A compound, its preparation method, and its application as a solid electrolyte

By preparing Li6-aPS5-aClFa compounds with specific chemical compositions, the problem of instability between sulfide solid electrolytes and metallic lithium was solved, achieving electrochemical stability under high voltage and improving the safety and stability of the battery.

CN118062814BActive Publication Date: 2026-11-17DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211476216.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-23
Publication Date
2026-11-17
Estimated Expiration
2042-11-23

AI Technical Summary

Technical Problem

Existing sulfide solid electrolytes are not stable enough with lithium metal or solid batteries above 4.2V, affecting the safety and stability of the batteries.

Method used

A solid sulfide-based lithium-ion conductor was prepared by using a Li6-aPS5-aClFa compound with a specific chemical composition, through ball milling of raw materials including lithium sulfide, phosphorus pentasulfide, lithium chloride, and lithium fluoride, combined with a specific annealing method, to form a semi-amorphous structure.

Benefits of technology

The stability of the solid electrolyte and lithium metal is improved, enabling electrochemical stability at 4.8V and enhancing the safety and stability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118062814B_ABST
    Figure CN118062814B_ABST
Patent Text Reader

Abstract

This application describes a compound, its preparation method, and its application as a solid electrolyte. A compound, characterized in that the chemical formula of the compound is Li. 6‑a PS 5‑a ClF a Where 0 ≤ a ≤ 2, and a is a rational number; wherein the compound is neutrally charged. This solid-state lithium-ion conductor has a specific chemical composition through crystallization and non-bonded arrangement and / or bonding. Furthermore, this application also relates to a process for preparing such a sulfide-based solid-state lithium-ion conductor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of sulfide solid electrolytes, and particularly to a compound, its preparation method, and its application as a solid electrolyte. Background Technology

[0002] Traditional lithium-ion batteries use liquid electrolytes that are highly flammable. To ensure battery safety, non-flammable, highly safe solid electrolytes are required.

[0003] Solid electrolytes mainly include polymer electrolytes, sulfide electrolytes, oxide electrolytes, and chloride electrolytes. Among them, sulfide electrolytes have high room temperature ionic conductivity, which is 10⁻⁶. -3 Approximately S / cm.

[0004] Although sulfide solid electrolytes have high room temperature ionic conductivity and good interfacial compatibility, current sulfide solid electrolytes are not stable enough in lithium metal batteries or solid batteries operating at 4.2V or higher. Summary of the Invention

[0005] The purpose of this application is to provide a novel solid sulfide-based lithium-ion (Li-ion) battery. + This solid-state ionic electrolyte is a conductor with a specific chemical composition, which is arranged and / or bonded through specific crystalline bonds, amorphous bonds, or combinations thereof. This application also provides these solid sulfide-based Li... + Electrolyte preparation methods, including certain annealing methods.

[0006] Another objective of this application is to provide a novel solid-state sulfide-based lithium-ion (Li... + Methods for preparing conductors. In some embodiments, the specific annealing method described in this application (i.e., the temperature and time of the reaction) affects most of the chemical composition, surface chemical composition, chemical structure (such as bond type and arrangement), crystallinity, stability, and conductivity of these solid sulfide-based lithium-ion conductors, as well as other properties of these solid sulfide-based lithium-ion conductors. In some embodiments, the solid electrolyte conductors described in this application are substantially composed of lithium, phosphorus, sulfur, chlorine, and fluorine. In some of these embodiments, the solid electrolyte conductors described in this application are semi-amorphous.

[0007] According to one aspect of this application, a compound is provided, the chemical formula of which is Li 6-a PS 5-a ClF a ;

[0008] Where 0 ≤ a ≤ 2, and a is a rational number;

[0009] The compound is electrically neutral.

[0010] According to another aspect of this application, a method for preparing the above-mentioned compound is provided, comprising the following steps:

[0011] The raw materials containing lithium sulfide, phosphorus pentasulfide, lithium chloride and lithium fluoride were ball-milled and mixed, and then reacted to obtain the compound.

[0012] The molar ratios of lithium, phosphorus, sulfur, and fluorine in the lithium sulfide, phosphorus pentasulfide, lithium chloride, and lithium fluoride correspond to the atomic ratios in the aforementioned chemical formulas.

[0013] The ball-to-material ratio for ball milling is (5-40):1;

[0014] Optionally, the ball-to-material ratio of the ball milling mixture is any value or a range between 5:1, 10:1, 15:1, 20:1, 25:1, 30:1, 35:1, and 40:1.

[0015] The ball milling speed is 100-600 r / min;

[0016] Optionally, the rotational speed of the ball milling is any value among 100 r / min, 200 r / min, 300 r / min, 400 r / min, 500 r / min, and 600 r / min, or a range between any two.

[0017] The ball milling mixing time is 1 to 40 hours.

[0018] Optionally, the ball milling mixing time is any value among 1h, 5h, 10h, 20h, 30h, and 40h, or a range between any two.

[0019] The reaction temperature is 200–700°C;

[0020] Optionally, the reaction temperature is 400–500°C.

[0021] Optionally, the temperature of the reaction is any value of 400°C, 450°C, 500°C, or a range between any two.

[0022] The reaction time is 1–24 hours;

[0023] Optionally, the reaction time is 2 to 10 hours.

[0024] Optionally, the reaction time is any value among 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, and 10h, or a range between any two.

[0025] The atmosphere in which the reaction takes place is a non-reactive gas atmosphere;

[0026] The inactive gas is selected from at least one of nitrogen, argon, helium, and xenon.

[0027] According to another aspect of this application, a solid electrolyte is provided, said solid electrolyte being selected from the compounds described above or compounds prepared by the methods described above.

[0028] According to another aspect of this application, a lithium secondary battery is provided, wherein the lithium secondary battery uses the above-described solid electrolyte.

[0029] The advantages of this application are:

[0030] This improves the stability of the solid electrolyte and lithium metal, and enables the solid electrolyte to achieve electrochemical stability at 4.8V. Attached Figure Description

[0031] To more clearly illustrate the technical solutions of the embodiments of this application, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of this application and should not be regarded as a limitation of the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.

[0032] Figure 1 The images show the XRD patterns of sulfide solid electrolytes with different fluorine doping contents in Examples 1, 2, 3, and 4 of this application.

[0033] Figure 2 Electrochemical impedance spectroscopy of sulfide solid electrolytes with different fluorine doping contents in Examples 1, 2, and 3 of this application;

[0034] Figure 3 The cycle performance of the all-solid-state battery using a fluorine-doped solid electrolyte in Example 6 of this application is shown. Detailed Implementation

[0035] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions in the embodiments of this application will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.

[0036] The features and performance of this application will be further described in detail below with reference to the embodiments.

[0037] Example 1 Preparation of Li 5.7 PS 4.7 ClF 0.3 The method.

[0038] To prepare Li 5.7 PS 4.7 ClF 0.3 For the ionic conductor, lithium sulfide (Li₂S), phosphorus sulfide (P₂S₅), lithium chloride (LiCl), and lithium fluoride (LiF) were mixed in a molar ratio of 22:5:10:3 into a 100 ml ball mill jar containing 8 mm zirconia grinding beads. The mass ratio of grinding media to the mixture powder was >40. The mixture was stirred in a planetary ball mill at 500 rpm for 30 hours.

[0039] The ball-milled powder was pressed into discs with a diameter of 10 mm under a pressure of 2 t, then placed in a quartz tube and sealed, and annealed at 450°C for 5 hours. The annealing conditions included an argon atmosphere.

[0040] In this embodiment, the powder is loaded into the ball mill jar in an argon-filled glove box.

[0041] Example 2 Preparation of Li 5.5 PS 4.5 ClF 0.5 The method.

[0042] To prepare Li 5.5 PS 4.5 ClF 0.5 For the ionic conductor, lithium sulfide (Li₂S), phosphorus sulfide (P₂S₅), lithium chloride (LiCl), and lithium fluoride (LiF) were mixed in a molar ratio of 4:1:2:1 into a 100 ml ball mill jar containing 8 mm zirconia grinding beads. The mass ratio of grinding media to the mixture powder was >40. The mixture was stirred in a planetary ball mill at 500 rpm for 30 hours.

[0043] The ball-milled powder was pressed into discs with a diameter of 10 mm under a pressure of 2 t, then placed in a quartz tube and sealed, and annealed at 450°C for 5 hours. The annealing conditions included an argon atmosphere.

[0044] In this embodiment, the powder is loaded into the ball mill jar in an argon-filled glove box.

[0045] Example 3 Preparation of Li 5.3 PS 4.5 ClF 0.7 The method.

[0046] To prepare Li 5.3 PS 4.3 ClF 0.7For the ionic conductor, lithium sulfide (Li₂S), phosphorus sulfide (P₂S₅), lithium chloride (LiCl), and lithium fluoride (LiF) were mixed in a molar ratio of 18:5:10:7 into a 100 ml ball mill jar containing 8 mm zirconia grinding beads. The mass ratio of grinding media to the mixture powder was >40. The mixture was stirred in a planetary ball mill at 500 rpm for 30 hours.

[0047] The ball-milled powder was pressed into discs with a diameter of 10 mm under a pressure of 2 t, then placed in a quartz tube and sealed, and annealed at 450°C for 5 hours. The annealing conditions included an argon atmosphere.

[0048] In this embodiment, the powder is loaded into the ball mill jar in an argon-filled glove box.

[0049] Example 4 Preparation of Li 5.1 PS 4.1 ClF 0.9 The method.

[0050] To prepare Li 5.1 PS 4.1 ClF 0.9 For the ionic conductor, lithium sulfide (Li₂S), phosphorus sulfide (P₂S₅), lithium chloride (LiCl), and lithium fluoride (LiF) were mixed in a molar ratio of 16:5:10:9 in a 100 ml ball mill jar containing 8 mm zirconia grinding beads. The mass ratio of grinding media to the mixture powder was >40. The mixture was stirred in a planetary ball mill at 500 rpm for 30 hours.

[0051] The ball-milled powder was pressed into discs with a diameter of 10 mm under a pressure of 2 t, then placed in a quartz tube and sealed, and annealed at 450°C for 5 hours. The annealing conditions included an argon atmosphere.

[0052] In this embodiment, the powder is loaded into the ball mill jar in an argon-filled glove box.

[0053] Example 5Li 6-a PS 5-a ClF a Relationship between crystallinity and fluorine content

[0054] For XRD analysis, the sulfide samples from Examples 1-4 were sealed in Kapton films and measured using a Smartlab X-ray diffractometer. The diffractometer was set to a divergence and scattering slit of 1.25 degrees, a receiving slit of 0.3 mm, and a graphite monochromator equipped with a copper k-α X-ray tube. The samples were scanned at 30 kV, 15 mA, and 10-70 degrees, with a sampling width of 0.020 degrees and a speed of 5 degrees / minute.

[0055] like Figure 1 As shown, the LPSClF material after annealing at 450°C is characterized by reflective X-ray powder diffraction (XRD) patterns at 20, 25, 27, 29, and 45 ± 1° (2θ).

[0056] The conductivity of the solid electrolytes prepared in Examples 1-3 was tested at room temperature, and the conductivity results are as follows: Figure 2 As shown.

[0057] Example 6Li 5.5 PS 4.5 ClF 0.5 How it is used in solid-state batteries.

[0058] The positive electrode was obtained by grinding lithium cobalt oxide and the solid electrolyte from Example 2 at a mass ratio of 7:3. 100 mg Li 5.5 PS 4.5 ClF 0.5 The powder was loaded into a 10mm diameter solid-state battery mold and pressed under 3t pressure. 10mg of the aforementioned positive electrode was then laid flat on one side and pressed under the same 3t pressure. Lithium metal was placed on the other side of the electrolyte, and finally the screws of the solid-state battery mold were tightened. Charge-discharge cycles were performed as follows... Figure 3 As shown.

[0059] In summary, the Li of the embodiments of this application 6-a PS 5-a ClF a The material preparation method can improve the stability with lithium metal and achieve stable cycling of solid-state batteries at a high voltage of 4.6V.

[0060] The above description is merely a few embodiments of this application and is not intended to limit this application in any way. Although this application discloses preferred embodiments as described above, it is not intended to limit this application. Any changes or modifications made by those skilled in the art without departing from the scope of the technical solution of this application using the disclosed technical content are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A compound, characterized in that, The chemical formula of the compound is Li 6-a PS 5-a ClF a ; Where 0 ≤ a ≤ 2, and a is a rational number; The compound is prepared by mixing raw materials containing lithium sulfide, phosphorus pentasulfide, lithium chloride and lithium fluoride in a specific molar ratio, followed by ball milling and heat treatment. X-ray diffraction analysis shows that it has characteristic reflection peaks at 2θ positions of 20°, 25°, 27°, 29° and 45±1°. The heat treatment temperature is 400~500℃; The heat treatment time is 1~24h; The compound is electrically neutral.

2. A method for preparing the compound according to claim 1, characterized in that, Includes the following steps: The raw materials containing lithium sulfide, phosphorus pentasulfide, lithium chloride and lithium fluoride were ball-milled and mixed, and then reacted to obtain the compound.

3. The preparation method according to claim 2, characterized in that, The molar ratios of lithium, phosphorus, sulfur, and fluorine in the lithium sulfide, phosphorus pentasulfide, lithium chloride, and lithium fluoride correspond to the atomic ratios in the chemical formula of claim 1.

4. The preparation method according to claim 2, characterized in that, The ball-to-material ratio for ball milling is (5~40):1; The ball milling speed is 100~600 r / min; The ball milling mixing time is 1~40h.

5. The preparation method according to claim 2, characterized in that, The reaction time is 2 to 10 hours.

6. The preparation method according to claim 2, characterized in that, The atmosphere in which the reaction takes place is a non-reactive gas atmosphere; The inactive gas is selected from at least one of nitrogen, argon, helium, and xenon.

7. A solid electrolyte, characterized in that, The solid electrolyte is selected from the compound described in claim 1 or the compound prepared by the preparation method described in any one of claims 2 to 6.

8. A lithium secondary battery, characterized in that, The lithium secondary battery uses the solid electrolyte described in claim 7.

Citation Information

Patent Citations

  • Sulfide-based compound particles, solid electrolyte, and lithium secondary battery

    CN113428880A

  • Sulfide-based solid electrolyte and power storage element

    JP2022091628A