A special cold rolling oil for galvanized substrate under extreme working conditions

By using nano-silica as a support in cold rolling oil, combined with the structure of p-vinyl benzoic acid and ethylene copolymer, the oil film strength and rolling mill cleanliness are improved, and the failure and failure of existing rolling oil under high temperature and pressure are solved. The problem of insufficient cleaning ability is applicable to extreme rolling conditions of galvanized substrates.

CN118064202BActive Publication Date: 2024-10-29SARK NEW MATERIAL TECH (SHANDONG) CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410197337.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-22
Publication Date
2024-10-29
Estimated Expiration
2044-02-22

AI Technical Summary

Technical Problem

Existing rolling oil is prone to failure due to heat and impact during the rolling process, and its cleaning ability is insufficient, affecting the rolling quality of galvanized sheets.

Method used

It uses nano-silica as the core, p-vinyl benzoic acid and ethylene copolymer as the shell layer, and modified silica bridged with vinyl silane coupling agent as the additive to improve the film strength of cold rolling oil and the cleaning of the rolling mill. It is suitable for rolling of galvanized substrates under extreme working conditions.

Benefits of technology

It significantly improves the lubrication performance of cold rolling oil and the cleanliness of the rolling mill, reduces the generation of sludge, and is suitable for rolling production under high-pressure and high-speed conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118064202B_ABST
    Figure CN118064202B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of rolling oil, specifically a kind of cold rolling oil special for galvanized substrate extreme working condition, comprising by mass percentage: base oil 85-95%, modified silicon dioxide 0.1-2%, emulsifier 1-6%, extreme pressure agent 1-4%, antioxidant 0.1-2%, rust inhibitor 0.1-2%; the modified silicon dioxide is based on nano silicon dioxide as core, p-vinyl benzoic acid and ethylene copolymer as shell layer, and bridged and capped with vinyl silane coupling agent. The cold rolling oil prepared by the present invention has good lubrication and mill cleanliness and annealing cleanliness, and the oil film strength is high, the generation of sludge in the rolling process can be reduced, and the rolling production requirements under high pressure and high speed conditions can be met, so it is suitable for the rolling of galvanized substrate extreme working conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rolling oil, and in particular to a special cold rolling oil for galvanized substrates under extreme working conditions. Background Art

[0002] Galvanized sheet refers to a steel sheet with a layer of zinc on the surface. Usually, the steel sheet is rolled to the target thickness before being galvanized. The quality of galvanizing is closely related to the surface structure of the steel sheet. During the rolling and cold rolling process, heat and friction and wear are easily generated on the surface of the steel sheet. Therefore, reducing the damage to the surface structure during the rolling process of the steel sheet has an important impact on the quality of subsequent galvanizing. Rolling oil can reduce the friction coefficient, reduce heat accumulation, and prevent oxidation, thereby effectively alleviating the structural damage of rolling. However, rolling oil will inevitably remain on the surface of the steel sheet during the rolling process. The iron powder shedding caused by surface friction during rolling will also form sludge that is difficult to disperse with the rolling oil, affecting the rolling quality. After rolling, degreasing is also required to remove the surface to clean it for galvanizing. Therefore, it is of great significance to provide a cold rolling oil with good mill cleanliness and annealing cleanliness.

[0003] Prior art provides a modified nanocellulose for rolling oil and its application (application number CN202310759339.9), the modified nanocellulose for rolling oil is a hydrophobic group modified nanocellulose; the hydrophobic group includes any one or a combination of at least two of fatty acids, fatty acid anhydrides, fatty acid esters, phosphates or silane coupling agents. The nanocellulose of the present invention can form a firm network structure through the hydrogen bond interaction of multiple hydroxyls on the surface of nanocellulose inside the rolling oil film through the modification of hydrophobic groups, thereby effectively enhancing the strength of the lubricating oil film, while the fatty acids, fatty acid anhydrides, phosphates or silane groups introduced by nanocellulose can further enhance the rolling oil boundary and extreme pressure lubrication performance, provide sufficient lubrication in the roll gap area, and greatly reduce the friction during its use. However, nanocellulose is easily damaged by rolling heat and impact during use, resulting in the failure of the corresponding function, and its cleaning ability needs to be further improved. Summary of the invention

[0004] The purpose of the present invention is to provide a special cold rolling oil for galvanized substrates under extreme working conditions, which uses nano-silica as a core, p-vinyl benzoic acid and ethylene copolymer as a shell layer, and is bridged and capped with a vinyl silane coupling agent. The modified silica obtained in this way can improve the oil film strength and rolling mill cleanliness of the cold rolling oil, and is suitable for rolling galvanized substrates under extreme working conditions.

[0005] To achieve the above object, the present invention provides a cold rolling oil for galvanized substrates, which comprises, by mass percentage: 85-95% base oil, 0.1-2% modified silicon dioxide, 1-6% emulsifier, 1-4% extreme pressure agent, 0.1-2% antioxidant, and 0.1-2% rust inhibitor;

[0006] The modified silica is a microsphere with nano-silicon dioxide as the core and the following structural formula as the shell:

[0007]

[0008] Wherein, A1 and A2 are both vinyl silane coupling agents, and A1 is connected to nano-silica, and m and n are positive integers.

[0009] Furthermore, the particle size of the nano-silicon dioxide is 50-150 nm, m is a positive integer of 3-20, and n is a positive integer of 3-10.

[0010] Furthermore, the preparation method of the modified silica includes: using the first batch of vinyltrimethoxysilane to modify nano-silica, then adding p-vinylbenzoic acid, and performing addition polymerization under the action of an initiator, adding ethylene after the reaction is completed to continue addition polymerization under the action of an initiator, and then adding a second batch of vinyltrimethoxysilane to obtain modified silica after polymerization.

[0011] Furthermore, the amount of the first batch of vinyltrimethoxysilane added is 2-15% of the mass of the nano dioxide, the amount of the p-vinylbenzoic acid added is 5-20% of the mass of the nano dioxide, the amount of the ethylene added is 1-8% of the mass of the nano dioxide, the amount of the second batch of vinyltrimethoxysilane added is 2-15% of the mass of the nano dioxide, and the initiator is benzoyl peroxide.

[0012] Further, it includes, by mass percentage: base oil 88-92%, modified silica 0.5-1.8%, emulsifier 2-5%, extreme pressure agent 2-3%, antioxidant 0.5-1%, rust inhibitor 0.5-1%;

[0013] In the modified silicon dioxide, m is a positive integer of 6-15, and n is a positive integer of 5-8.

[0014] Furthermore, the emulsifier is one or more of octylphenol polyoxyethylene ether, sorbitol polyoxyethylene ether, nonylphenol polyoxyethylene ether, hexadecanol polyoxyethylene ether, caprylic acid polyoxyethylene ether, oleic acid polyoxyethylene ether.

[0015] Furthermore, the base oil is one or more of coconut oil, palm oil, oxidized rapeseed oil, pentaerythritol tetraheptyl ester and pentaerythritol tetraoctyl ester.

[0016] Further, the extreme pressure agent is at least one of isooctyl acid phosphate octadecylamine salt, di-n-butyl phosphite, dialkyl dithiocarbamate molybdenum or dialkyl dithiophosphate;

[0017] Furthermore, the rust inhibitor is diethanolamine oleate or triethanolamine oleate; the antioxidant is at least one of 2,6-di-tert-butyl-p-cresol and benzotriazole octadecylamine salt.

[0018] Furthermore, the preparation method of the cold rolling oil for the galvanized substrate includes: mixing the emulsifier and the base oil and heating it to 40-60°C, then adding modified silica and an extreme pressure agent, stirring evenly, adding an antioxidant and a rust inhibitor, stirring evenly at 50-65°C, and cooling to room temperature to discharge.

[0019] The beneficial effects of the present invention are as follows:

[0020] The cold rolling oil for galvanized substrates provided by the present invention has nano silicon dioxide as a core, p-vinyl benzoic acid and ethylene copolymer as a shell layer, and is bridged and capped with a vinyl silane coupling agent. The cold rolling oil is used as an additive for the cold rolling oil. The obtained cold rolling oil has good lubrication and rolling mill cleanliness, and has high oil film strength, can reduce the generation of sludge during rolling, can meet the rolling production requirements under high pressure and high speed conditions, and is therefore suitable for rolling of galvanized substrates under extreme working conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a schematic diagram of the structure of the modified silicon dioxide provided by the present invention. DETAILED DESCRIPTION

[0022] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention is described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] The present invention provides a cold rolling oil for galvanized substrates, which comprises, by mass percentage: 85-95% base oil, 0.1-2% modified silicon dioxide, 1-6% emulsifier, 1-4% extreme pressure agent, 0.1-2% antioxidant, and 0.1-2% rust inhibitor;

[0024] The modified silica is a microsphere with nano-silicon dioxide as the core and the following structural formula as the shell:

[0025]

[0026] Wherein, A1 and A2 are both vinyl silane coupling agents, and A1 is connected to nano-silica, and m and n are positive integers.

[0027] Preferably, the particle size of the nano-silicon dioxide is 50-150nm, preferably 80-100nm, m is a positive integer of 3-20, preferably a positive integer of 5-15, and n is a positive integer of 3-10, preferably a positive integer of 3-8. Nano-silicon dioxide is used as a supporting skeleton to improve the oil film strength of the cold rolling oil. The chain segments containing benzoic acid in the side chains can not only improve the lubrication and temperature resistance, but also can produce metal bonds with the iron mud produced in the rolling process through the carboxyl group to prevent the agglomeration of the iron mud and produce an oil mud mixture that is difficult to disperse and remove; the ethylene chain segments improve the compatibility with oily raw materials such as base oil, thereby improving the film-forming and lubricity of the cold rolling oil; the end silane coupling agent can produce a certain cross-linking effect to further improve the oil film strength.

[0028] Furthermore, the preparation method of the modified silica includes: using the first batch of vinyltrimethoxysilane to modify nano-silica, then adding p-vinylbenzoic acid, and performing addition polymerization under the action of an initiator, adding ethylene after the reaction is completed to continue addition polymerization under the action of an initiator, and then adding a second batch of vinyltrimethoxysilane to obtain modified silica after polymerization.

[0029] Preferably, the first batch of vinyl trimethoxy silane is added in an amount of 2-15% of the mass of the nano dioxide, preferably 3-10%; the p-vinyl benzoic acid is added in an amount of 5-20% of the mass of the nano dioxide, preferably 8-20%; the ethylene is added in an amount of 1-8% of the mass of the nano dioxide, preferably 2-5%; the second batch of vinyl trimethoxy silane is added in an amount of 2-15% of the mass of the nano dioxide, preferably 3-10%; the initiator is benzoyl peroxide. By regulating the raw material content, the hydrophilicity and hydrophobicity of the shell and the coordination effect with the metal can be regulated.

[0030] Preferably, the composition comprises, by mass percentage: 88-92% base oil, 0.5-1.8% modified silicon dioxide, 2-5% emulsifier, 2-3% extreme pressure agent, 0.5-1% antioxidant, and 0.5-1% rust inhibitor.

[0031] In the modified silicon dioxide, m is a positive integer of 6-15, and n is a positive integer of 5-8.

[0032] Preferably, the emulsifier is one or more of octylphenol polyoxyethylene ether, sorbitol polyoxyethylene ether, nonylphenol polyoxyethylene ether, hexadecanol polyoxyethylene ether, caprylic acid polyoxyethylene ether, and oleic acid polyoxyethylene ether.

[0033] Preferably, the base oil is one or more of coconut oil, palm oil, oxidized rapeseed oil, pentaerythritol tetraheptyl ester and pentaerythritol tetraoctyl ester.

[0034] Preferably, the extreme pressure agent is at least one of isooctyl acid phosphate octadecylamine salt, di-n-butyl phosphite, dialkyl dithiocarbamate molybdenum or dialkyl dithiophosphate;

[0035] Preferably, the rust inhibitor is diethanolamine oleate or triethanolamine oleate; the antioxidant is at least one of 2,6-di-tert-butyl-p-cresol and benzotriazole octadecylamine salt.

[0036] Preferably, the preparation method of the cold rolling oil for galvanized substrate comprises: mixing the emulsifier and the base oil and heating it to 40-60°C, then adding modified silica and an extreme pressure agent, stirring evenly, adding an antioxidant and a rust inhibitor, stirring evenly at 50-65°C, and cooling to room temperature for discharging.

[0037] During the rolling process, the cold rolling oil for the galvanized substrate is dispersed in deionized water to form an emulsion system, and rolling is performed in the form of an emulsion. The pH of the emulsion system is 4-5, and the conductivity is less than 300 μs / cm. The mass concentration of the cold rolling oil for the galvanized substrate in the emulsion system is 1%-5%.

[0038] Examples 1-5 and Comparative Example 1

[0039] The cold rolling oil for galvanized substrates provided in Examples 1-5 has a composition ratio as shown in Table 1.

[0040] Table 1 Component mass content of Examples 1-5 and Comparative Example 1

[0041]

[0042] Among them, the base oil is palm oil and pentaerythritol tetraoctyl ester in a mass ratio of 2:1; the emulsifier is octylphenol polyoxyethylene ether and sorbitol polyoxyethylene ether in a mass ratio of 1:1; the extreme pressure agent is di-n-butyl phosphite and molybdenum dialkyl dithiocarbamate in a mass ratio of 1:1; the rust inhibitor is triethanolamine oleate; and the antioxidant is 2,6-di-tert-butyl-p-cresol.

[0043] The preparation method of modified silicon dioxide comprises:

[0044] Nano-silica (average particle size of 100 nm) is added to a mixed solvent of water and ethanol in a volume ratio of 1:3, and then 5% of the mass of the nano-silica is added with vinyl trimethoxy silane, and the mixture is reacted at 40°C for 2 hours, and then 15% of the mass of the silica is added with p-vinyl benzoic acid, the temperature is raised to 80°C, benzoyl peroxide is added, and the mixture is reacted at a constant temperature for 4 hours, and then 3% of the mass of the silica is added with ethylene, and the mixture is reacted at a constant temperature for 2 hours, and then 5% of the mass of the nano-silica is added with vinyl trimethoxy silane, and the mixture is reacted at 80°C for 1 hour, the temperature is lowered to room temperature, and the solid-liquid separation is performed to obtain modified silica, such as Figure 1 shown.

[0045] Example 6

[0046] The difference from Example 1 is that the preparation method of modified silicon dioxide comprises:

[0047] Nano-silica (average particle size of 100 nm) was added to a mixed solvent of water and ethanol in a volume ratio of 1:3, and then 5% of vinyltrimethoxysilane by mass of the nano-silica was added, and the mixture was reacted at 40°C for 2 hours, and then 20% of p-vinylbenzoic acid by mass of the silica was added, the temperature was raised to 80°C, benzoyl peroxide was added, and the mixture was reacted at a constant temperature for 5 hours, and then 3% of ethylene by mass of the silica was added, and the mixture was reacted at a constant temperature for 2 hours, and then 5% of vinyltrimethoxysilane by mass of the nano-silica was added, and the mixture was reacted at 80°C for 1 hour, and the temperature was lowered to room temperature, and the solid-liquid separation was performed to obtain modified silica.

[0048] Example 7

[0049] The difference from Example 1 is that the preparation method of modified silicon dioxide comprises:

[0050] Nano-silica (average particle size of 100 nm) was added to a mixed solvent of water and ethanol in a volume ratio of 1:3, and then 5% of vinyltrimethoxysilane by mass of the nano-silica was added, and the mixture was reacted at 40°C for 2 hours. Then, 5% of p-vinylbenzoic acid by mass of the silica was added, the temperature was raised to 80°C, benzoyl peroxide was added, and the mixture was reacted at a constant temperature for 3 hours. Then, 3% of ethylene by mass of the silica was added, and the mixture was reacted at a constant temperature for 2 hours. Then, 5% of vinyltrimethoxysilane by mass of the nano-silica was added, the mixture was reacted at 80°C for 1 hour, the temperature was lowered to room temperature, and the solid-liquid separation was performed to obtain modified silica.

[0051] Example 8

[0052] The difference from Example 1 is that the preparation method of modified silicon dioxide comprises:

[0053] Nano-silica (average particle size of 100 nm) was added to a mixed solvent of water and ethanol in a volume ratio of 1:3, and then 5% of the mass of the nano-silica was added with vinyltrimethoxysilane, and the mixture was reacted at 40°C for 2 h. Then 15% of the mass of the silica was added with p-vinylbenzoic acid, the temperature was raised to 80°C, benzoyl peroxide was added, and the mixture was reacted at a constant temperature for 5 h. Then 3% of the mass of the silica was added with ethylene, and the mixture was reacted at a constant temperature for 2 h. Then 8% of the mass of the nano-silica was added with vinyltrimethoxysilane, the mixture was reacted at 80°C for 2 h, the temperature was lowered to room temperature, and the solid-liquid separation was performed to obtain modified silica.

[0054] Comparative Example 2

[0055] The difference from Example 1 is that the preparation method of modified silicon dioxide comprises:

[0056] Nano-silica (average particle size of 100 nm) was added to a mixed solvent of water and ethanol in a volume ratio of 1:3, and then 5% of vinyl trimethoxy silane by mass of the nano-silica was added, and the mixture was reacted at 40°C for 2 h, and then 1% of p-vinyl benzoic acid by mass of the silica was added, the temperature was raised to 80°C, benzoyl peroxide was added, and the mixture was reacted at a constant temperature for 2 h, and then 3% of ethylene by mass of the silica was added, and the mixture was reacted at a constant temperature for 2 h, and then 5% of vinyl trimethoxy silane by mass of the nano-silica was added, and the mixture was reacted at 80°C for 1 h, the temperature was lowered to room temperature, and the solid-liquid separation was performed to obtain modified silica.

[0057] Comparative Example 3

[0058] The difference from Example 1 is that the preparation method of modified silicon dioxide comprises:

[0059] Nano-silica (average particle size of 100 nm) was added to a mixed solvent of water and ethanol in a volume ratio of 1:3, and then 5% of vinyl trimethoxy silane by mass of the nano-silica was added, and the mixture was reacted at 40°C for 2 h. Then, 15% of p-vinyl benzoic acid by mass of the silica was added, the temperature was raised to 80°C, benzoyl peroxide was added, and the mixture was reacted at a constant temperature for 4 h. Subsequently, 5% of vinyl trimethoxy silane by mass of the nano-silica was added, the mixture was reacted at 80°C for 1 h, the temperature was lowered to room temperature, and the solid-liquid separation was performed to obtain modified silica.

[0060] Comparative Example 4

[0061] The difference from Example 1 is that the preparation method of modified silicon dioxide comprises:

[0062] Nano-silica (average particle size of 100 nm) was added to a mixed solvent of water and ethanol in a volume ratio of 1:3, and then 5% of vinyltrimethoxysilane by mass of the nano-silica was added, and the reaction was carried out at 40°C for 2 hours. Then, 15% of p-vinylbenzoic acid by mass of the silica was added, the temperature was raised to 80°C, benzoyl peroxide was added, and the reaction was carried out at a constant temperature for 4 hours. Then, 3% of ethylene by mass of the silica was added, and the reaction was carried out at a constant temperature for 2 hours. The temperature was lowered to room temperature, and the solid-liquid separation was carried out to obtain modified silica.

[0063] Performance Testing

[0064] 1) Kinematic viscosity at 40℃, test standard is GB / T 265, not more than 70mm 2 / s.

[0065] 2) PB value of four-ball test, test standard is GB / T 3142, not less than 588N.

[0066] 3) Mill cleanliness test: Prepare 5% emulsion, transfer 100mL to a stoppered measuring cylinder, add 1g iron powder (commercial standard iron powder), stir at 200r / min for 2min at 120℃, and then observe the suspension of iron powder. According to the dispersion of iron powder, it is divided into 4 levels, namely, level 1, completely free suspension; level 2, the iron powder in the foam is released quickly and the iron powder is coarsely dispersed; level 3, the iron powder is slightly agglomerated; level 4, the iron powder is agglomerated and adheres to the inner wall of the measuring cylinder.

[0067] Table 2 Test results of Examples 1-8 and Comparative Examples 1-4

[0068]

[0069] As can be seen from Table 2, the addition of modified silica can significantly improve the oil film strength and mill cleanliness, and it is not easy to form agglomerated sludge with iron powder at high temperature. In addition, the content of vinyl benzoic acid and ethylene segments has an important influence on mill cleanliness, and the coupling effect of the end silane coupling agent also helps to improve the oil film strength and mill cleanliness.

[0070] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A cold rolling oil for galvanized substrates, It is characterized in that In terms of mass percentage, it includes: base oil 85-95%, modified silica 0.1-2%, emulsifier 1-6%, extreme pressure agent 1-4%, antioxidant 0.1-2%, rust inhibitor 0.1-2%; The modified silica is a microsphere with nano-silicon dioxide as the core and the following structural formula as the shell: Wherein, A1 and A2 are both vinyl silane coupling agents, and A1 is connected to nano-silica, and m and n are positive integers; The preparation method of the modified silicon dioxide comprises: using the first batch of vinyl trimethoxysilane to modify nano silicon dioxide, then adding p-vinyl benzoic acid, and performing addition polymerization under the action of an initiator, adding ethylene after the reaction is completed, and continuing to perform addition polymerization under the action of an initiator, and then adding the second batch of vinyl trimethoxysilane, and obtaining the modified silicon dioxide after polymerization; The amount of the first batch of vinyl trimethoxy silane added is 2-15% of the mass of the nano silicon dioxide, the amount of the p-vinyl benzoic acid added is 5-20% of the mass of the nano silicon dioxide, the amount of the ethylene added is 1-8% of the mass of the nano silicon dioxide, the amount of the second batch of vinyl trimethoxy silane added is 2-15% of the mass of the nano silicon dioxide, and the initiator is benzoyl peroxide; The base oil is one or more of coconut oil, palm oil, oxidized rapeseed oil, pentaerythritol tetraheptyl ester and pentaerythritol tetraoctyl ester.

2. The cold rolling oil for galvanized substrate according to claim 1, It is characterized in that The particle size of the nano silicon dioxide is 50-150 nm, m is a positive integer of 3-20, and n is a positive integer of 3-10.

3. The cold rolling oil for galvanized substrate according to claim 1, It is characterized in that In terms of mass percentage, it includes: base oil 88-92%, modified silica 0.5-1.8%, emulsifier 2-5%, extreme pressure agent 2-3%, antioxidant 0.5-1%, rust inhibitor 0.5-1%; In the modified silicon dioxide, m is a positive integer of 6-15, and n is a positive integer of 5-8.

4. The cold rolling oil for galvanized substrate according to claim 1, It is characterized in that The emulsifier is one or more of octylphenol polyoxyethylene ether, sorbitol polyoxyethylene ether, nonylphenol polyoxyethylene ether, hexadecanol polyoxyethylene ether, caprylic acid polyoxyethylene ether, and oleic acid polyoxyethylene ether.

5. The cold rolling oil for galvanized substrate according to claim 1, It is characterized in that The extreme pressure agent is at least one of isooctyl acid phosphate octadecylamine salt, di-n-butyl phosphite, dialkyl dithiocarbamate molybdenum or dialkyl dithiophosphate.

6. The cold rolling oil for galvanized substrate according to claim 1, It is characterized in that The rust inhibitor is diethanolamine oleate or triethanolamine oleate; the antioxidant is at least one of 2,6-di-tert-butyl-p-cresol and benzotriazole octadecylamine salt.

7. The cold rolling oil for galvanized substrate according to any one of claims 1 to 6, It is characterized in that The preparation method of the cold rolling oil for galvanized substrate comprises: mixing an emulsifier and a base oil, heating to 40-60° C., then adding modified silicon dioxide and an extreme pressure agent, stirring evenly, adding an antioxidant and a rust inhibitor, stirring evenly at 50-65° C., cooling to room temperature and discharging.

Citation Information

Patent Citations

  • Modified nanocellulose for rolling oil and application of modified nanocellulose

    CN116836302A

  • Cold-rolled sheet rolling emulsified oil containing modified nano copper and preparation method thereof

    CN102796594A

  • Solvent-free silica nanofluid and application thereof

    CN108085089A