Composite material, composite solid electrolyte membrane and preparation method and application thereof
By combining inorganic solid electrolytes with fluorine-containing organic lithium salts and adding binders and fluorine-containing polymers, the ionic conductivity and mechanical strength of the composite solid electrolyte membrane are improved, solving the problem of poor performance of existing electrolyte membranes and achieving better performance. Efficient lithium-ion transfer and better battery performance.
Patent Information
- Application Number
- CN202410228057.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-28
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-02-28
AI Technical Summary
Existing organic-inorganic composite solid-state electrolyte membranes have poor performance. Low lithium ion conductivity and high interface resistance inhibit the development of all-solid-state batteries.
A combination of an inorganic solid electrolyte and a fluorine-containing organic lithium salt is used to improve the dissociation ability of lithium ions through the coating layer, and a binder and fluoropolymer are added to the composite material to improve the ion transmission performance of the electrolyte membrane.
The ionic conductivity and mechanical strength of the composite solid electrolyte membrane are improved, the interface impedance is reduced, and the overall performance of the electrolyte membrane is enhanced.
Smart Images

Figure CN118040024B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a composite material, a method for preparing a composite material, a composite solid electrolyte membrane, a method for preparing a composite solid electrolyte membrane, and a lithium-ion battery. Background Art
[0002] The safety performance of traditional liquid electrolytes is one of the major bottlenecks restricting the development of lithium-ion batteries. Compared with traditional liquid electrolytes, solid-state electrolytes not only reduce the risk of combustion and potential side reactions with electrodes, but also retain the excellent adhesion and film-forming properties of polymers. In addition, solid-state electrolyte membranes can inhibit the growth of lithium dendrites, further ensuring battery safety during charge and discharge. However, the low lithium-ion conductivity and large interfacial resistance of solid-state electrolytes have severely hindered the development of all-solid-state batteries.
[0003] Inorganic solid electrolytes have high interfacial resistance and uneven current density distribution at the interface. LLZO and cathode materials can undergo side reactions at high temperatures or under electrochemical conditions. The accumulation of byproducts at the interface can impair the battery's cycling performance. Organic-inorganic composite solid thin film electrolytes have attracted attention because they combine the advantages of both organic and inorganic materials. However, the performance of existing organic-inorganic composite solid electrolyte membranes is poor and needs further improvement. Summary of the Invention
[0004] In view of this, the present application provides a composite solid electrolyte membrane, aiming to improve the problem of poor performance of existing organic-inorganic composite solid electrolyte membranes.
[0005] The embodiment of the present application is implemented as follows: a composite material includes an inorganic solid electrolyte and a coating layer covering the inorganic solid electrolyte, wherein the material of the coating layer includes a fluorine-containing organic lithium salt.
[0006] Optionally, in some embodiments of the present application, the inorganic solid electrolyte includes LLZO powder; and / or
[0007] The fluorine-containing organic lithium salt includes one or more of lithium trifluoroacetate, lithium perfluorobutyrate, lithium perfluoropentanoate, lithium perfluorohexanoate, lithium perfluoroheptanoate, lithium perfluorooctanoate, lithium hexafluorophosphate, and lithium trifluoromethanesulfonate.
[0008] Optionally, in some embodiments of the present application, in the composite material, the mass fraction of the fluorine-containing organic lithium salt is 0.1% to 1%; and / or
[0009] The average particle size of the inorganic solid electrolyte is 300nm to 2000nm; and / or
[0010] The coating layer has a thickness of 2 nm to 10 nm; and / or
[0011] The LLZO powder includes one or more doped or undoped LLZO powders.
[0012] Optionally, in some embodiments of the present application, the doping elements in the doped LLZO powder include one or more of Al, Ta, Nb, and Ga; and / or
[0013] The molar mass fraction of the doping element in the doped LLZO powder is 0.1% to 1%.
[0014] Accordingly, an embodiment of the present application further provides a method for preparing a composite material, comprising:
[0015] Providing an inorganic solid electrolyte and a fluorine-containing organic acid, wherein the surface of the inorganic solid electrolyte contains lithium carbonate, and mixing the inorganic solid electrolyte and the fluorine-containing organic acid to obtain a mixture;
[0016] The mixture is subjected to a first grinding to obtain a composite material.
[0017] Optionally, in some embodiments of the present application, the mass ratio of the inorganic solid electrolyte to the fluorine-containing organic acid is 90:(2-6); and / or
[0018] The fluorine-containing organic acid includes one or more of trifluoroacetic acid, perfluorobutyric acid, perfluoropentanoic acid, perfluorohexanoic acid, perfluoroheptanoic acid, perfluorooctanoic acid, hexafluorophosphoric acid, and trifluoromethanesulfonic acid.
[0019] Optionally, in some embodiments of the present application, the first grinding speed is
[0020] 5000 rpm to 20000 rpm; and / or
[0021] The first grinding time is 10 min to 60 min.
[0022] Correspondingly, an embodiment of the present application further provides a composite solid electrolyte membrane, which includes the composite material, or includes the composite material prepared by the preparation method.
[0023] Optionally, in some embodiments of the present application, the composite solid electrolyte membrane further comprises an adhesive and a fluorine-containing polymer; and / or
[0024] The thickness of the composite solid electrolyte membrane is 20 μm to 60 μm.
[0025] Optionally, in some embodiments of the present application, the mass ratio of the composite material, the adhesive and the fluoropolymer is (80-99): (0.5-10): (0.3-10); and / or
[0026] The adhesive comprises polytetrafluoroethylene; and / or
[0027] The fluorine-containing polymer includes one or more of polyvinylidene fluoride and polyvinylidene fluoride-hexafluoropropylene copolymer.
[0028] Accordingly, an embodiment of the present application further provides a method for preparing a composite solid electrolyte membrane, comprising:
[0029] Providing an adhesive, a fluorine-containing polymer and the composite material, mixing them, and performing a second grinding to obtain a composite electrolyte flocculent mixture;
[0030] The composite electrolyte flocculent mixture is pressed to obtain a composite solid electrolyte membrane.
[0031] Optionally, in some embodiments of the present application, the second grinding speed is
[0032] 5000 rpm to 20000 rpm; and / or
[0033] The second grinding time is 10 min to 60 min.
[0034] Correspondingly, an embodiment of the present application further provides a battery, which includes a positive electrode, a negative electrode, an electrolyte and the composite solid electrolyte membrane, or the composite solid electrolyte membrane prepared by the preparation method described above.
[0035] In the composite material provided by this application, the fluorine-containing organic lithium salt has a weaker bond to lithium ions due to the group steric effect of fluorine atoms, thus allowing for easier dissociation of lithium ions. The composite material of this application is applied to a composite solid electrolyte membrane. Due to the presence of the fluorine-containing organic lithium salt, which is an organic substance, close contact with the organic electrolyte is promoted, reducing interfacial impedance. In addition, because the composite material can easily dissociate lithium ions, ion transport at the interface between the inorganic electrolyte and the organic electrolyte is improved, thereby improving the ionic conductivity of the entire electrolyte membrane. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.
[0037] Figure 1 This is a flow chart of a method for preparing a composite material provided in an embodiment of the present application;
[0038] Figure 2 This is a flow chart of a method for preparing a composite solid electrolyte membrane provided in an embodiment of the present application;
[0039] Figure 3 This is a TEM image of the coated LLZO powder provided in Example 7 of the present application;
[0040] Figure 4 This is the XRD pattern of LLZO powder before and after coating provided in Example 7 of the present application. DETAILED DESCRIPTION
[0041] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work are within the scope of protection of this application. In addition, it should be understood that the specific embodiments described herein are only used to illustrate and explain the present application and are not used to limit the present application.
[0042] In this application, unless otherwise indicated, directional terms such as "upper" and "lower" generally refer to the upper and lower positions of a device in actual use or operation, specifically in the drawing directions of the accompanying drawings; whereas "inner" and "outer" refer to the outline of the device. Furthermore, in the description of this application, the term "including" means "including but not limited to." Terms such as first, second, and third are used merely as designations and do not impose numerical requirements or establish a sequential order.
[0043] In this application, "and / or" describes the association relationship between associated objects, indicating that three relationships can exist. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural.
[0044] In this application, "at least one" means one or more, and "plurality" means two or more. "One or several", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple.
[0045] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity and should not be understood as a hard limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numbers within the range. For example, the description of a range from 1 to 6 should be considered to have specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which applies regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0046] Currently, conventional organic-inorganic composite solid electrolyte membrane technologies primarily include wet and dry processes. The wet process uses an organic solvent to dissolve a polymer, then adds a small amount of inorganic solid electrolyte, stirs and disperses it evenly, coats it on a substrate, and dries the resulting organic-inorganic composite solid electrolyte membrane. Existing wet processes for preparing composite electrolyte membranes use organic solvents, which are harmful to humans and the environment. They also require pulping, coating, and drying, resulting in complex, energy-intensive, and inefficient processes. Dry-processed composite electrolyte membranes suffer from uneven inorganic electrolyte distribution and poor interface contact with the polymer, leading to poor membrane performance.
[0047] The technical solution of this application is as follows:
[0048] In a first aspect, an embodiment of the present application provides a composite material, comprising an inorganic solid electrolyte and a coating layer coating the inorganic solid electrolyte, wherein the coating layer comprises a fluorine-containing organic lithium salt.
[0049] In this application, the fluorine-containing organic lithium salt has a weaker binding force on lithium ions due to the steric effect of the fluorine atoms, allowing the lithium ions to be dissociated more easily. The composite material of this application is applied to a composite solid electrolyte membrane. Due to the presence of the fluorine-containing organic lithium salt, which is an organic substance, it promotes close contact with the organic electrolyte and reduces the interfacial impedance. In addition, because the composite material can easily dissociate lithium ions, the ion transport at the interface between the inorganic electrolyte and the organic electrolyte is improved, thereby improving the ionic conductivity of the entire electrolyte membrane.
[0050] In some embodiments, the inorganic solid electrolyte includes LLZO powder.
[0051] In some embodiments, the average particle size of the inorganic solid electrolyte is 300nm to 2000nm, for example, 300nm, 320nm, 350nm, 400nm, 430nm, 450nm, 500nm, 520nm, 550nm, 600nm, 630nm, 650nm, 700nm, 750nm, 780nm, 800nm, 820nm, 850nm, 880nm, 900nm, 920nm, 950nm m, 980nm, 1000nm, 1100nm, 1150nm, 1200nm, 1250nm, 1300nm, 1350nm, 1400nm, 1450nm, 1500nm, 1550nm, 1600nm, 1650nm, 1700nm, 1750nm, 1800nm, 1850nm, 1900nm, 1950nm, 2000nm, etc., within the range of the average particle size, is conducive to coating.
[0052] In some embodiments, in the composite material, the mass fraction of the fluorine-containing organic lithium salt is 0.1% to 1%, for example, it can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, etc. Within the range of the mass fraction, it is beneficial for the coating layer to completely cover the inorganic solid electrolyte core.
[0053] In some embodiments, the thickness of the coating layer is 2 nm to 10 nm, for example, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, etc. Within the thickness range, the composite material has good conductivity.
[0054] In some embodiments, the LLZO powder includes one or more of doped or undoped LLZO powders.
[0055] Furthermore, the doping elements in the doped LLZO powder include one or more of Al, Ta, Nb, and Ga.
[0056] Furthermore, the molar mass fraction of the doping element in the doped LLZO powder is 0.1% to 1%, for example, it can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, etc. Within the mass fraction range, it is beneficial to improve the ionic conductivity of the composite electrolyte membrane.
[0057] In some embodiments, the fluorine-containing organic lithium salt includes one or more of lithium trifluoroacetate, lithium perfluorobutyrate, lithium perfluoropentanoate, lithium perfluorohexanoate, lithium perfluoroheptanoate, lithium perfluorooctanoate, lithium hexafluorophosphate, and lithium trifluoromethanesulfonate.
[0058] Second, see Figure 1 , the present application also provides a method for preparing a composite material, comprising:
[0059] S01. Providing an inorganic solid electrolyte and a fluorine-containing organic acid, wherein the surface of the inorganic solid electrolyte contains lithium carbonate, and mixing the inorganic solid electrolyte and the fluorine-containing organic acid to obtain a mixture;
[0060] S02. Performing a first grinding on the mixture to obtain a composite material.
[0061] In the preparation method of the composite material of the present application, an inorganic solid electrolyte will form an inert lithium carbonate impurity layer when exposed to the air for a long time. The low lithium conductivity of lithium carbonate will greatly hinder the transmission of lithium ions between the organic electrolyte and the inorganic solid electrolyte, making the ionic conductivity of the composite electrolyte very low. The present application creatively uses fluorine-containing organic acids to treat inorganic solid electrolytes. The carboxylic acid groups in the fluorine-containing organic acids react with carbonate ions to generate corresponding fluorine-containing carboxylic acid lithium salts, carbon dioxide and water. During grinding and stirring, the surface of the inorganic solid electrolyte can be fully contacted with the fluorine-containing organic carboxylic acid, and the reaction generates a fluorine-containing carboxylic acid lithium salt coating layer. The heat generated during high-speed stirring causes the carbon dioxide and water to volatilize, so that the reaction coating layer is a fluorine-containing carboxylic acid lithium salt.
[0062] The material, average particle size, coating layer thickness, etc. of the inorganic solid electrolyte are as described above and will not be described in detail here.
[0063] In some embodiments, the mass ratio of the inorganic solid electrolyte to the fluorine-containing organic acid is 90:(2-6), for example, it can be 90:2, 90:2.2, 90:2.5, 90:2.8, 90:3, 90:3.2, 90:3.4, 90:3.6, 90:3.8, 90:4, 90:4.2, 90:4.5, 90:4.8, 90:5, 90:5.2, 90:5.5, 90:5.8, 90:6, etc. Within the mass ratio range, it is beneficial for the fluorine-containing organic acid to completely react with the lithium carbonate impurity layer on the surface of the inorganic solid electrolyte.
[0064] In some embodiments, the fluorine-containing organic acid includes one or more of trifluoroacetic acid, perfluorobutyric acid, perfluoropentanoic acid, perfluorohexanoic acid, perfluoroheptanoic acid, perfluorooctanoic acid, hexafluorophosphoric acid, and trifluoromethanesulfonic acid.
[0065] In some embodiments, the first grinding speed is 5000 rpm to 20000 rpm. For example, it can be 5000 rpm, 5500 rpm, 5800 rpm, 6000 rpm, 6200 rpm, 6500 rpm, 6800 rpm, 7000 rpm, 7500 rpm, 8000 rpm, 8500 rpm, 9000 rpm, 9500 rpm, 10000 rpm, 11000 rpm, 12000 rpm, 13000 rpm, 14000 rpm, 15000 rpm, 16000 rpm, 17000 rpm, 18000 rpm, 19000 rpm. , 20000rpm, etc., and the time is 10min~60min, for example, it can be 10min, 12min, 15min, 16min, 18min, 20min, 22min, 25min, 28min, 30min, 32min, 35min, 38min, 40min, 42min, 45min, 48min, 50min, 53min, 56min, 58min, 60min, etc. Within the range of the rotation speed and time, the surface of the inorganic solid electrolyte can be fully contacted with the fluorine-containing organic acid.
[0066] In a third aspect, an embodiment of the present application further provides a composite solid electrolyte membrane, which includes the composite material described in the first aspect, or includes the composite material prepared by the preparation method described in the second aspect.
[0067] In some embodiments, the composite solid electrolyte membrane further includes a binder and a fluorine-containing polymer.
[0068] Furthermore, the adhesive includes polytetrafluoroethylene (PTFE).
[0069] Furthermore, the fluorine-containing polymer includes one or more of polyvinylidene fluoride (PVDF) and polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP).
[0070] In some embodiments, the mass ratio of the composite material, the adhesive and the fluoropolymer is (80-99):(0.5-10):(0.3-10), for example, 80:0.5:0.3, 80:0.5:0.8, 80:0.5:1, 80:0.5:2, 80:0.5:3, 80:0.5:4, 80:0.5:5, 80:0.5:6 、80:0.5:7、80:0.5:8、80:0.5:9、80:0.5:10、85:0.5:0.3、85:1:0.8、85:1:2、85:2:3、85:4:5、85:5:6、85:6:7、85:7:8、85:8:9、85:9:10、90:0.5:0.3、90:0.8:0.5、90: 1:0.8、90:2:1、90:3:2、90:4:3、90:5:4、90:6:5、90:7:6、90:8:7、90:9:8、90:10:9、95:0.5:0.3、95:0.6:0.4、95:0.8:0.6、95:1:0.8、95:2:1、95:3:2、95:4:3、95:5:5、 95:6:7, 95:8:9, 95:9:10, 99:0.5:0.3, 99:0.6:0.4, 99:0.8:0.6, 99:1:1, 99:2:3, 99:4:5, 99:7:10, 99:10:1, 99:9:2, 99:10:10, etc. Within the mass ratio range, ultra-high ionic conductivity and good mechanical strength can be obtained.
[0071] In some embodiments, the thickness of the composite solid electrolyte membrane is 20μm to 60μm, for example, it can be 20μm, 22μm, 25μm, 28μm, 30μm, 32μm, 35μm, 38μm, 40μm, 42μm, 45μm, 48μm, 50μm, 52μm, 55μm, 58μm, 60μm, etc.
[0072] For the fourth aspect, please refer to Figure 2 , the present application also provides a method for preparing a composite solid electrolyte membrane, comprising:
[0073] S1. Providing an adhesive, a fluorine-containing polymer, and the composite material, mixing them, and performing a second grinding to obtain a composite electrolyte flocculent mixture;
[0074] S2. Pressing the composite electrolyte flocculent mixture to obtain a composite solid electrolyte membrane.
[0075] The materials of the adhesive and the fluoropolymer, as well as the mass ratio of the adhesive, the fluoropolymer and the composite material are as described above and will not be elaborated here.
[0076] In S1:
[0077] In some embodiments, the second grinding speed is 5000 rpm to 20000 rpm. For example, it can be 5000 rpm, 5500 rpm, 5800 rpm, 6000 rpm, 6200 rpm, 6500 rpm, 6800 rpm, 7000 rpm, 7500 rpm, 8000 rpm, 8500 rpm, 9000 rpm, 9500 rpm, 10000 rpm, 11000 rpm, 12000 rpm, 13000 rpm, 14000 rpm, 15000 rpm, 16000 rpm, 17000 rpm, The rotation speed and time range are 18000 rpm, 19000 rpm, 20000 rpm, etc., and the time is 10 min to 60 min, for example, 10 min, 12 min, 15 min, 16 min, 18 min, 20 min, 22 min, 25 min, 28 min, 30 min, 32 min, 35 min, 38 min, 40 min, 42 min, 45 min, 48 min, 50 min, 53 min, 56 min, 58 min, 60 min, etc. Within the rotation speed and time range, the adhesive, the fluoropolymer and the above-mentioned composite material are facilitated to fully contact and extrude, thereby obtaining a composite electrolyte flocculent mixture.
[0078] In S2:
[0079] The pressing method comprises: placing the composite electrolyte flocculent mixture on a double-roller mill at 60-100° C. and pressing the mixture to obtain a composite solid electrolyte membrane.
[0080] The lithium carbonate in the prior art is an inorganic lithium salt, which has poor compatibility with organic electrolytes. The composite solid electrolyte membrane of the present application, in which the fluorine-containing organic lithium salt generated by the in-situ reaction is an organic substance, thus greatly improving the compatibility between the inorganic solid electrolyte and the fluorine-containing polymer. Therefore, the composite solid electrolyte membrane of the present invention has excellent mechanical properties. Lithium carbonate usually dissociates into lithium ions in solution. Fluorine-containing organic lithium salts have a weaker binding on lithium ions due to the larger group steric effect, and thus can more easily dissociate into lithium ions, thereby greatly improving the ion transport at the interface. Therefore, the ionic conductivity of the composite solid electrolyte membrane of the present invention is improved. The above two advantages improve the performance of the electrolyte membrane manufactured by the present invention.
[0081] In a fifth aspect, an embodiment of the present application further provides a battery comprising a positive electrode, a negative electrode, an electrolyte and the composite solid electrolyte membrane described in the third aspect above, or the composite solid electrolyte membrane prepared by the preparation method described in the fourth aspect above.
[0082] The present application will be described in detail below through specific examples. The following examples are only some examples of the present application and are not limitations of the present application.
[0083] Example 1
[0084] This embodiment provides a composite material, and the preparation method is as follows:
[0085] 0.9 g of Ga-doped LLZO powder and 0.02 g of trifluoroacetic acid were added to a high-speed grinder and ground at 5000 rpm for 30 minutes to obtain Ga-LLZO powder coated with lithium trifluoroacetate, i.e., a composite material.
[0086] This embodiment also provides a composite solid electrolyte membrane, the preparation method of which is as follows:
[0087] 0.02 g PTFE and 0.06 g PVDF were added to the above-mentioned Ga-LLZO powder coated with lithium trifluoroacetate, and the mixture was milled again at 5000 rpm for 30 minutes to obtain a composite electrolyte flocculent mixture;
[0088] The composite electrolyte flocculent mixture was repeatedly rolled on a double-roller mill at 80° C. and thinned to 50 μm to obtain a composite solid electrolyte membrane.
[0089] Example 2
[0090] This embodiment is basically the same as embodiment 1, except that Ga-LLZO powder is replaced with Ta-LLZO.
[0091] Example 3
[0092] This embodiment is substantially the same as embodiment 1, except that trifluoroacetic acid is replaced with perfluoropentanoic acid.
[0093] Example 4
[0094] This embodiment is substantially the same as embodiment 1, except that trifluoroacetic acid is replaced with perfluorooctanoic acid.
[0095] Example 5
[0096] This embodiment is substantially the same as embodiment 1, except that trifluoroacetic acid is replaced by hexafluorophosphoric acid.
[0097] Example 6
[0098] This embodiment is substantially the same as Example 1, except that trifluoroacetic acid is replaced by trifluoromethanesulfonic acid.
[0099] Example 7
[0100] This embodiment is substantially the same as embodiment 6, except that the content of trifluoromethanesulfonic acid in embodiment 6 is increased from 0.02 g to 0.04 g, and the content of PVDF is changed from 0.06 g to 0.04 g, while the rest remain unchanged.
[0101] The final composite electrolyte membrane of Example 7 contains: 0.932 g of Ga-LLZO coated with lithium trifluoromethanesulfonate, 0.06 g of PVDF and 0.02 g of PTFE.
[0102] Example 8
[0103] This example is substantially the same as Example 1, except that the content of trifluoromethanesulfonic acid in Example 6 is increased from 0.02 g to 0.06 g, and the content of PVDF is changed from 0.06 g to 0.02 g, while the rest remain unchanged.
[0104] Example 9
[0105] This embodiment is substantially the same as embodiment 1, with the only difference being that Ga-LLZO powder is replaced with Nb-LLZO.
[0106] Example 10
[0107] This embodiment is basically the same as embodiment 1, with the only difference being that Ga-LLZO powder is replaced with Al-Ga-LLZO.
[0108] Example 11
[0109] This embodiment is basically the same as Example 1, except that the content of Ga-LLZO powder in Example 1 is replaced by 0.9 g, the content of trifluoroacetic acid is replaced by 0.04 g, the content of PTFE is replaced by 0.005 g, and the content of PVDF is replaced by 0.003 g.
[0110] Example 12
[0111] This embodiment is basically the same as Example 1, except that the content of Ga-LLZO powder in Example 1 is replaced by 0.9 g, the content of trifluoroacetic acid is replaced by 0.06 g, the content of PTFE is replaced by 0.1 g, and the content of PVDF is replaced by 0.1 g.
[0112] Comparative Example 1
[0113] 0.9g of Ga-LLZO powder and 0.04g of trifluoromethanesulfonic acid were added to DMF solvent and stirred at 1000 rpm for 30 minutes. 0.06g of PVDF was added and stirred again for 4 hours to obtain an electrolyte slurry. The electrolyte slurry was coated on a PET substrate and dried at 80°C for 8 hours to obtain a wet-process composite electrolyte membrane.
[0114] Comparative Example 2
[0115] 0.9g of Ga-LLZO powder and 0.04g of lithium triflate were added to a high-speed grinder and milled at 5000 rpm for 30 minutes. 0.02g of PTFE and 0.04g of PVDF were then added and milled again at 5000 rpm for 30 minutes. The resulting mixture was repeatedly rolled on an open mill at 80°C, thinning the mixture to 50μm.
[0116] Comparative Example 3
[0117] The difference between this comparative example and Example 7 is that the trifluoromethanesulfonic acid in Example 7 is replaced by hydrochloric acid.
[0118] The Ga-LLZO powder coated with lithium trifluoromethanesulfonate in Example 7 was tested by transmission electron microscopy, and the TEM image of the coated LLZO powder was obtained as shown in FIG. Figure 3 As shown. Figure 3 It can be seen that the surface of Ga-LLZO powder is evenly coated with lithium trifluoromethanesulfonate.
[0119] Figure 4 The XRD patterns of LLZO powder before and after coating in Example 7 are shown in Figure 2. Figure 4 It can be seen that the lithium carbonate impurity peak appears before coating, and disappears after coating, indicating that the lithium carbonate on the surface of LLZO powder has been completely reacted after coating.
[0120] The film forming performance, ionic conductivity and tensile strength of the composite electrolyte membranes of Examples 1 to 12 and Comparative Examples 1 to 3 were tested respectively. The test results are shown in Table 1.
[0121] Table 1
[0122]
[0123]
[0124] From Table 1 we can see that:
[0125] The wet method of Comparative Example 1 failed to form a film, while the dry methods of Examples 1 to 12 and Comparative Examples 2 and 3 all formed films well.
[0126] Compared with the composite electrolyte membrane of Comparative Example 3, the composite solid electrolyte membranes of Examples 1 to 12 all have higher ionic conductivities than Comparative Example 3. This is because the fluorinated organic lithium salt has a larger group steric effect, which weakens the binding of lithium ions and allows for easier dissociation of lithium ions, thereby significantly improving ion transfer at the interface and thus improving ionic conductivity. The tensile strength of the composite solid electrolyte membranes of Examples 1 to 12 is all higher than that of Comparative Example 3. This is because the fluorinated organic lithium salt is a fluorinated organic lithium salt, which significantly improves the compatibility between LLZO and the fluorinated polymer in the composite solid electrolyte membrane, thereby increasing the tensile strength.
[0127] In Comparative Example 2, directly adding lithium trifluoromethanesulfonate did not significantly improve the performance of the electrolyte membrane.
[0128] The above is a detailed introduction to the light-emitting device, preparation method, and display device provided in the embodiments of the present application. Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method and core idea of the present application. At the same time, for those skilled in the art, based on the ideas of the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.
Claims
1. A composite material, characterized in that: The composite material comprises an inorganic solid electrolyte and a coating layer covering the inorganic solid electrolyte, wherein the material of the coating layer comprises a fluorine-containing organic lithium salt; The inorganic solid electrolyte includes LLZO powder; The preparation method of the composite material comprises: Providing an inorganic solid electrolyte and a fluorine-containing organic acid, wherein the surface of the inorganic solid electrolyte contains lithium carbonate, and mixing the inorganic solid electrolyte and the fluorine-containing organic acid to obtain a mixture; The mixture is subjected to a first grinding to obtain a composite material.
2. The composite material according to claim 1, characterized in that The fluorine-containing organic lithium salt includes one or more of lithium trifluoroacetate, lithium perfluorobutyrate, lithium perfluoropentanoate, lithium perfluorohexanoate, lithium perfluoroheptanoate, lithium perfluorooctanoate, lithium hexafluorophosphate, and lithium trifluoromethanesulfonate.
3. The composite material according to claim 2, characterized in that In the composite material, the mass fraction of the fluorine-containing organic lithium salt is 0.1% to 1%; and / or The average particle size of the inorganic solid electrolyte is 300nm to 2000nm; and / or The coating layer has a thickness of 2 nm to 10 nm; and / or The LLZO powder includes one or more of doped or undoped LLZO powders.
4. The composite material according to claim 3, characterized in that The doping elements in the doped LLZO powder include one or more of Al, Ta, Nb, and Ga; and / or The molar mass fraction of the doping element in the doped LLZO powder is 0.1% to 1%.
5. A method for preparing a composite material, characterized in that: include: Providing an inorganic solid electrolyte and a fluorine-containing organic acid, wherein the surface of the inorganic solid electrolyte contains lithium carbonate, and mixing the inorganic solid electrolyte and the fluorine-containing organic acid to obtain a mixture; performing a first grinding on the mixture to obtain a composite material; Wherein, the inorganic solid electrolyte includes LLZO powder.
6. The preparation method according to claim 5, characterized in that: The mass ratio of the inorganic solid electrolyte to the fluorine-containing organic acid is 90:(2-6); and / or The fluorine-containing organic acid includes one or more of trifluoroacetic acid, perfluorobutyric acid, perfluoropentanoic acid, perfluorohexanoic acid, perfluoroheptanoic acid, perfluorooctanoic acid, hexafluorophosphoric acid, and trifluoromethanesulfonic acid.
7. The preparation method according to claim 5, characterized in that: The first grinding speed is 5000 rpm to 20000 rpm; and / or The first grinding time is 10 min to 60 min.
8. A composite solid electrolyte membrane, characterized in that: The composite solid electrolyte membrane comprises the composite material according to any one of claims 1 to 4, or comprises a composite material prepared by the preparation method according to any one of claims 5 to 7.
9. The composite solid electrolyte membrane according to claim 8, characterized in that: The composite solid electrolyte membrane further includes an adhesive and a fluorine-containing polymer; and / or The thickness of the composite solid electrolyte membrane is 20 μm to 60 μm.
10. The composite solid electrolyte membrane according to claim 9, characterized in that: The mass ratio of the composite material, the adhesive and the fluorine-containing polymer is (80-99):(0.5-10):(0.3-10); and / or The adhesive comprises polytetrafluoroethylene; and / or The fluorine-containing polymer includes one or more of polyvinylidene fluoride and polyvinylidene fluoride-hexafluoropropylene copolymer.
11. The method for preparing a composite solid electrolyte membrane according to any one of claims 8 to 10, characterized in that: include: Providing a binder, a fluorine-containing polymer and the composite material, mixing them, and performing a second grinding to obtain a composite electrolyte flocculent mixture; The composite electrolyte flocculent mixture is pressed to obtain a composite solid electrolyte membrane.
12. The preparation method according to claim 11, characterized in that: The second grinding speed is 5000 rpm to 20000 rpm; and / or The second grinding time is 10 min to 60 min.
13. A battery, characterized in that: The battery comprises a positive electrode, a negative electrode, an electrolyte and a composite solid electrolyte membrane as described in any one of claims 8 to 10, or a composite solid electrolyte membrane prepared by the preparation method as described in any one of claims 11 to 12.