is not easy to powder, and is not easily affected by climate and temperature. Summary of the invention
[0004] In view of the deficiencies in the above-mentioned prior art, the present invention provides an environmentally friendly water-based paint, which significantly improves the damping performance of the water-based paint by adding a specific composite damping reinforcement material to work synergistically with expanded graphite and expanded vermiculite, so that the water-based paint has stable noise reduction and sound insulation effects, and is wear-resistant and durable. The present invention also provides a method for preparing the above-mentioned environmentally friendly water-based paint, which is simple and suitable for industrial production.
[0005] The technical solution adopted by the present invention is:
[0006] An environmentally friendly water-based paint comprises the following raw materials:
[0007] Acrylic emulsion, fluorocarbon emulsion, expanded graphite, expanded vermiculite, composite damping reinforcement, film-forming aid, dispersant, defoamer, leveling agent, water.
[0008] Preferably, an environmentally friendly water-based paint is composed of the following raw materials in parts by weight:
[0009] 20-60 parts by weight of acrylic emulsion, 10-50 parts by weight of fluorocarbon emulsion, 1-15 parts by weight of expanded graphite, 1-15 parts by weight of expanded vermiculite, 2-10 parts by weight of composite damping reinforcement material, 0.5-5 parts by weight of film-forming aid, 0.5-5 parts by weight of dispersant, 0.5-5 parts by weight of defoamer, 0.5-5 parts by weight of leveling agent, and 5-30 parts by weight of water.
[0010] Preferably, an environmentally friendly water-based paint is composed of the following raw materials in parts by weight:
[0011] 40-50 parts by weight of acrylic emulsion, 20-30 parts by weight of fluorocarbon emulsion, 5-10 parts by weight of expanded graphite, 5-10 parts by weight of expanded vermiculite, 5-8 parts by weight of composite damping reinforcement material, 1-3 parts by weight of film-forming aid, 1-3 parts by weight of dispersant, 1-2 parts by weight of defoamer, 1-2 parts by weight of leveling agent, and 10-20 parts by weight of water.
[0012] Preferably, the acrylic emulsion is a water-based acrylic emulsion; and the fluorocarbon emulsion is a water-based elastic fluorocarbon emulsion. In the present invention, a specific water-based elastic fluorocarbon emulsion is added to the coating formula to match the water-based acrylic emulsion as a base emulsion, which can effectively improve the elongation, durability and weather resistance of the water-based coating, and help improve its comprehensive performance.
[0013] The present invention adopts expanded graphite and expanded vermiculite as porous functional fillers, which have a sound-absorbing effect. When sound passes through, the noise reduction effect of the coating can be improved by sound absorption. Among them, the expanded graphite has a space steric hindrance effect due to the increased spacing between graphite layers, which can not only enhance the damping performance of the coating, but also give full play to the graphite to improve the high temperature resistance and corrosion resistance of the coating. Expanded vermiculite has a porous layered structure, which can effectively absorb sound waves in the environment and convert them into micro-vibration and heat energy. Its porosity and layered structure help to produce a space steric hindrance effect, which can further slow down the propagation of sound waves, reduce the sound wave energy, and achieve a noise reduction effect. It also has good fireproof and insulation properties, and can improve the flame retardancy and stability of the coating.
[0014] Preferably, the composite damping reinforcement material is prepared by the following method:
[0015] D1: 3-aminopropylmethyldiethoxysilane and ethanol aqueous solution are mixed, stirred at 35-40° C. to obtain a treated liquid, and then inorganic particles are added, stirred at 50-60° C., filtered, and dried at 60-80° C. to obtain pretreated inorganic particles, and the pretreated inorganic particles are added to cyclohexane at room temperature, ultrasonicated, and filtered to obtain modified inorganic particles;
[0016] D2: at 65-70°C and in a nitrogen atmosphere, n-butyl methacrylate, hydroxypropyl acrylate, glycidyl methacrylate, acrylic acid and sodium polyacrylate are added to water and mixed evenly, and then ammonium persulfate is added dropwise, and then the modified inorganic particles obtained in the above step D1 are added, mixed evenly, reacted, filtered, and dried at 90-100°C to obtain the composite damping reinforcement material.
[0017] Preferably, the composite damping reinforcement material is prepared by the following method:
[0018] D1: 3-6 parts by weight of 3-aminopropylmethyldiethoxysilane and 200-400 parts by weight of 70-90wt% ethanol aqueous solution are mixed, stirred at 35-40°C and 400-500rpm for 10-30min to obtain a treated liquid, then 12-20 parts by weight of inorganic particles are added, stirred at 50-60°C and 400-500rpm for 90-120min, filtered, and dried at 60-80°C for 10-15h to obtain pretreated inorganic particles, and the pretreated inorganic particles are added to cyclohexane at a solid-liquid ratio of 1g:7-10mL at room temperature, ultrasonicated for 10-30min, filtered, and modified inorganic particles are obtained;
[0019] D2: At 65-70° C. and in a nitrogen atmosphere, 20-30 parts by weight of n-butyl methacrylate, 3-7 parts by weight of hydroxypropyl acrylate, 1-3 parts by weight of glycidyl methacrylate, 5-10 parts by weight of acrylic acid and 1-5 parts by weight of sodium polyacrylate are added to 100-300 parts by weight of water and mixed evenly, then 0.2-0.8 parts by weight of ammonium persulfate are added dropwise, and then the modified inorganic particles obtained in the above step D1 are added, mixed evenly, reacted for 1-3 hours, filtered, and dried at 90-100° C. for 3-8 hours to obtain the composite damping reinforcement material.
[0020] Preferably, in step D1, the ultrasonic power is 50-100 W and the ultrasonic frequency is 20-40 kHz.
[0021] Preferably, the inorganic particles in step D1 are a mixture of diatomaceous earth and dolomite in a weight ratio of 1-2:1.
[0022] Further, the present invention also adds a specific composite damping reinforcement material to synergize with expanded graphite and expanded vermiculite, significantly improving the damping performance of the water-based coating, so that it has a stable noise reduction and sound insulation effect. The composite damping reinforcement material is a porous microsphere of a core-shell structure, the microsphere shell is a thermoplastic acrylic polymer, and the microsphere core is an inorganic particle with a surface impregnated with low-boiling cyclohexane (boiling point of about 80°C). When dried at a temperature above 90°C, the low-boiling cyclohexane is gasified, and the thermoplastic shell expands, while the inorganic particles remain unchanged. It exists as a core inside the expanded microsphere shell. After the preparation is completed, as the temperature decreases, the low-boiling cyclohexane liquefies, but the expanded microsphere shell cannot restore the initial volume, thereby forming a hollow pore structure inside the microsphere. When subjected to external periodic vibration, due to the mass inertia and intermolecular friction of the internal high-density inorganic particles, a vibration reduction effect similar to a tuned mass damping system is formed, consuming more kinetic energy, thereby improving the damping performance and service life of the coating.
[0023] The present invention preferably uses a mixture of diatomite and dolomite as inorganic particles, and utilizes the respective advantages of the two in terms of physical and chemical properties to produce a synergistic effect, so that the composite damping reinforcement material performs better in terms of damping performance, etc. In addition, the present invention first modifies the inorganic particles, and the hydrolyzate of the treatment liquid 3-aminopropylmethyldiethoxysilane is bound to the surface of the inorganic particles through electrostatic and hydrogen bonding, which improves the wettability and dispersibility of the inorganic particles in the reaction system on the one hand, and on the other hand, the amino groups contained on the surface after modification can assist the curing of the acrylic resin, so that the acrylic polymer effectively coats the inorganic particles.
[0024] Preferably, the film-forming aid is at least one of dipropylene glycol methyl ether, dipropylene glycol butyl ether, tripropylene glycol butyl ether, propylene glycol dimethyl ether, and dodecyl alcohol ester.
[0025] Preferably, the dispersant is any one of BYK-190 dispersant, BYK-182 dispersant and BYK-2010 dispersant.
[0026] Preferably, the defoamer is any one of BYK-012 defoamer, BYK-016 defoamer and BYK-092 defoamer.
[0027] Preferably, the leveling agent is any one of TEGO-500 leveling agent, TEGO-450 leveling agent, and TEGO-270 leveling agent.
[0028] Preferably, the particle size of the expanded graphite is 10-100 μm, and the particle size of the expanded vermiculite is 10-100 μm.
[0029] The present invention also provides a method for preparing an environmentally friendly water-based coating, comprising the following steps:
[0030] Acrylic emulsion, fluorocarbon emulsion and water are mixed, stirred at 500-1000 rpm for 10-20 minutes, then expanded graphite, expanded vermiculite and composite damping reinforcement are added and stirred for 30-50 minutes, and then a film-forming aid, a dispersant, a defoamer and a leveling agent are added and stirred for 20-40 minutes to obtain the environmentally friendly water-based coating.
[0031] Beneficial effects of the present invention:
[0032] 1. The environmentally friendly water-based coating prepared by the present invention uses a specific water-based elastic fluorocarbon emulsion in combination with a water-based acrylic emulsion as a base emulsion, which can effectively improve the elongation, durability and weather resistance of the water-based coating and help improve its comprehensive performance.
[0033] 2. The present invention adopts expanded graphite and expanded vermiculite as porous functional fillers, wherein the expanded graphite has a larger spacing between graphite layers, and the steric hindrance effect can not only enhance the damping performance of the coating, but also give full play to the graphite to improve the high temperature resistance and corrosion resistance of the coating. Expanded vermiculite has a porous layered structure, which can effectively absorb sound waves in the environment. Its porosity and layered structure help to produce a steric hindrance effect, which can further slow down the propagation of sound waves, reduce the energy of sound waves, and achieve noise reduction effects. It also has good fireproof and insulation properties, and can improve the flame retardancy and stability of the coating.
[0034] 3. The present invention further improves the damping performance of the water-based coating by adding a specific composite damping reinforcement material to work synergistically with expanded graphite and expanded vermiculite, so that the water-based coating has a stable noise reduction and sound insulation effect. DETAILED DESCRIPTION
[0035] The following will be combined with the specific embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] The acrylic emulsion used is water-based acrylic emulsion produced by Shanghai Wenhua Chemical Pigment Co., Ltd., model: RW-116, with a solid content of 40%.
[0037] Fluorocarbon emulsion uses water-based elastic fluorocarbon emulsion produced by Beijing Runbo Hengtong Technology Co., Ltd., model: HT-116EF, with a solid content of 50%.
[0038] Example 1
[0039] An environmentally friendly water-based paint is composed of the following raw materials in parts by weight:
[0040] 45 parts by weight of acrylic emulsion, 25 parts by weight of fluorocarbon emulsion, 9 parts by weight of expanded graphite (particle size 100 μm), 6 parts by weight of expanded vermiculite (particle size 50 μm), 6.5 parts by weight of composite damping reinforcing material, 2.5 parts by weight of film-forming aid dipropylene glycol butyl ether, 2 parts by weight of BYK-190 dispersant, 1.2 parts by weight of BYK-012 defoamer, 1.2 parts by weight of TEGO-450 leveling agent, and 15 parts by weight of water.
[0041] The composite damping reinforcement material is prepared by the following method:
[0042] D1: 4.5 parts by weight of 3-aminopropylmethyldiethoxysilane (CAS: 3179-76-8) and 300 parts by weight of 80 wt% ethanol aqueous solution were mixed, stirred at 37°C and 450 rpm for 20 min to obtain a treated liquid, then 16 parts by weight of inorganic particles were added, stirred at 56°C and 450 rpm for 100 min, filtered, and dried at 70°C for 12 h to obtain pretreated inorganic particles, and the pretreated inorganic particles were added to cyclohexane at a solid-liquid ratio of 1 g:8 mL at room temperature, ultrasonicated for 20 min, filtered, and modified inorganic particles were obtained; the inorganic particles were a mixture of diatomaceous earth (particle size 40 μm) and dolomite (particle size 50 μm) at a weight ratio of 1.5:1; wherein the ultrasonic power was 60 W and the ultrasonic frequency was 30 kHz;
[0043] D2: At 70°C and in a nitrogen atmosphere, 25 parts by weight of n-butyl methacrylate, 5 parts by weight of hydroxypropyl acrylate, 2 parts by weight of glycidyl methacrylate, 8 parts by weight of acrylic acid and 3 parts by weight of dispersant sodium polyacrylate are added to 200 parts by weight of water and mixed evenly, then 0.5 parts by weight of initiator ammonium persulfate is added dropwise, and then the modified inorganic fine particles obtained in the above step D1 are added, mixed evenly, reacted for 2.5 hours, filtered, and dried at 95°C for 6 hours to obtain the composite damping reinforcement material.
[0044] A method for preparing an environmentally friendly water-based coating comprises the following steps:
[0045] Acrylic emulsion, fluorocarbon emulsion and water were mixed, stirred at room temperature and 700 rpm for 15 minutes, then expanded graphite, expanded vermiculite and composite damping reinforcement were added and stirred for 45 minutes, and then film-forming aid dipropylene glycol butyl ether, BYK-190 dispersant, BYK-012 defoamer and TEGO-450 leveling agent were added and stirred for 30 minutes to obtain the environmentally friendly water-based coating.
[0046] Example 2
[0047] An environmentally friendly water-based paint is composed of the following raw materials in parts by weight:
[0048] 45 parts by weight of acrylic emulsion, 25 parts by weight of fluorocarbon emulsion, 9 parts by weight of expanded graphite (particle size 100 μm), 6 parts by weight of expanded vermiculite (particle size 50 μm), 6.5 parts by weight of composite damping reinforcing material, 2.5 parts by weight of film-forming aid dipropylene glycol butyl ether, 2 parts by weight of BYK-190 dispersant, 1.2 parts by weight of BYK-012 defoamer, 1.2 parts by weight of TEGO-450 leveling agent, and 15 parts by weight of water.
[0049] The composite damping reinforcement material is prepared by the following method:
[0050] D1 Take 16 parts by weight of inorganic particles, add them into cyclohexane at a solid-liquid ratio of 1g:8mL at room temperature, ultrasonicate for 20 minutes, filter, and obtain modified inorganic particles; the inorganic particles are a mixture of diatomaceous earth (particle size 40μm) and dolomite (particle size 50μm) at a weight ratio of 1.5:1; wherein the ultrasonic power is 60W and the ultrasonic frequency is 30kHz;
[0051] D2: At 70°C and in a nitrogen atmosphere, 25 parts by weight of n-butyl methacrylate, 5 parts by weight of hydroxypropyl acrylate, 2 parts by weight of glycidyl methacrylate, 8 parts by weight of acrylic acid and 3 parts by weight of dispersant sodium polyacrylate are added to 200 parts by weight of water and mixed evenly, then 0.5 parts by weight of initiator ammonium persulfate is added dropwise, and then the modified inorganic fine particles obtained in the above step D1 are added, mixed evenly, reacted for 2.5 hours, filtered, and dried at 95°C for 6 hours to obtain the composite damping reinforcement material.
[0052] A method for preparing an environmentally friendly water-based coating comprises the following steps:
[0053] Acrylic emulsion, fluorocarbon emulsion and water were mixed, stirred at room temperature and 700 rpm for 15 minutes, then expanded graphite, expanded vermiculite and composite damping reinforcement were added and stirred for 45 minutes, and then film-forming aid dipropylene glycol butyl ether, BYK-190 dispersant, BYK-012 defoamer and TEGO-450 leveling agent were added and stirred for 30 minutes to obtain the environmentally friendly water-based coating.
[0054] Example 3
[0055] An environmentally friendly water-based paint is composed of the following raw materials in parts by weight:
[0056] 45 parts by weight of acrylic emulsion, 25 parts by weight of fluorocarbon emulsion, 9 parts by weight of expanded graphite (particle size 100 μm), 6 parts by weight of expanded vermiculite (particle size 50 μm), 6.5 parts by weight of composite damping reinforcing material, 2.5 parts by weight of film-forming aid dipropylene glycol butyl ether, 2 parts by weight of BYK-190 dispersant, 1.2 parts by weight of BYK-012 defoamer, 1.2 parts by weight of TEGO-450 leveling agent, and 15 parts by weight of water.
[0057] The composite damping reinforcement material is prepared by the following method:
[0058] D1: 4.5 parts by weight of 3-aminopropylmethyldiethoxysilane (CAS: 3179-76-8) and 300 parts by weight of 80 wt% ethanol aqueous solution were mixed, stirred at 37°C and 450 rpm for 20 min to obtain a treated liquid, then 16 parts by weight of inorganic particles were added, stirred at 56°C and 450 rpm for 100 min, filtered, and dried at 70°C for 12 h to obtain pretreated inorganic particles, and the pretreated inorganic particles were added to n-hexane at a solid-liquid ratio of 1 g:8 mL at room temperature, ultrasonicated for 20 min, filtered, and modified inorganic particles were obtained; the inorganic particles were a mixture of diatomaceous earth (particle size 40 μm) and dolomite (particle size 50 μm) at a weight ratio of 1.5:1; wherein the ultrasonic power was 60 W and the ultrasonic frequency was 30 kHz;
[0059] D2: At 70°C and in a nitrogen atmosphere, 25 parts by weight of n-butyl methacrylate, 5 parts by weight of hydroxypropyl acrylate, 2 parts by weight of glycidyl methacrylate, 8 parts by weight of acrylic acid and 3 parts by weight of dispersant sodium polyacrylate are added to 200 parts by weight of water and mixed evenly, then 0.5 parts by weight of initiator ammonium persulfate is added dropwise, and then the modified inorganic fine particles obtained in the above step D1 are added, mixed evenly, reacted for 2.5 hours, filtered, and dried at 95°C for 6 hours to obtain the composite damping reinforcement material.
[0060] A method for preparing an environmentally friendly water-based coating comprises the following steps:
[0061] Acrylic emulsion, fluorocarbon emulsion and water were mixed, stirred at room temperature and 700 rpm for 15 minutes, then expanded graphite, expanded vermiculite and composite damping reinforcement were added and stirred for 45 minutes, and then film-forming aid dipropylene glycol butyl ether, BYK-190 dispersant, BYK-012 defoamer and TEGO-450 leveling agent were added and stirred for 30 minutes to obtain the environmentally friendly water-based coating.
[0062] Example 4
[0063] An environmentally friendly water-based paint is composed of the following raw materials in parts by weight:
[0064] 45 parts by weight of acrylic emulsion, 25 parts by weight of fluorocarbon emulsion, 9 parts by weight of expanded graphite (particle size 100 μm), 6 parts by weight of expanded vermiculite (particle size 50 μm), 6.5 parts by weight of composite damping reinforcing material, 2.5 parts by weight of film-forming aid dipropylene glycol butyl ether, 2 parts by weight of BYK-190 dispersant, 1.2 parts by weight of BYK-012 defoamer, 1.2 parts by weight of TEGO-450 leveling agent, and 15 parts by weight of water.
[0065] The composite damping reinforcement material is prepared by the following method:
[0066] D1: 4.5 parts by weight of 3-aminopropylmethyldiethoxysilane (CAS: 3179-76-8) and 300 parts by weight of 80 wt% ethanol aqueous solution were mixed, stirred at 37°C and 450 rpm for 20 min to obtain a treated liquid, then 16 parts by weight of inorganic particles were added, stirred at 56°C and 450 rpm for 100 min, filtered, and dried at 70°C for 12 h to obtain pretreated inorganic particles, and the pretreated inorganic particles were added to cyclohexane at a solid-liquid ratio of 1 g:8 mL at room temperature, ultrasonicated for 20 min, filtered, and modified inorganic particles were obtained; the inorganic particles were diatomaceous earth (particle size 40 μm); wherein the ultrasonic power was 60 W and the ultrasonic frequency was 30 kHz;
[0067] D2: At 70°C and in a nitrogen atmosphere, 25 parts by weight of n-butyl methacrylate, 5 parts by weight of hydroxypropyl acrylate, 2 parts by weight of glycidyl methacrylate, 8 parts by weight of acrylic acid and 3 parts by weight of dispersant sodium polyacrylate are added to 200 parts by weight of water and mixed evenly, then 0.5 parts by weight of initiator ammonium persulfate is added dropwise, and then the modified inorganic fine particles obtained in the above step D1 are added, mixed evenly, reacted for 2.5 hours, filtered, and dried at 95°C for 6 hours to obtain the composite damping reinforcement material.
[0068] A method for preparing an environmentally friendly water-based coating comprises the following steps:
[0069] Acrylic emulsion, fluorocarbon emulsion and water were mixed, stirred at room temperature and 700 rpm for 15 minutes, then expanded graphite, expanded vermiculite and composite damping reinforcement were added and stirred for 45 minutes, and then film-forming aid dipropylene glycol butyl ether, BYK-190 dispersant, BYK-012 defoamer and TEGO-450 leveling agent were added and stirred for 30 minutes to obtain the environmentally friendly water-based coating.
[0070] Example 5
[0071] An environmentally friendly water-based paint is composed of the following raw materials in parts by weight:
[0072] 45 parts by weight of acrylic emulsion, 25 parts by weight of fluorocarbon emulsion, 9 parts by weight of expanded graphite (particle size 100 μm), 6 parts by weight of expanded vermiculite (particle size 50 μm), 6.5 parts by weight of composite damping reinforcing material, 2.5 parts by weight of film-forming aid dipropylene glycol butyl ether, 2 parts by weight of BYK-190 dispersant, 1.2 parts by weight of BYK-012 defoamer, 1.2 parts by weight of TEGO-450 leveling agent, and 15 parts by weight of water.
[0073] The composite damping reinforcement material is prepared by the following method:
[0074] D1: 4.5 parts by weight of 3-aminopropylmethyldiethoxysilane (CAS: 3179-76-8) and 300 parts by weight of 80 wt% ethanol aqueous solution were mixed, stirred at 37°C and 450 rpm for 20 min to obtain a treated liquid, then 16 parts by weight of inorganic particles were added, stirred at 56°C and 450 rpm for 100 min, filtered, and dried at 70°C for 12 h to obtain pretreated inorganic particles, and the pretreated inorganic particles were added to cyclohexane at a solid-liquid ratio of 1 g: 8 mL at room temperature, ultrasonicated for 20 min, filtered, and modified inorganic particles were obtained; the inorganic particles were dolomite (particle size 50 μm); wherein the ultrasonic power was 60 W and the ultrasonic frequency was 30 kHz;
[0075] D2: At 70°C and in a nitrogen atmosphere, 25 parts by weight of n-butyl methacrylate, 5 parts by weight of hydroxypropyl acrylate, 2 parts by weight of glycidyl methacrylate, 8 parts by weight of acrylic acid and 3 parts by weight of dispersant sodium polyacrylate are added to 200 parts by weight of water and mixed evenly, then 0.5 parts by weight of initiator ammonium persulfate is added dropwise, and then the modified inorganic fine particles obtained in the above step D1 are added, mixed evenly, reacted for 2.5 hours, filtered, and dried at 95°C for 6 hours to obtain the composite damping reinforcement material.
[0076] A method for preparing an environmentally friendly water-based coating comprises the following steps:
[0077] Acrylic emulsion, fluorocarbon emulsion and water were mixed, stirred at room temperature and 700 rpm for 15 minutes, then expanded graphite, expanded vermiculite and composite damping reinforcement were added and stirred for 45 minutes, and then film-forming aid dipropylene glycol butyl ether, BYK-190 dispersant, BYK-012 defoamer and TEGO-450 leveling agent were added and stirred for 30 minutes to obtain the environmentally friendly water-based coating.
[0078] Example 6
[0079] An environmentally friendly water-based paint is composed of the following raw materials in parts by weight:
[0080] 45 parts by weight of acrylic emulsion, 25 parts by weight of fluorocarbon emulsion, 9 parts by weight of expanded graphite (particle size 100 μm), 6 parts by weight of expanded vermiculite (particle size 50 μm), 6.5 parts by weight of composite damping reinforcing material, 2.5 parts by weight of film-forming aid dipropylene glycol butyl ether, 2 parts by weight of BYK-190 dispersant, 1.2 parts by weight of BYK-012 defoamer, 1.2 parts by weight of TEGO-450 leveling agent, and 15 parts by weight of water.
[0081] The composite damping reinforcement material is prepared by the following method:
[0082] 4.5 parts by weight of 3-aminopropylmethyldiethoxysilane (CAS: 3179-76-8) and 300 parts by weight of 80wt% ethanol aqueous solution were mixed, stirred at 37°C and 450rpm for 20min to obtain a treatment liquid, and then 16 parts by weight of inorganic particles were added, stirred at 56°C and 450rpm for 100min, filtered, and dried at 70°C for 12h to obtain the composite damping reinforcement material; the inorganic particles were a mixture of diatomaceous earth (particle size 40μm) and dolomite (particle size 50μm) in a weight ratio of 1.5:1.
[0083] A method for preparing an environmentally friendly water-based coating comprises the following steps:
[0084] Acrylic emulsion, fluorocarbon emulsion and water were mixed, stirred at room temperature and 700 rpm for 15 minutes, then expanded graphite, expanded vermiculite and composite damping reinforcement were added and stirred for 45 minutes, and then film-forming aid dipropylene glycol butyl ether, BYK-190 dispersant, BYK-012 defoamer and TEGO-450 leveling agent were added and stirred for 30 minutes to obtain the environmentally friendly water-based coating.
[0085] Test Example 1
[0086] Take the environmentally friendly water-based paints of Examples 1-6 respectively, and then apply a layer of the environmentally friendly water-based paint on a metal copper plate to obtain a dry film with a thickness of 2 mm. The dry film is used as a sample, and the composite loss factor of the sample at different temperatures is tested with reference to the standard GB / T 16406-1996. The larger the composite loss factor, the better the damping performance of the environmentally friendly water-based paint, and the better the sound insulation and noise reduction effect it has. The test results are shown in Table 1.
[0087] Table 1. Damping properties of environmentally friendly water-based coatings
[0088]
[0089] Test Example 2
[0090] The sample obtained in Test Example 1 was immersed in a 3.5% sodium chloride solution for two weeks and then subjected to a composite loss factor (40° C.) test to evaluate the salt spray resistance of the environmentally friendly water-based coating. The test results are shown in Table 2.
[0091] Table 2. Salt spray resistance of environmentally friendly water-based coatings
[0092] Composite loss factor (40℃) Example 1 0.170 Example 6 0.082
[0093] As can be seen from the above test results, the environmentally friendly water-based paint prepared by the present invention significantly improves the damping performance of water-based paint by adding specific composite damping reinforcement material and expanded graphite, expanded vermiculite synergy, so that it has stable noise reduction, sound insulation effect.Compared with Example 2-6, the damping and anticorrosion performance of Example 1 are the best.This is because the composite damping reinforcement material used in Example 1 is a microsphere shell with thermoplastic acrylic polymer, and the inorganic particles impregnated with low-boiling-point cyclohexane on the surface are microsphere kernels, and low-boiling-point cyclohexane is gasified during drying, and the thermoplastic shell expands, and the inorganic particles are constant, and it is present as a core inside the expanded microsphere shell, and after the preparation is completed, as the temperature is reduced, the low-boiling-point cyclohexane is liquefied, but the expanded microsphere shell cannot restore the initial volume, so as to form a hollow pore structure inside the microsphere, when subjected to external periodic vibration, due to the mass inertia and intermolecular friction of internal high-density inorganic particles, a vibration reduction effect similar to a tuned mass damping system is formed, more kinetic energy is consumed, so as to improve the damping performance and service life of coating. By selecting a mixture of diatomite and dolomite as inorganic particles, the respective advantages of the two in physical and chemical properties are utilized to produce a synergistic effect, so that the composite damping reinforcement material performs better in terms of damping performance, etc. In addition, the inorganic particles are also modified, and the hydrolyzate of the treatment liquid 3-aminopropylmethyldiethoxysilane is bound to the surface of the inorganic particles through electrostatic and hydrogen bonding. On the one hand, the wettability and dispersibility of the inorganic particles in the reaction system are improved, and on the other hand, the amino groups contained on the surface after modification can assist the curing of the acrylic resin, so that the acrylic polymer effectively coats the inorganic particles.
[0094] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. An environmentally friendly water-based paint, composed of the following raw materials in parts by weight: 20-60 parts by weight of acrylic emulsion, 10-50 parts by weight of fluorocarbon emulsion, 1-15 parts by weight of expanded graphite, 1-15 parts by weight of expanded vermiculite, 2-10 parts by weight of composite damping reinforcement material, 0.5-5 parts by weight of film-forming aid, 0.5-5 parts by weight of dispersant, 0.5-5 parts by weight of defoamer, 0.5-5 parts by weight of leveling agent, 5-30 parts by weight of water; The composite damping reinforcement material is prepared by the following method: D1: 3-aminopropylmethyldiethoxysilane and ethanol aqueous solution are mixed, stirred at 35-40° C. to obtain a treated liquid, and then inorganic particles are added, stirred at 50-60° C., filtered, and dried at 60-80° C. to obtain pretreated inorganic particles, and the pretreated inorganic particles are added to cyclohexane at room temperature, ultrasonicated, and filtered to obtain modified inorganic particles; D2: adding n-butyl methacrylate, hydroxypropyl acrylate, glycidyl methacrylate, acrylic acid and sodium polyacrylate to water at 65-70°C and nitrogen atmosphere, mixing evenly, then dropping ammonium persulfate, and then adding the modified inorganic particles obtained in the above step D1, mixing evenly, reacting, filtering, and drying at 90-100°C to obtain the composite damping reinforcement material; The inorganic particles in step D1 are a mixture of diatomaceous earth and dolomite.
2. The environmentally friendly water-based paint according to claim 1, characterized in that: The invention is composed of the following raw materials in parts by weight: 40-50 parts by weight of acrylic emulsion, 20-30 parts by weight of fluorocarbon emulsion, 5-10 parts by weight of expanded graphite, 5-10 parts by weight of expanded vermiculite, 5-8 parts by weight of composite damping reinforcement material, 1-3 parts by weight of film-forming aid, 1-3 parts by weight of dispersant, 1-2 parts by weight of defoamer, 1-2 parts by weight of leveling agent and 10-20 parts by weight of water.
3. The environmentally friendly water-based paint according to claim 1, characterized in that: The film-forming aid is at least one of dipropylene glycol methyl ether, dipropylene glycol butyl ether, tripropylene glycol butyl ether, propylene glycol dimethyl ether and dodecyl alcohol ester.
4. The environmentally friendly water-based paint according to claim 1, characterized in that: The dispersant is any one of BYK-190 dispersant, BYK-182 dispersant and BYK-2010 dispersant.
5. The environmentally friendly water-based paint according to claim 1, characterized in that: The defoamer is any one of BYK-012 defoamer, BYK-016 defoamer and BYK-092 defoamer.
6. The environmentally friendly water-based paint according to claim 1, characterized in that: The leveling agent is any one of TEGO-500 leveling agent, TEGO-450 leveling agent and TEGO-270 leveling agent.
7. The method for preparing the environmentally friendly water-based coating according to any one of claims 1 to 6, characterized in that: The method comprises the following steps: mixing acrylic emulsion, fluorocarbon emulsion and water, stirring, then adding expanded graphite, expanded vermiculite and composite damping reinforcement material and continuing to stir, and then adding film-forming aid, dispersant, defoamer and leveling agent and stirring to obtain the environmentally friendly water-based paint.