Optical cable water-blocking filling ointment and preparation method thereof

By adding modified carbon nanotubes and water absorption expansion agent to the optical cable water-blocking paste, the problem of low oil separation and water absorption efficiency of oil paste in the prior art is solved, and higher water absorption and aging resistance are achieved, and antibacterials are enhanced performance and remain stable at high temperatures.

CN118994928AInactive Publication Date: 2024-11-22ANHUI LANGDE NEW MATERIALS CO LTD

Patent Information

Application Number
CN202411291558.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing optical cable water-blocking filler paste is prone to oil separation and water absorption efficiency reduction in long-term use, resulting in attenuation of optical fiber signal and affecting the transmission performance of optical cables. The hydrophilicity and oil absorption of inorganic fillers lead to serious particle agglomeration, affecting water-blocking. performance.

Method used

By adding modified carbon nanotubes and water-absorbing expansion agent, the modified carbon nanotubes are treated with triethylenetetramine and grafted with antioxidant to form modified carbon nanotubes with antioxidant and antibacterial properties; the water-absorbing expansion agent uses carboxylic Methylcellulose and bentonite form a three-dimensional network structure to improve the water absorption and water locking ability of the paste.

Benefits of technology

It significantly improves the water absorption efficiency and aging resistance of the optical cable water-blocking oil paste, avoids oil precipitation and signal attenuation, enhances antibacterial performance, and maintains stability under high temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to the field of filling factice, and discloses optical cable water-blocking filling factice and a preparation method thereof.The optical cable water-blocking filling factice comprises, by weight, 70-85 parts of base oil, 5-10 parts of an oil separation inhibitor, 8-15 parts of modified carbon nanotubes and 7-12 parts of a water absorption expanding agent; the modified carbon nanotubes are prepared by the following steps: treating oxidized carbon nanotubes with triethylene tetramine, grafting glycidyl methacrylate, further grafting with an antioxidant 3-(3, 5-di-tert-butyl-4-hydroxyphenyl) propionic acid, and polymerizing with N-phenylmaleimide. The water absorption expanding agent is prepared by taking carboxymethyl cellulose as a framework, grafting polyacrylic acid by adopting an aqueous solution polymerization method and compounding with bentonite, and the filling ointment is endowed with excellent water absorption efficiency and aging resistance by adding the modified carbon nanotubes and the water absorption expanding agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of filling grease, and in particular to an optical cable water-blocking filling grease and a preparation method thereof. Background Art

[0002] Optical communication relies on optical cables to transmit information. The core material of optical cables is optical fiber. Optical fiber will corrode under the influence of water, moisture and stress. Once the optical fiber is corroded, the information transmission performance of the optical cable will be greatly reduced. The optical cable water-blocking filling grease is a water-blocking material widely used in optical cables. It plays the role of sealing, water absorption and moisture isolation in optical cables. It can protect the optical fiber from the influence of the external environment, thereby maintaining the stability and reliability of optical fiber transmission.

[0003] Inorganic fillers are added to the existing optical cable water-blocking filling paste to improve its physical properties, heat resistance and flame retardant properties. However, the inorganic filler has a hydrophilic surface and a high oil absorption value, and is poorly dispersed in the oily matrix, resulting in serious particle agglomeration. It also consumes oil, resulting in the optical cable water-blocking filling paste having a long water absorption time and being unable to quickly absorb and swell when in contact with water, which seriously affects the water-blocking properties of the optical cable water-blocking filling paste. In addition, the existing optical cable water-blocking filling paste is prone to severe oil separation, aging, reduced water absorption efficiency, and other problems under long-term high temperature conditions, which in turn causes optical fiber signal attenuation and affects the transmission performance of the optical cable. Summary of the invention

[0004] In order to solve the deficiencies mentioned in the above background technology, the purpose of the present invention is to provide a water-blocking filling paste for optical cables and a preparation method thereof, and to give the filling paste excellent water absorption efficiency and aging resistance by adding modified carbon nanotubes and water-absorbing swelling agents.

[0005] The purpose of the present invention can be achieved through the following technical solutions: An optical cable water-blocking filling paste comprises the following components in parts by weight: 70-85 parts of base oil, 5-10 parts of oil separation inhibitor, 8-15 parts of modified carbon nanotubes, and 7-12 parts of water absorption swelling agent; The modified carbon nanotubes are prepared by treating oxidized carbon nanotubes with triethylenetetramine, grafting glycidyl methacrylate, further grafting with antioxidant 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid, and polymerizing with N-phenylmaleimide; the water-absorbing swelling agent is prepared by using carboxymethyl cellulose as a skeleton, grafting polyacrylic acid by aqueous solution polymerization, and compounding with bentonite.

[0006] Preferably, the method for preparing the modified carbon nanotubes comprises the following steps: (1) Place carbon nanotubes in a reactor, add concentrated nitric acid with a mass fraction of 65-68%, stir and mix, place at 105-110° C. for reflux reaction for 4-8 hours, and after the reaction is completed, filter, wash and dry to prepare oxidized carbon nanotubes; (2) N, N-diisopropylcarbodiimide, 1-hydroxybenzotriazole and oxidized carbon nanotubes are placed in a reactor, N, N-dimethylformamide is added for ultrasonic dispersion, and then triethylenetetramine is added for stirring and reaction for 20 to 24 hours. After the reaction is completed, the mixture is filtered, washed and dried to obtain amino carbon nanotubes; (3) ultrasonically dispersing the amino carbon nanotubes in N,N-dimethylformamide, then adding glycidyl methacrylate, and reacting at 90-110°C for 3-4 hours. After the reaction is completed, filtering, washing, and drying to prepare functionalized carbon nanotubes; (4) ultrasonically dispersing the functionalized carbon nanotubes in dichloromethane to obtain a dispersion, placing 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid and 4-dimethylaminopyridine in a reactor, adding dichloromethane, stirring for 10-25 min at 0-4 °C in a nitrogen atmosphere, then dissolving 1-ethyl-3 (3-dimethylpropylamine) carbodiimide in dichloromethane and adding the mixture to the reactor, stirring for 2-3 h to obtain a reaction solution, stirring the dispersion and the reaction solution in a nitrogen atmosphere for 18-24 h, filtering, washing, and drying after the reaction is completed to obtain antioxidant carbon nanotubes; (5) Antioxidant carbon nanotubes and N-phenylmaleimide are placed in a reactor filled with xylene solvent and dispersed evenly. The temperature is raised to 70-85°C in a nitrogen atmosphere and the reaction is carried out for 0.5-1h. Then, azobisisobutyronitrile is added and the reaction is carried out at 105-120°C for 4-6h. After the reaction is completed, the reaction solution is poured into anhydrous ethanol, filtered and dried to prepare modified carbon nanotubes.

[0007] Preferably, in step (2), the mass ratio of N,N-diisopropylcarbodiimide, 1-hydroxybenzotriazole, oxidized carbon nanotubes and triethylenetetramine is 0.02-0.05: 0.02-0.04: 1: 0.5-0.7.

[0008] Preferably, in step (4), the mass ratio of the functionalized carbon nanotubes, 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid, 4-dimethylaminopyridine and 1-ethyl-3(3-dimethylpropylamine)carbodiimide is 1-3:5-8:0.2-0.8:4-7.

[0009] Preferably, the preparation method of the water-swelling agent comprises the following steps: In an ice water bath, use a sodium hydroxide solution with a mass fraction of 20-30% to pre-neutralize acrylic acid until the neutralization degree reaches 65-75%, then add potassium persulfate to mix, and obtain a mixed solution; put carboxymethyl cellulose and deionized water in a reactor, place it at 55-65°C and stir for 0.5-1h, cool to room temperature after the carboxymethyl cellulose is dissolved, add the obtained mixed solution and stir for 0.5-1h to obtain solution 1; take bentonite and ultrasonically disperse it in deionized water, then add N, N'-methylenebisacrylamide and mix evenly to obtain solution 2; stir and mix solution 1 and solution 2, raise the temperature to 65-80°C in a nitrogen atmosphere to react for 3-4h, and after the reaction is completed, dry and crush to prepare a water-absorbing expansion agent.

[0010] Preferably, the mass ratio of the acrylic acid, potassium persulfate, N,N'-methylenebisacrylamide and bentonite is 10-12: 0.04-0.07: 0.01-0.05: 0.8-1.5.

[0011] Preferably, the base oil is one or a combination of hydrogenated white oil and paraffin rubber oil.

[0012] Preferably, the oil separation inhibitor is a high molecular polymer synthetic rubber.

[0013] A method for preparing the optical cable water-blocking filling grease as described above comprises the following steps: S1. Weigh each raw material by weight, add the oil separation inhibitor to the base oil, stir at 100-170° C. for 3-6 hours to obtain a mixed solution; S2. Add modified carbon nanotubes to the mixed solution, stir at 120-200°C for 0.5-1.5h, then add water-absorbing swelling agent and stir at this temperature for 0.5-1h. Grind homogenously, degas in vacuum and filter to obtain the optical cable water-blocking filling paste.

[0014] Beneficial effects of the present invention: The present invention utilizes concentrated nitric acid to oxidize carbon nanotubes, so that the surface of the carbon nanotubes is rich in hydroxyl groups and carboxyl groups, and then the carboxyl groups on the surface of the oxidized carbon nanotubes are subjected to an amidation reaction with triethylenetetramine to prepare amino carbon nanotubes, and then some amino groups on the surface of the amino carbon nanotubes are subjected to a ring-opening reaction with epoxy groups in the structure of glycidyl methacrylate to prepare functionalized carbon nanotubes with double bond groups introduced into the structure, and the remaining amino groups on the surface of the amino carbon nanotubes can react with Ca in the bacterial outer membrane. 2+ or Mg 2+The present invention relates to a novel nanotube having a water-blocking effect, destroying the stability of the cell membrane, thereby improving the antibacterial property of the optical cable water-blocking filling ointment. At the same time, due to the presence of the amino group, the performance of the carbon nanotube is more stable. Then, the hydroxyl group on the surface of the functionalized carbon nanotube is further reacted with the carboxyl group in the structure of 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid, thereby introducing the antioxidant 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid into the structure of the carbon nanotube to prepare an antioxidant carbon nanotube. Finally, the antioxidant carbon nanotube is polymerized with N-phenylmaleimide. The obtained modified carbon nanotube contains two rigid groups, imide and benzene ring, which hinder the movement and rotation of the molecular chain, and are beneficial to improving the aging resistance of the optical cable water-blocking filling ointment. At the same time, the problem of easy volatilization, migration and extraction of the antioxidant during processing or long-term use is avoided, and the prepared modified carbon nanotube has good dispersibility and strong interface bonding force.

[0015] The present invention uses carboxymethyl cellulose as a skeleton, N, N'-methylenebisacrylamide as a cross-linking agent, potassium persulfate as an initiator, adopts an aqueous solution polymerization method to graft polyacrylic acid, and is compounded with bentonite to prepare a water-absorbing swelling agent. Bentonite has a porous structure and a large specific surface area. After the polypropylene monomer enters, grafting and cross-linking occur. The hydroxyl groups on the surface of the bentonite form a large number of hydrogen bonds with the polyacrylic acid to form a physical cross-linking network, making the three-dimensional network structure more perfect, which is conducive to improving the water absorption and water locking capacity. The surface of the bentonite has a large number of hydrophilic groups, which can generate hydrogen bonds, van der Waals forces and other interactions with water molecules, and use the three-dimensional network structure to bind water molecules, making it difficult to break free, thereby reducing the volatilization rate of water molecules. When water or moisture enters the optical cable, the filling ointment can quickly absorb water and swell, blocking the water seepage channel and the damaged point, so that the water cannot flow, and the water-blocking gel formed by the filling ointment in contact with water has high viscosity and long-term stability, thereby achieving the purpose of water blocking. DETAILED DESCRIPTION

[0016] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0017] In the examples and comparative examples of the present invention, the hydrogenated white oil was purchased from Hengshui Diyi Petrochemical Co., Ltd.; the high molecular polymer synthetic rubber was purchased from polyisobutylene BP2400 produced by Guangzhou Caixin Trading Co., Ltd.

[0018] Example 1 A method for preparing modified carbon nanotubes comprises the following steps: (1) 1.2 g of carbon nanotubes were placed in a reactor, 100 mL of 65% concentrated nitric acid was added, and the mixture was stirred and mixed. The mixture was refluxed at 110 °C for 6 h. After the reaction was completed, the mixture was filtered, washed, and dried to prepare oxidized carbon nanotubes. (2) 0.02 g of N, N-diisopropylcarbodiimide, 0.02 g of 1-hydroxybenzotriazole and 1 g of oxidized carbon nanotubes were placed in a reactor, 100 mL of N, N-dimethylformamide was added for ultrasonic dispersion, and then 0.5 g of triethylenetetramine was added for stirring and reaction for 24 h. After the reaction was completed, the mixture was filtered, washed and dried to obtain amino carbon nanotubes. (3) 1 g of amino-modified carbon nanotubes was ultrasonically dispersed in 100 mL of N,N-dimethylformamide, and then 2.4 g of glycidyl methacrylate was added and reacted at 105 °C for 4 h. After the reaction was completed, the functionalized carbon nanotubes were prepared by filtering, washing, and drying. (4) 1.2 g of functionalized carbon nanotubes were ultrasonically dispersed in 100 mL of dichloromethane to obtain a dispersion, 5.6 g of 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid and 0.3 g of 4-dimethylaminopyridine were placed in a reactor, 40 mL of dichloromethane was added, and the mixture was stirred at 0°C for 20 min in a nitrogen atmosphere. Then 4.1 g of 1-ethyl-3 (3-dimethylpropylamine) carbodiimide was dissolved in 40 mL of dichloromethane and added to the reactor. The mixture was stirred for 2 h to obtain a reaction solution. The dispersion and the reaction solution were stirred and reacted in a nitrogen atmosphere for 24 h. After the reaction was completed, the mixture was filtered, washed, and dried to obtain antioxidant carbon nanotubes. (5) Take 1 g of antioxidant carbon nanotubes and 0.7 g of N-phenylmaleimide and put them into a reactor filled with 100 mL of xylene solvent and disperse them evenly. Heat the mixture to 80 °C in a nitrogen atmosphere and react for 1 h. Then add 0.03 g of azobisisobutyronitrile and react at 110 °C for 5 h. After the reaction is completed, pour the reaction solution into anhydrous ethanol, filter and dry to prepare modified carbon nanotubes.

[0019] Example 2 A method for preparing a water-absorbing swelling agent comprises the following steps: In an ice water bath, 12 g of acrylic acid was pre-neutralized with a 25% sodium hydroxide solution to a neutralization degree of 70%, and then 0.05 g of potassium persulfate was added to mix to obtain a mixed solution. 1 g of carboxymethyl cellulose and 30 mL of deionized water were placed in a reactor and stirred at 65° C. for 1 h. After the carboxymethyl cellulose was dissolved, the mixture was cooled to room temperature and added with the obtained mixed solution and stirred for 0.5 h to obtain solution 1. 1.2 g of bentonite was ultrasonically dispersed in 75 mL of deionized water, and then 0.03 g of N, N'-methylenebisacrylamide was added and mixed evenly to obtain solution 2. Solution 1 and solution 2 were stirred and mixed, and the temperature was raised to 75° C. in a nitrogen atmosphere for reaction for 4 h. After the reaction was completed, the water-absorbing expansion agent was prepared by drying and crushing.

[0020] Example 3 An optical cable water-blocking filling paste comprises the following components in parts by weight: 72 parts of base oil, 5 parts of oil separation inhibitor, 8 parts of modified carbon nanotubes prepared in Example 1, and 7 parts of water-absorbing swelling agent prepared in Example 2, wherein the base oil is hydrogenated white oil, and the oil separation inhibitor is polyisobutylene BP2400.

[0021] The preparation method of the above-mentioned optical cable water-blocking filling grease comprises the following steps: S1. Weigh each raw material by weight, add the oil separation inhibitor to the base oil, stir at 150° C. for 4 hours to obtain a mixed solution; S2. Add modified carbon nanotubes to the mixed solution, stir at 185°C for 1 hour, then add a water-absorbing swelling agent and stir at this temperature for 0.5 hour. Grind homogenously, degas in vacuum, and filter to prepare an optical cable water-blocking filling paste.

[0022] Example 4 A water-blocking filling paste for optical cables comprises the following components in parts by weight: 77 parts of base oil, 8 parts of oil separation inhibitor, 12 parts of modified carbon nanotubes prepared in Example 1, and 10 parts of water-absorbing swelling agent prepared in Example 2, wherein the base oil is hydrogenated white oil, and the oil separation inhibitor is polyisobutylene BP2400.

[0023] The preparation method of the above optical cable water-blocking filling grease is the same as that of Example 3.

[0024] Example 5 A water-blocking filling paste for optical cables comprises the following components in parts by weight: 84 parts of base oil, 10 parts of oil separation inhibitor, 15 parts of modified carbon nanotubes prepared in Example 1, and 12 parts of water-absorbing swelling agent prepared in Example 2, wherein the base oil is hydrogenated white oil, and the oil separation inhibitor is polyisobutylene BP2400.

[0025] The preparation method of the above optical cable water-blocking filling grease is the same as that of Example 3.

[0026] Comparative Example 1 An optical cable water-blocking filling paste comprises the following components in parts by weight: 84 parts of base oil, 10 parts of oil separation inhibitor, 15 parts of carbon nanotubes, and 12 parts of the water-absorbing swelling agent prepared in Example 2, wherein the base oil is hydrogenated white oil, and the oil separation inhibitor is polyisobutylene BP2400.

[0027] The preparation method of the above optical cable water-blocking filling grease is the same as that of Example 3.

[0028] Comparative Example 1 An optical cable water-blocking filling paste comprises the following components in parts by weight: 84 parts of base oil, 10 parts of oil separation inhibitor, 15 parts of modified carbon nanotubes prepared in Example 1, and 12 parts of polyacrylic acid, wherein the base oil is hydrogenated white oil, and the oil separation inhibitor is polyisobutylene BP2400.

[0029] The preparation method of the above optical cable water-blocking filling grease is the same as that of Example 3.

[0030] Performance Testing The ointments prepared in Examples 3-5 and Comparative Examples 1-2 were subjected to performance tests: Aging resistance test: The ointments prepared in Examples 3-5 and Comparative Examples 1-2 were aged in an oven at 80°C, and a small portion was taken out every 24 hours. After cooling in a dryer, the water absorption time of the ointment was tested, and the data results were shown in Table 1; the ointments prepared in Examples 3-5 and Comparative Examples 1-2 were placed in an oven and aged at 100°C, 150°C, 180°C, and 200°C, respectively. After 10 minutes, they were taken out and cooled in a dryer. The water absorption time of the ointment was tested, and the data results were shown in Table 2; Antibacterial performance test: 9.6×10 5 The total number of CFU of bacteria was recorded once every 7 days for a total of 21 days, and the data results are shown in Table 3.

[0031] Table 1 Test results of long-term aging performance of samples at 80℃

[0032] It can be seen from the data in Table 1 that the ointments prepared in Examples 3-5 of the present invention have excellent water absorption and aging resistance. In Comparative Example 1, the carbon nanotubes were not modified, and it was measured that after aging at 80°C, the water absorption time increased significantly with the extension of the aging time, indicating that the modification of the carbon nanotubes can improve the aging resistance of the ointment. In Comparative Example 2, the water absorption swelling agent was replaced with polyacrylic acid in equal amount, and the measured water absorption time was increased compared with Examples 3-5, indicating that the addition of the water absorption swelling agent can reduce the water absorption time of the ointment.

[0033] Table 2 Test results of aging performance of samples at different temperatures for 10 min

[0034] From the data in Table 2, it can be seen that the ointments prepared in Examples 3-5 of the present invention have excellent aging resistance at high temperatures and no oil precipitation. In Comparative Example 1, the water absorption time increased significantly with the increase of aging temperature, the ointment became thinner and oil precipitated on the surface. The reason is that the carbon nanotubes were not modified, resulting in a sharp decrease in their water absorption capacity at high temperatures.

[0035] Table 3 Test results of antibacterial properties of samples

[0036] It can be seen from the data in Table 3 that the ointments prepared in Examples 3-5 of the present invention have excellent antibacterial effects. The antibacterial effect of Comparative Example 1 is worse than that of Examples 3-5 because the presence of amino cations in the modified carbon nanotubes can improve the antibacterial properties of the ointment.

[0037] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0038] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.

Claims

1. An optical cable water-blocking filling grease, characterized in that: The invention comprises the following components by weight: 70-85 parts of base oil, 5-10 parts of oil separation inhibitor, 8-15 parts of modified carbon nanotubes, and 7-12 parts of water absorption swelling agent; The modified carbon nanotubes are prepared by treating oxidized carbon nanotubes with triethylenetetramine, grafting glycidyl methacrylate, further grafting with antioxidant 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid, and polymerizing with N-phenylmaleimide; the water-absorbing swelling agent is prepared by using carboxymethyl cellulose as a skeleton, grafting polyacrylic acid by aqueous solution polymerization, and compounding with bentonite.

2. The optical cable water blocking filling grease according to claim 1, characterized in that: The preparation method of the modified carbon nanotubes comprises the following steps: (1) Place carbon nanotubes in a reactor, add concentrated nitric acid with a mass fraction of 65-68%, stir and mix, place at 105-110° C. for reflux reaction for 4-8 hours, and after the reaction is completed, filter, wash and dry to prepare oxidized carbon nanotubes; (2) N, N-diisopropylcarbodiimide, 1-hydroxybenzotriazole and oxidized carbon nanotubes are placed in a reactor, N, N-dimethylformamide is added for ultrasonic dispersion, and then triethylenetetramine is added for stirring and reaction for 20 to 24 hours. After the reaction is completed, the mixture is filtered, washed and dried to obtain amino carbon nanotubes; (3) ultrasonically dispersing the amino carbon nanotubes in N,N-dimethylformamide, then adding glycidyl methacrylate, and reacting at 90-110°C for 3-4 hours. After the reaction is completed, filtering, washing, and drying to prepare functionalized carbon nanotubes; (4) ultrasonically dispersing the functionalized carbon nanotubes in dichloromethane to obtain a dispersion, placing 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid and 4-dimethylaminopyridine in a reactor, adding dichloromethane, stirring for 10-25 min at 0-4 °C in a nitrogen atmosphere, then dissolving 1-ethyl-3 (3-dimethylpropylamine) carbodiimide in dichloromethane and adding the mixture to the reactor, stirring for 2-3 h to obtain a reaction solution, stirring the dispersion and the reaction solution in a nitrogen atmosphere for 18-24 h, filtering, washing, and drying after the reaction is completed to obtain antioxidant carbon nanotubes; (5) Antioxidant carbon nanotubes and N-phenylmaleimide are placed in a reactor filled with xylene solvent and dispersed evenly. The temperature is raised to 70-85°C in a nitrogen atmosphere and the reaction is carried out for 0.5-1h. Then, azobisisobutyronitrile is added and the reaction is carried out at 105-120°C for 4-6h. After the reaction is completed, the reaction solution is poured into anhydrous ethanol, filtered and dried to prepare modified carbon nanotubes.

3. The optical cable water blocking filling grease according to claim 2, characterized in that: In the step (2), the mass ratio of N,N-diisopropylcarbodiimide, 1-hydroxybenzotriazole, oxidized carbon nanotubes and triethylenetetramine is 0.02-0.05: 0.02-0.04: 1: 0.5-0.

7.

4. The optical cable water blocking filling grease according to claim 2, characterized in that: In the step (4), the mass ratio of the functionalized carbon nanotubes, 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid, 4-dimethylaminopyridine and 1-ethyl-3(3-dimethylpropylamine)carbodiimide is 1-3:5-8:0.2-0.8:4-7.

5. The optical cable water blocking filling grease according to claim 1, characterized in that: The preparation method of the water-swelling agent comprises the following steps: In an ice water bath, use a sodium hydroxide solution with a mass fraction of 20-30% to pre-neutralize acrylic acid until the neutralization degree reaches 65-75%, then add potassium persulfate to mix, and obtain a mixed solution; put carboxymethyl cellulose and deionized water in a reactor, place it at 55-65°C and stir for 0.5-1h, cool to room temperature after the carboxymethyl cellulose is dissolved, add the obtained mixed solution and stir for 0.5-1h to obtain solution 1; take bentonite and ultrasonically disperse it in deionized water, then add N, N'-methylenebisacrylamide and mix evenly to obtain solution 2; stir and mix solution 1 and solution 2, raise the temperature to 65-80°C in a nitrogen atmosphere to react for 3-4h, and after the reaction is completed, dry and crush to prepare a water-absorbing expansion agent.

6. The optical cable water blocking filling grease according to claim 5, characterized in that: The mass ratio of the acrylic acid, potassium persulfate, N,N'-methylenebisacrylamide and bentonite is 10-12: 0.04-0.07: 0.01-0.05: 0.8-1.

5.

7. The optical cable water blocking filling grease according to claim 1, characterized in that: The base oil is one of hydrogenated white oil and paraffin rubber oil or a combination of both.

8. The optical cable water blocking filling grease according to claim 1, characterized in that: The oil separation inhibitor is a high molecular polymer synthetic rubber.

9. A method for preparing the optical cable water blocking filling grease according to claims 1 to 8, characterized in that: The following steps are involved: S1. Weigh each raw material by weight, add the oil separation inhibitor to the base oil, stir at 100-170° C. for 3-6 hours to obtain a mixed solution; S2. Add modified carbon nanotubes to the mixed solution, stir at 120-200°C for 0.5-1.5h, then add water-absorbing swelling agent and stir at this temperature for 0.5-1h. Grind homogenously, degas in vacuum and filter to obtain the optical cable water-blocking filling paste.

Citation Information

Patent Citations

  • Formula of hydrogen absorption type fiber paste and manufacture method thereof

    CN102660351A

  • Super absorbent expansion water blocking paste and preparation method thereof

    CN106398845A

  • Optical fiber filling paste with ultralow loss for optical fiber and preparation method thereof

    CN111808431A

  • Preparation method of polymer modified bentonite

    CN112744823A

  • Shield tail sealing grease for shield tunneling machine

    CN114410366A

Cited By

  • Molded wire stranded high-insulation power cable and preparation method thereof

    CN120319531A

  • A type of stranded high-insulation power cable and its preparation method

    CN120319531B