Preparation method of heat-treatment-free die-cast aluminum-silicon alloy material and die-casting method
By adding specific components and steps to the aluminum-silicon alloy material, a high-strength tough aluminum-silicon alloy material suitable for integrated die-casting is prepared, which solves the problem of insufficient material strength and toughness under heat-free conditions in the prior art, and achieves thin walls and thickness Both the wall parts and the cost reduction.
Patent Information
- Application Number
- CN202410129730.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-31
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-01-31
AI Technical Summary
The prior art is difficult to provide large integrated die castings with high-strength tough aluminum-silicon alloy materials suitable for both thin and thick wall parts under heat-free conditions, and the cost is high and cannot meet the requirements of integrated die casting.
Using low-ferrous aluminum ingots, low-ferrous metal silicon, preheated manganese additives, titanium additives and metal magnesium, and adding preheated aluminum strontium intermediate alloys and new TCB seed alloys, and preparing through specific casting and degassing steps A near eutectic aluminum-silicon alloy material with excellent fluidity and comprehensive mechanical properties is produced.
It realizes a high-strength and low-cost aluminum-silicon alloy material with both thin and thick walls under heat-free conditions, which is suitable for large-scale integrated die castings, improving the performance and production efficiency of the material.
Smart Images

Figure BDA0004689452480000101 
Figure BDA0004689452480000111
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of die-cast aluminum alloys, and in particular relates to a preparation method and a die-casting method of a heat-treatment-free die-cast aluminum-silicon alloy material. Background Art
[0002] With the advent of Tesla's integrated die-casting technology, my country's die-casting industry will face huge challenges and changes. Traditional automobile manufacturing usually connects dozens or hundreds of small parts into a large component by welding or riveting, while integrated die-casting technology can integrate the above small parts into 1 to 2 parts through a large-tonnage die-casting machine, which not only shortens the manufacturing time and simplifies the production process, but also improves the product's precision, improves the utilization rate of raw materials, and most importantly, reduces production costs. The maturity and mass production of integrated die-casting technology have brought challenges and opportunities to the aluminum alloy material industry. Previously, each component was independently die-casted, and the size and wall thickness of the product were convenient for heat treatment to achieve the performance indicators required by the product. However, the size of large integrated die-castings has increased by dozens or hundreds of times, and the wall thickness is thin in some places and thick in some places, which is no longer suitable for heat treatment. The reason is that heat treatment can easily cause deformation of large die-castings, increase the difficulty of subsequent shaping, thereby increasing the scrap rate of die-castings and increasing manufacturing costs. Therefore, the first material required for integrated die-casting is to meet the requirements of heat treatment exemption.
[0003] At present, research on aluminum alloys that do not require heat treatment has also been conducted at home and abroad, and some results have been achieved. However, the research breakthroughs of these heat-treatment-free materials are mainly concentrated on hypoeutectic aluminum-silicon alloys. For example, CN114293058A discloses a method for preparing a high-strength and toughness heat-treatment-free material, and CN114438380A discloses a heat-treatment-free high-toughness AlSi aluminum alloy and its preparation method, both of which are studies on heat-treatment-free hypoeutectic aluminum-silicon alloys. However, the fluidity and die-casting performance of hypoeutectic aluminum-silicon alloys are average, which are not as good as the die-casting performance of near-eutectic and eutectic aluminum-silicon alloys, and it is difficult to meet the requirements of large-scale integrated die-casting.
[0004] In order to better meet the requirements of integrated die-casting, there are some studies on near-eutectic aluminum-silicon alloys with good fluidity and die-casting properties in the prior art. However, although the near-eutectic aluminum-silicon alloy has good fluidity and die-casting properties, its comprehensive mechanical properties are not as good as those of hypoeutectic aluminum-silicon alloys. At present, some schemes are to improve its mechanical properties by adding precious metals or using vacuum die-casting conditions, but this scheme greatly increases the cost of preparation, and the improvement of mechanical properties is limited, and it cannot meet the current requirements of achieving high strength and toughness (tensile strength ≥ 260MPa, yield strength ≥ 120MPa, elongation ≥ 10%) without going through a heat treatment process. For example, patent CN 115679162A provides a new energy vehicle heat-treatment-free aluminum alloy material and a low-carbon preparation method, which has good fluidity and die-casting properties, belongs to high-strength properties, and has an elongation of 5%. Its elongation does not reach 10%, which does not belong to the performance range of high strength and toughness. And it adds precious metals such as nickel, vanadium, and beryllium, and its production cost cannot be reduced.
[0005] In addition, the performance of die-cast parts will be different due to the different thicknesses. The mechanical properties of die-cast thin-walled parts are higher than those of die-cast thick-walled parts. Therefore, it is not easy to obtain good mechanical properties for thick-walled die-cast parts with near-eutectic aluminum-silicon alloys. Castasil 37, a high-strength and tough aluminum-silicon alloy that does not require heat treatment, has been announced by the German company Ryan. For die-cast parts with a wall thickness of 2-3 mm, the tensile strength is 260-300 MPa, the yield strength is 120-150 MPa, and the elongation is 10-14% in the state without heat treatment. For die-cast parts with a wall thickness of 5-7 mm, the tensile strength is 200-250 MPa, the yield strength is 80-110 MPa, and the elongation is 10-14% in the state without heat treatment. The high strength and toughness requirements cannot be met in thick-walled die-cast parts. Germany's Ryan Company also announced a heat-treatment-free, high-strength and tough aluminum-magnesium alloy Magsimal-59. For die-castings with a wall thickness of 2-4 mm, the alloy has a tensile strength of 310-340 MPa, a yield strength of 160-220 MPa, and an elongation of 12-18% in a heat-free state. For die-castings with a wall thickness of 6-12 mm, the tensile strength is 220-260 MPa, the yield strength is 120-145 MPa, and the elongation is 8-12% in a heat-free state, which cannot meet the high strength and toughness requirements in thick-walled die-castings. For another example, patent application No. 202111516888.0 provides a treatment-free aluminum alloy and a preparation method thereof, which is a near-eutectic aluminum-silicon alloy, but it requires vacuum die-casting conditions and is relatively costly. Moreover, this scheme can only achieve good mechanical properties for thin-walled parts of 2-3 mm, and cannot meet the requirement that thicker walls can still have good mechanical properties. In large integrated die castings, there are both thin-walled parts and thick-walled parts, all of which are required to meet high strength and toughness requirements at the same time.
[0006] In summary, it is very difficult to obtain a near-eutectic aluminum-silicon alloy that can achieve high strength and toughness in both thin-walled and thick-walled die-casting parts without heat treatment and at low cost. Summary of the invention
[0007] In view of the deficiencies in the prior art, the present invention provides a method for preparing a heat-treatment-free die-cast aluminum-silicon alloy material and a die-casting method.
[0008] The present invention provides a method for preparing a heat treatment-free die-cast aluminum-silicon alloy material, comprising the following steps:
[0009] Adding low-iron aluminum ingot, low-iron metal silicon, preheated manganese additive, titanium additive and metal magnesium;
[0010] Add the preheated aluminum-strontium master alloy and check that the metal composition meets the following conditions: by mass percentage, Si: 9.6-11.8%; Fe: ≤0.15%; Cu: ≤0.03%; Mn: 0.3-0.8%; Mg: 0-0.2%; Zn: ≤0.05%; Ti: 0-0.15%; Zr: 0-0.25%; rare earth 0-0.2%; Sr: 0.01-0.05%; Pb: ≤0.1%; Sn: ≤0.01%; Cd: ≤0.01%, and the rest is Al;
[0011] A TCB seed alloy is added, wherein the TCB seed alloy comprises, by mass percentage, Ti: 4.5-5.5%, C: 0.1-0.2%, B: 0.15-0.25%, Ce: 0.4-0.6%, Mn: ≤0.1%, Fe: ≤0.4%, Si: ≤0.1%, V: ≤0.1%, and the balance is Al.
[0012] The aluminum liquid temperature is cast between 700±10℃.
[0013] Preferably, the inspection metal components meet the conditions that the Mg content is 0.0075-0.2%; and the Zr content is 0.0003-0.25%.
[0014] Preferably, the rare earth includes Ce and La, wherein the Ce content is 0.0012-0.1%; and the La content is 0.0003-0.1%.
[0015] Preferably, when the aluminum liquid temperature is 720-760° C., the preheated TCB seed alloy is added, melted, stirred evenly, and then left alone for 5-10 minutes.
[0016] Preferably, the specific step of adding the preheated aluminum-strontium master alloy is: when the aluminum liquid temperature is 720-760° C., add the preheated aluminum-strontium master alloy, stir slightly to evenly melt, and leave it alone for 20-30 minutes.
[0017] Preferably, the method further comprises the step of adding an aluminum-zirconium master alloy before adding the metal magnesium.
[0018] Preferably, the specific steps of adding low-iron aluminum ingot, low-iron metal silicon, preheated manganese additive, titanium additive and metal magnesium are:
[0019] S11, after adding 85-90% low-iron aluminum ingot and low-iron metal silicon, start melting and heat to 800-850°C, leave it for 30-40 minutes; remove the surface scum for the first time;
[0020] S12. When the temperature is 800-850℃, add half of the preheated manganese additive, stir and melt, and then leave it for 10-20 minutes;
[0021] S13, add the remaining preheated manganese additive and titanium additive, stir and melt, and then leave for 10-20 minutes.
[0022] S14, when the temperature is 800-850°C, add aluminum-zirconium master alloy, stir and melt, and then leave for 10-20 minutes, take samples to check the composition, and if the composition is qualified, proceed to the next step;
[0023] S15, add the remaining aluminum ingots, adjust the aluminum liquid temperature to 740-760℃, and remove the surface slag for the second time;
[0024] S16, using argon or nitrogen as the carrier gas, adding a refining agent in an amount of 0.1-0.2% of the total amount of the aluminum liquid, performing refining and purification, and removing the surface slag for the third time;
[0025] S17, add the preheated magnesium metal, melt and stir evenly, let stand for 5-10 minutes, take samples to check the composition, if the composition is qualified, proceed to the next step;
[0026] S18, aluminum liquid temperature is 720-760℃, use argon or nitrogen to degas for 20-30 minutes, then remove the slag, and check the pinholes to meet the level 1 requirement.
[0027] Preferably, during the casting process, argon or nitrogen is used to pass through a gas-permeable brick with a pore size of 15-25 μm at the bottom of the filter box or flow channel for online degassing, and it is ensured that the pinhole is not higher than level 2.
[0028] Preferably, after adding the TCB seed alloy, the step of degassing the aluminum melt with argon or nitrogen is also included before casting. During degassing, the tumbling height of the aluminum liquid is no more than 15 cm, and the gas pressure is between 0.1-0.2 MPa.
[0029] The present invention also provides a die-casting method for a heat-treatment-free die-cast aluminum-silicon alloy material. The heat-treatment-free die-cast aluminum-silicon alloy material is prepared by the above-mentioned preparation method. Before die-casting, the aluminum melt is degassed with argon or nitrogen for 20-30 minutes, and the slag is removed after degassing.
[0030] The temperature of the aluminum melt remelted before die-casting of the aluminum-silicon alloy material is ≤760°C; during die-casting, the temperature of the die-casting aluminum liquid is controlled at 700±15°C, and the temperature of the die-casting mold is controlled at 200±10°C.
[0031] The aluminum-silicon alloy material prepared by the method for preparing the heat-treatment-free die-casting aluminum-silicon alloy material provided by the present invention has the advantages of no heat treatment, high strength and toughness, and low cost. DETAILED DESCRIPTION
[0032] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0033] The embodiment of the present invention provides a near-eutectic die-casting aluminum-silicon alloy material that does not require heat treatment. The aluminum-silicon alloy material includes, by mass percentage, Si: 9.6-11.8%; Fe: ≤0.15%; Cu: ≤0.03%; Mn: 0.3-0.8%; Mg: 0-0.2%; Zn: ≤0.05%; Ti: 0-0.15%; Zr: 0-0.25%; Ce: 0-0.1%; La: 0-0.1%; Sr: 0.01-0.05%; Pb: ≤0.1%; Sn: ≤0.01%; Cd: ≤0.01%; 0.05%-0.5% of seed, the rest is Al, the seed is a TCB seed, and other unavoidable and common impurity elements are individually ≤0.05%, and the total impurities are ≤0.15%.
[0034] The heat-treatment-free near-eutectic die-casting aluminum-silicon alloy material provided by the present invention belongs to the near-eutectic aluminum-silicon alloy, and the alloy has excellent castability and fluidity. The heat-treatment-free die-casting aluminum alloy of the present invention achieves the advantages of good fluidity, die-casting performance, good comprehensive mechanical properties and low cost. Among the heat-treatment-free die-casting aluminum alloy materials in the prior art, when the comprehensive mechanical properties are similar to those of the present invention, its fluidity and die-casting performance are not as good as those of the present invention; when it has similar fluidity and die-casting performance to those of the present invention, its comprehensive mechanical properties are not as good as those of the present invention; when it has similar mechanical properties, fluidity and die-casting performance to those of the present invention, its production cost is higher than that of the present invention.
[0035] The heat-treatment-free near-eutectic die-casting aluminum-silicon alloy material provided by the present invention is suitable for large-scale integrated die-casting parts and has the advantages of heat-treatment-free, high strength and toughness, and low cost.
[0036] The heat-treatment-free near-eutectic die-casting aluminum-silicon alloy material provided by the present invention has low contents of iron, copper and zinc, thereby ensuring excellent mechanical properties of the material; at the same time, it also has excellent corrosion resistance; in order to reduce the adverse effects of Fe on the plasticity of the alloy, the Fe content is controlled within a relatively low range in the present invention, and then the Fe content is increased to replace Fe, thereby solving the die sticking problem of the alloy during die casting; a certain amount of manganese is added, which can not only solve the metal mold sticking problem that is easy to occur during die casting of the alloy, but also improve the morphology of the iron-rich phase and improve the plasticity of the casting; in addition, adding Mn to the near-eutectic Al-Si alloy can also improve the hot cracking tendency of the casting.
[0037] Magnesium is a strengthening element in alloys. An appropriate amount of magnesium content can increase the yield strength of the material, but magnesium also has a negative impact on reducing its toughness, increasing the brittleness of the material, and the thermal stability of the mechanical properties in the cast state.
[0038] The role of trace Zr is to form Al3Zr with Al, refine the grains, and significantly improve the thermal stability of the die casting.
[0039] The heat treatment-free near-eutectic die-casting aluminum-silicon alloy material provided by the present invention uses a seed crystal as a constraint condition.
[0040] When using seed as a constraint, the microalloying of Zr and the new TCB seed suitable for near-eutectic form are used, which makes the alloy have a good grain refinement effect and good thermal stability and toughness. By combining TCB seed with Zr, the zirconium poisoning phenomenon in the alloy can be eliminated, so that its thermal stability can be more fully exerted. This unique new TCB seed alloy can play a good role in increasing heterogeneous nucleation cores to refine the α-Al phase in near-eutectic aluminum-silicon alloys. The refinement effect is very good, long-lasting and non-fading, the pre-crystallization structure is small, and the grain size of the structure is fine, which plays a role in improving the comprehensive performance of near-eutectic aluminum-silicon alloys. In addition, B in the seed alloy exists in the form of a compound, which is different from the aluminum-boron master alloy, so after adding this TCB seed, it can also coexist with strontium, and there will be no conflict between boron and strontium.
[0041] The heat-treatment-free near-eutectic die-casting aluminum-silicon alloy material provided by the present invention uses Zr microalloying and a new TCB seed suitable for near-eutectic type for microalloying and grain refinement, which results in good grain refinement of the alloy and good thermal stability and toughness.
[0042] In a preferred embodiment, Mg is 0.0075-0.2%; Zr is 0.0003-0.25%; Ce is 0.0012-0.1%; and La is 0.0003-0.1%.
[0043] In a preferred embodiment, the TCB seed crystal includes, by mass percentage, Ti: 4.5-5.5%, C: 0.1-0.2%, B: 0.15-0.25%, Ce: 0.4-0.6%, Mn: ≤0.1%, Fe: ≤0.4%, Si: ≤0.1%, V: ≤0.1%, and the balance is Al.
[0044] Existing TCB seeds (aluminum-titanium-carbon-boron seed alloys) are mostly suitable for hypoeutectic aluminum-silicon alloys but not for near-eutectic aluminum-silicon alloys. Conventional TCB seeds have a composition of Ti: 1.8-2.2%, C: 0.28-0.35%, B: 0.28-0.35%, Mn: ≤0.1%, Fe: ≤0.3%, Si: ≤0.3%, V: ≤0.1%, and the balance is Al. They are suitable for aluminum-silicon alloys with a silicon content of less than 9.5%. Their refinement effect is seriously degraded for aluminum alloys with a silicon content of more than 9.5%, and they are ineffective for aluminum alloys with a silicon content of 10%. In this embodiment, the TCB seed crystal includes Ti: 4.5-5.5%, C: 0.1-0.2%, B: 0.15-0.25%, Ce: 0.4-0.6%, Mn: ≤0.1%, Fe: ≤0.4%, Si: ≤0.1%, V: ≤0.1%, and the balance is Al. The TCB used in the present invention is a new type of TCB seed crystal, and its component content is different from that of the usual TCB, and can be applied to aluminum alloys with a silicon content as high as 12.5%. It can greatly improve the performance of near-eutectic aluminum-silicon alloys.
[0045] In a preferred embodiment, the near-eutectic die-casting aluminum-silicon alloy material that does not require heat treatment is degassed with argon or nitrogen for 20-30 minutes before die-casting, and the slag is removed after degassing. When the Sr content in the die-cast aluminum melt drops below the lower limit due to burning, aluminum-strontium intermediate alloy needs to be added for adjustment.
[0046] In a preferred embodiment, the temperature of the aluminum melt remelted before die casting of the near-eutectic die-casting aluminum-silicon alloy material that does not require heat treatment is ≤760°C; during die casting, the temperature of the die-casting aluminum liquid is controlled at 700±15°C, and the temperature of the die-casting mold is controlled at 200±10°C.
[0047] The method for preparing a near-eutectic die-casting aluminum-silicon alloy material without heat treatment provided in an embodiment of the present invention comprises the following steps:
[0048] Adding low-iron aluminum ingot, low-iron metal silicon, preheated manganese additive, titanium additive and metal magnesium;
[0049] Add the preheated aluminum-strontium master alloy and check that the metal composition meets the following conditions: by mass percentage, Si: 9.6-11.8%; Fe: ≤0.15%; Cu: ≤0.03%; Mn: 0.3-0.8%; Mg: 0-0.2%; Zn: ≤0.05%; Ti: 0-0.15%; Zr: 0-0.25%; rare earth 0-0.2%; Sr: 0.01-0.05%; Pb: ≤0.1%; Sn: ≤0.01%; Cd: ≤0.01%, and the rest is Al;
[0050] A TCB seed alloy is added, wherein the TCB seed alloy comprises, by mass percentage, Ti: 4.5-5.5%, C: 0.1-0.2%, B: 0.15-0.25%, Ce: 0.4-0.6%, Mn: ≤0.1%, Fe: ≤0.4%, Si: ≤0.1%, V: ≤0.1%, and the balance is Al.
[0051] The aluminum liquid temperature is cast between 700±10℃.
[0052] In a preferred embodiment, the casting process uses argon or nitrogen to pass through a 15-25 μm pore size air-permeable brick at the bottom of the filter box or flow trough for online degassing, and ensure that the pinhole is no higher than level 2;
[0053] Before casting, the aluminum melt is degassed with argon or nitrogen. During degassing, the tumbling height of the aluminum liquid is no more than 15 cm and the gas pressure is between 0.1-0.2 MPa.
[0054] When the preparation method adopts microalloying, the overall preparation method includes the following steps:
[0055] S11, after adding 85-90% low-iron aluminum ingot and low-iron metal silicon, start melting and heat to 800-850°C, leave it for 30-40 minutes; remove the surface scum for the first time;
[0056] S12. When the temperature is 800-850℃, add half of the preheated manganese additive, stir and melt, and then leave it for 10-20 minutes;
[0057] S13, add the remaining preheated manganese additive and titanium additive, stir and melt, and then leave for 10-20 minutes.
[0058] S14, when the temperature is 800-850°C, add aluminum-zirconium master alloy, stir and melt, and then leave for 10-20 minutes, take samples to check the composition, and if the composition is qualified, proceed to the next step;
[0059] S15, add the remaining aluminum ingots, adjust the aluminum liquid temperature to 740-760℃, and remove the surface slag for the second time;
[0060] S16, using argon or nitrogen as the carrier gas, adding a refining agent in an amount of 0.1-0.2% of the total amount of the aluminum liquid, performing refining and purification, and removing the surface slag for the third time;
[0061] S17, add the preheated magnesium metal, melt and stir evenly, let stand for 5-10 minutes, take samples to check the composition, if the composition is qualified, proceed to the next step;
[0062] S18, aluminum liquid temperature is 720-760℃, use argon or nitrogen to degas for 20-30 minutes, then remove slag, and check the pinholes to meet the requirement of level 1;
[0063] S19. When the aluminum liquid temperature is 720-760℃, add the preheated aluminum-strontium master alloy, stir lightly to evenly melt, and leave it for 20-30 minutes;
[0064] S20, when the temperature is 720-760℃, add the preheated new TCB seed alloy suitable for near-eutectic form. Melt and stir evenly, then let stand for 5-10 minutes;
[0065] S21. The aluminum liquid temperature is cast between 700±10℃.
[0066] In order to have a further understanding and recognition of the technical solution of the present invention, several preferred embodiments are listed and described in further detail.
[0067] Example 1
[0068] Calculated by weight percentage: Si: 9.83%; Fe: 0.12%; Cu: 0.0013%; Mn: 0.51%; Mg: 0.0075%; Zn: 0.0195%; Ti: 0.02%; Zr: 0.22%; Ce: 0.0012%; La: 0.0003%; Sr: 0.016%; Pb: 0.00068%; Sn: 0.004%; Cd: 0.0001%; the addition amount of new TCB seed alloy: 0.3%; the common impurity elements are individually ≤0.05%, the total impurity content: 0.11%; the rest is Al.
[0069] The TCB seed alloy includes Ti: 4.5-5.5%, C: 0.1-0.2%, B: 0.15-0.25%, Ce: 0.4-0.6%, Mn: ≤0.1%, Fe: ≤0.4%, Si: ≤0.1%, V: ≤0.1%, and the balance is Al.
[0070] According to the above ratio, the aluminum alloy is prepared in the following steps:
[0071] S11. Clean the furnace bottom and furnace wall to avoid impurities; add 90% low-iron aluminum ingots and low-iron metal silicon, open the fire to melt and heat to 820℃, and leave it for 35 minutes; remove the surface slag for the first time.
[0072] S12. When the temperature reaches 820°C, add half of the preheated manganese additive, stir until melted, and then leave it alone for 15 minutes.
[0073] S13, add the remaining preheated manganese additive and titanium additive, stir and melt, and then leave for 15 minutes.
[0074] S14. When the temperature is 850°C, add aluminum-zirconium master alloy, stir and melt, let stand for 15 minutes, take samples to check the composition, and if the composition is qualified, proceed to the next step.
[0075] S15. Add the remaining aluminum ingots and adjust the aluminum liquid temperature to 750°C. Remove the surface slag for the second time.
[0076] S16, using argon or nitrogen as carrier gas, adding refining agent in an amount of 0.15% of the total amount of aluminum liquid for refining and purification. The surface scum is removed for the third time.
[0077] S17. Add preheated magnesium metal, melt and stir evenly, let stand for 5 minutes, take samples to check the composition, and if the composition is qualified, proceed to the next step.
[0078] S18, aluminum liquid temperature is 740℃, use argon or nitrogen to degas for 25 minutes and then remove slag, check the pinholes to reach level 1.
[0079] S19, when the aluminum liquid temperature is 730℃, add the preheated aluminum-strontium master alloy, stir it slightly to evenly melt it, and leave it for 30 minutes. Take a sample to check the composition, if the composition is qualified, proceed to the next step.
[0080] S20, add the preheated new TCB seed alloy suitable for near-eutectic at 730°C, melt and stir evenly, and then stand for 5 minutes.
[0081] S21. Aluminum liquid is cast at 700℃. During the casting process, nitrogen is used to pass through a 15μm pore size air brick at the bottom of the filter box for online degassing. And the pinhole level 1 is checked.
[0082] illustrate:
[0083] (1) Allow the aluminum liquid to stand for 5-10 minutes before each purification and slag removal.
[0084] (2) When using nitrogen to degas the aluminum melt, the tumbling height of the aluminum liquid is no more than 15 cm and the gas pressure is between 0.1-0.2 MPa.
[0085] The die casting was carried out using the die casting method of Example 2.
[0086] Example 2
[0087] The prepared aluminum alloy material is die-cast into a die-casting part by ordinary high-pressure die-casting according to the following process requirements. The wall thickness of the die-casting part is Φ6.3mm. The die-casting process is as follows:
[0088] (1) The aluminum melt temperature (remelting temperature) before die casting is ≤760℃.
[0089] (2) The die-casting aluminum liquid temperature is 705°C. The thicker the wall thickness, the lower the limit, while the thinner the wall thickness, the upper the limit.
[0090] (3) Die casting mold temperature is 205°C. The wall thickness is on the lower limit, and the wall thickness is on the upper limit.
[0091] (4) Degas the aluminum melt with argon or nitrogen for 20-30 minutes before die casting. Remove the slag after degassing.
[0092] (5) When the Sr content in the die-cast aluminum melt drops below the lower limit due to burnout, it is necessary to add aluminum-strontium intermediate alloy for adjustment.
[0093] (6) During the die-casting process, do not add return materials or other cold materials into the furnace to avoid melt aspiration and increase impurities.
[0094] (7) Iron tools need to be coated and dried to prevent the aluminum melt from increasing iron and absorbing air during the die-casting process.
[0095] Comparative Example 1-Comparative Example 10
[0096] The formulas and material preparation methods of Comparative Examples 1 to 10 are shown in Table 1, and the die-casting methods are the same as those of Example 2.
[0097] Table 1
[0098]
[0099] In the above table, the conventional TCB seed crystal composition is Ti: 1.8-2.2%, C: 0.28-0.35%, B: 0.28-0.35%, Mn: ≤0.1%, Fe: ≤0.3%, Si: ≤0.3%, V: ≤0.1%, and the balance is Al.
[0100] The aluminum alloy materials prepared in Example 1 and Comparative Examples 1-10 were die-casted by the die-casting method of Example 2. The wall thickness of the die-casting was Φ6.3 mm. The die-casting with a wall thickness of Φ6.3 mm was tested in the die-cast state. Alternatively, the die-casting was subjected to a tensile test after baking. The performance in the baked state refers to the performance of the simulated integrated die-casting after high-temperature electrostatic baking. The process parameters of the baking simulation are 190°C and 35 minutes of heat preservation.
[0101] The test results are shown in Table 2.
[0102] Table 2
[0103]
[0104] In summary, the heat-treatment-free die-casting aluminum alloy material provided by the present invention, and the aluminum alloy die-castings prepared under heat-treatment-free conditions, have good strength and toughness, thermal stability, corrosion resistance, die-casting performance and relatively low production cost in both thin-walled and thick-walled parts. The standard test bar die-casting tensile strength: 270-300MPa, yield: 120-145MPa, elongation: 10-16%; the standard test bar baked tensile strength: 275-295MPa, yield: 125-165MPa, elongation: 10-18%. The near-eutectic aluminum-silicon alloy with good flowability and die-casting performance has the advantages of high strength and toughness in both thin-walled and thick-walled die-casting parts, which greatly improves the performance of the integrated die-casting material. The improvement of the front-end material performance provides more possibilities for the development of back-end products.
[0105] The above are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing a near-eutectic aluminum-silicon alloy material that is suitable for large-scale integrated die casting and does not require heat treatment, characterized in that: The steps include: Adding low-iron aluminum ingots, low-iron metal silicon, preheated manganese additives, titanium additives and metal magnesium; before adding the metal magnesium, the process also includes the step of adding an aluminum-zirconium master alloy; Add the preheated aluminum-strontium master alloy and check that the metal composition meets the following conditions: by mass percentage, Si: 9.6-11.8%; Fe: ≤0.15%; Cu: ≤0.03%; Mn: 0.3-0.8%; Mg: 0.0075-0.2%; Zn: ≤0.05%; Ti :0.02-0.15%; Zr: 0.0003-0.25%; Ce: 0.0012-0.1%; La: 0.0003-0.1%; Sr: 0.01-0.05%; Pb: ≤0.1%; Sn: ≤0.01%; Cd: ≤0.01%, the rest is Al; The specific steps of adding the preheated aluminum-strontium master alloy are: when the aluminum liquid temperature is 720-760° C., adding the preheated aluminum-strontium master alloy, slightly stirring to evenly melt, and leaving it alone for 20-30 minutes; When the aluminum liquid temperature is 720-760°C, a preheated TCB seed alloy is added, the amount of the TCB seed alloy added is 0.05%-0.5%, and the mixture is melted and stirred evenly and then left alone for 5-10 minutes. The TCB seed alloy comprises, by mass percentage, Ti: 4.5-5.5%, C: 0.1-0.2%, B: 0.15-0.25%, Ce: 0.4-0.6%, Mn: ≤0.1%, Fe: ≤0.4%, Si: ≤0.1%, V: ≤0.1%, and the balance is Al; The aluminum liquid temperature is cast between 700±10℃.
2. The method for preparing a near-eutectic aluminum-silicon alloy material suitable for large-scale integrated die casting and free of heat treatment as claimed in claim 1, characterized in that: The specific steps of adding low-iron aluminum ingot, low-iron metal silicon, preheated manganese additive, titanium additive and metal magnesium are: S11, after adding 85-90% low-iron aluminum ingot and low-iron metal silicon, start the fire to melt and heat up to 800-850℃, leave it for 30-40 minutes; remove the surface scum for the first time; S12. When the temperature is 800-850℃, add half of the preheated manganese additive, stir and melt, and then leave it for 10-20 minutes; S13, adding the remaining preheated manganese additive and titanium additive, stirring and melting, and then leaving for 10-20 minutes; S14, when the temperature is 800-850°C, add aluminum-zirconium master alloy, stir and melt, and then leave for 10-20 minutes, take samples to check the composition, and if the composition is qualified, proceed to the next step; S15, add the remaining aluminum ingots, adjust the aluminum liquid temperature to 740-760℃, and remove the surface slag for the second time; S16, using argon or nitrogen as the carrier gas, adding a refining agent in an amount of 0.1-0.2% of the total amount of the aluminum liquid, performing refining and purification, and removing the surface scum for the third time; S17, add the preheated magnesium metal, melt and stir evenly, let stand for 5-10 minutes, take samples to check the composition, if the composition is qualified, proceed to the next step; S18, aluminum liquid temperature is 720-760℃, use argon or nitrogen to degas for 20-30 minutes, then remove the slag, and check the pinholes to meet the level 1 requirement.
3. The method for preparing the near-eutectic aluminum-silicon alloy material suitable for large-scale integrated die casting and free of heat treatment as claimed in claim 1, characterized in that: During the casting process, argon or nitrogen is used to pass through a gas-permeable brick with a pore size of 15-25μm at the bottom of the filter box or flow trough for online degassing, and it is ensured that the pinhole is no higher than level 2.
4. The method for preparing a near-eutectic aluminum-silicon alloy material suitable for large-scale integrated die casting and free of heat treatment as claimed in claim 1, characterized in that: After adding the TCB seed alloy, a degassing step using argon or nitrogen is also included before casting. During degassing, the tumbling height of the aluminum liquid is no more than 15 cm, and the gas pressure is between 0.1-0.2 MPa.
5. The method for preparing a near-eutectic aluminum-silicon alloy material suitable for large-scale integrated die casting and free of heat treatment as claimed in claim 1, characterized in that: The aluminum silicon alloy material is degassed with argon or nitrogen for 20-30 minutes before die casting, and the slag is removed after degassing; The temperature of the aluminum melt remelted before die-casting of the aluminum-silicon alloy material is ≤760°C; during die-casting, the temperature of the die-casting aluminum liquid is controlled at 700±15°C, and the temperature of the die-casting mold is controlled at 200±10°C.