An anti-oxidation magnesium-aluminum spinel-based composite coating and its preparation method
Magnesium-aluminum spinel-based composite coatings were prepared by ball milling and microwave technology using a mixture of magnesium-aluminum spinel powder, SiC powder, metallic aluminum powder, and low-melting-point glass powder. This method solved the problems of high cost and complex process of ceramic coatings and achieved a highly efficient anti-oxidation effect.
Patent Information
- Application Number
- CN202410107508.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-26
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-01-26
AI Technical Summary
In the existing technology, the preparation methods of ceramic coatings have the problems of high cost and complex process, and it is difficult to effectively solve the problem of material oxidation.
Magnesium aluminum spinel powder, SiC powder, metallic aluminum powder and low-melting-point glass powder are mixed in a certain proportion and a magnesium aluminum spinel-based composite coating is prepared by wet ball milling and microwave technology. The fluidity of the low-melting-point glass powder and the chemical stability of SiC are utilized to form multiphase entangled magnesium aluminum spinel crystals, thereby improving the adhesion and stability of the coating.
The prepared magnesium-aluminum spinel-based composite coating has excellent high-temperature resistance and anti-oxidation properties, low cost, simple process, and high bonding strength between the coating and the substrate, making it suitable for the surface of metal and alloy materials.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of ceramic coatings, specifically relating to an anti-oxidation magnesium-aluminum spinel-based composite coating and its preparation method. Background Technology
[0002] With the rapid development of modern industrial technology, the problem of material oxidation has become increasingly prominent in many fields, leading to a series of serious consequences such as equipment wear and tear, energy waste, and decreased production efficiency. To address this issue, ceramic coating technology has emerged, becoming a research and application hotspot due to its unique advantages in oxidation prevention.
[0003] The patent technology "A method for preparing a SiC-ZrC composite coating in the inner hole of a slender metal tube" (CN116590689A) introduces a SiC-ZrC composite coating in the inner hole of a slender metal tube. The method involves using silicon powder and silica powder as vapor deposition powders, reacting them in situ with CH4 or C3H6 to prepare an inner coating; then using zirconium powder, potassium chloride, and lithium chloride as vapor deposition powders, reacting them in situ with CH4 or C3H6 to prepare an outer coating, thus forming the SiC-ZrC composite coating. The SiC-ZrC composite coating prepared by this method suffers from high cost and complex processing. The patent technology "A composite structure rare earth modified tungsten coating and its preparation method" (CN116590688A) introduces a composite structure rare earth modified tungsten coating. A composite Gd₂C₃ / W / Sm₂O₃ anti-oxidation coating was prepared on the surface of a cobalt-based superalloy using chemical vapor deposition (CVD) with Gd particles, Sm particles, WF₆ gas, and related process gases as raw materials. This method involves controlling factors such as the vacuum chamber heating temperature, vacuum level, external reactor temperature, process gas flow rate, and deposition time of the CVD equipment to create a composite anti-oxidation coating with Gd₂C₃ as the interface layer, W as the main phase coating, and Sm₂O₃ as the sealing layer. However, this method also suffers from drawbacks such as high cost and complex processing.
[0004] "Bonding and Antioxidant Properties of Nickel-Containing Metal Ceramic Coating on Surface of GH4586 Nickel Alloy for Aerospace Engines" (Gao Bo, Zeng Fanhao, Gu Yi, et al. Bonding and Antioxidant Properties of Nickel-Containing Metal Ceramic Coating on Surface of GH4586 Nickel Alloy for Aerospace Engines [J]. Powder Metallurgy Materials Science and Engineering, 2018, 23(05): 527-533.) A high-temperature nickel-containing B2O3-A12O3-BaO-CeO2-ZrO2 (Ni / BACZ) metal ceramic coating was prepared on the surface of GH4586 nickel-based alloy for aerospace engines using a flow coating method, based on nickel powder and glass phase as raw materials. The prepared metal ceramic coating showed strong bonding with the substrate and its oxidation resistance was 7 times higher than that of the uncoated substrate. However, this method requires mixing, melting, water quenching, grinding, sieving, viscosity adjustment, ball milling, and then flow coating to prepare the coating; it also suffers from high cost and complex process. Summary of the Invention
[0005] In order to solve the above-mentioned technical problems, the present invention provides an anti-oxidation magnesium aluminum spinel-based composite coating and its preparation method. The present invention mainly involves mixing high-performance magnesium aluminum spinel powder, SiC powder, metallic aluminum powder and low-melting-point glass powder in a certain proportion, and reacting them through an Al phase reaction, that is, reacting metallic aluminum powder with SiO2, to form an Al-bonded phase inside the coating.
[0006] This invention utilizes the flow effect of low-melting-point glass powder at high temperatures to fill the pores of the coating material, thereby increasing the adhesion of the coating to the substrate material. This invention uses fewer raw materials, has low preparation costs, and a relatively simple preparation process, resulting in a magnesium-aluminum spinel-based composite coating with excellent oxidation resistance.
[0007] The technical solution adopted in this invention is: an anti-oxidation magnesium-aluminum spinel-based composite coating, wherein the premixed material is composed of: 20-40 parts magnesium-aluminum spinel powder, 35-55 parts SiC powder, 5-25 parts metallic aluminum powder and 25-45 parts low-melting glass powder by weight. The premixed material is added to modified organosilicon resin, and the mass ratio of the premixed material to the modified organosilicon resin is 1-3:3-11.
[0008] The purity of the magnesium aluminum spinel powder is >90%, and the particle size is ≤5μm.
[0009] The purity of the SiC powder is >98%, and the particle size is ≤10μm.
[0010] The purity of the aluminum powder is >96wt%, and the particle size is ≤1μm.
[0011] The low-melting-point glass powder has a melting point below 500℃ and a particle size ≤5μm.
[0012] The modified organosilicon resin is one or more of Fe-modified organosilicon resin, La-modified organosilicon resin, and Cu-modified organosilicon resin, with a solid content >45%.
[0013] A method for preparing an anti-oxidation magnesium-aluminum spinel-based composite coating, characterized by comprising the following steps: Step 1: Mix and dry the raw materials; Magnesium spinel powder, SiC powder, metallic aluminum powder and low melting glass powder are put into a ball mill in the above proportion and wet ball milled for 1 to 5 hours. After being ground into fine powder, they are dried at 110°C for 24 hours to obtain a premix. Step 2: Preparation of an anti-oxidation magnesium-aluminum spinel-based composite coating; The premixed material and modified silicone resin were stirred in a magnetic stirrer at a speed of 60-300 rpm for 10-50 minutes to obtain an anti-oxidation magnesium-aluminum spinel-based composite coating precursor that could be drawn into filaments of 9-11 mm. The anti-oxidation magnesium-aluminum spinel-based composite coating precursor was then coated onto the substrate to a thickness of less than 3 mm. The substrate coated with the anti-oxidation magnesium-aluminum spinel-based composite coating precursor was dried and cured at 80-200℃ for 2-3 hours. Then, it was heated in a microwave oven to 700-900℃ and held for 0.1-1 hours to obtain the magnesium-aluminum spinel-based composite coating.
[0014] The substrate is a stainless steel layer, an inorganic non-metallic material layer, or a metal layer.
[0015] The particle size distribution of this invention aims to ensure uniform distribution of raw materials without segregation, thereby giving the mixture low electromagnetic wave absorption rate and excellent wave transmission, resulting in more uniform heating.
[0016] The invention features microwave heating, which is fast and environmentally friendly. More importantly, the modified silicone resin has extremely strong microwave absorption properties and can quickly react with the substrate to form a bond, thereby improving the strength between the interfaces. This results in the multiphase entangled magnesium aluminum spinel effectively improving the bonding strength with the substrate.
[0017] In step one, the material-to-ball mass ratio during wet ball milling is 1-5:5-9.
[0018] The magnesium aluminum spinel is a solid product of the reaction between MgO and Al2O3. It has a high melting point (2135℃), high chemical stability, low coefficient of thermal expansion, excellent thermal shock resistance, chemical corrosion resistance and wear resistance.
[0019] The SiC has the advantages of stable chemical properties, high thermal conductivity, low coefficient of thermal expansion, and good wear resistance.
[0020] The aluminum powder is the main antioxidant, with a melting point of 660℃. Under high temperature, it reacts with oxygen in the air to form an Al-O gas phase, which is deposited and acts as a gas sol.
[0021] The low-melting-point glass powder is composed of the SiO2 phase, which, under high temperature, generates a liquid phase, improving the fluidity and viscosity of the coating and solving the problem of resin failure at high temperatures. Simultaneously, during microwave-assisted processing, it excites SiO plasma gas, which reacts with CO gas in the environment to form SiC whiskers, strengthening the bonding mechanism.
[0022] This invention is primarily used for anti-oxidation coatings on the surface of metal or alloy substrates. It utilizes the low-temperature melting characteristics of low-melting glass powder to react with a carbon source to generate SiC. Combined with the ceramic phase transformation of an aluminum source, periclase crystals, SiC crystals, and corundum crystals undergo mutual solid solution to form magnesium aluminum spinel crystals. The interpenetration and entanglement of these crystals during the solid solution process create a multiphase entangled magnesium aluminum spinel-based composite material. This significantly improves the adhesion and stability of the coating, demonstrating outstanding technological advancement.
[0023] In step one, the magnesium aluminum spinel powder, SiC powder, metallic aluminum powder, and low-melting glass powder are pre-ball-milled, which not only achieves the purpose of uniform mixing, but also further reduces the particle size of the powder during the milling process, increases the specific surface area of the powder to a certain extent, reduces the surface activation energy of the particles, and improves the uniformity of the coating.
[0024] The beneficial effects of this invention are as follows: This invention obtains a premix by wet ball milling magnesium aluminum spinel powder, SiC powder, metallic aluminum powder, and low-melting-point glass powder, and then stirs the premix with a phosphate solution to obtain a magnesium aluminum spinel-based composite material. Pre-ball milling of the magnesium aluminum spinel powder, SiC powder, metallic aluminum powder, and low-melting-point glass powder increases the specific surface area of the powder and reduces the surface activation energy of the particles. This invention uses inexpensive and readily available raw materials, featuring low cost and simple preparation process. The prepared magnesium aluminum spinel-based composite material exhibits excellent high-temperature resistance and oxidation resistance, and good overall performance.
[0025] The magnesium-aluminum spinel-based composite coating of this invention is produced by mixing magnesium-aluminum spinel powder, SiC powder, metallic aluminum powder and low-melting-point glass powder in a certain proportion, and generating a multiphase entangled anti-oxidation magnesium-aluminum spinel-based composite coating through microwave technology combined with carbothermal reduction method. It uses fewer raw materials, has low preparation cost, and relatively simple preparation process. The resulting anti-oxidation magnesium-aluminum spinel-based composite coating has excellent high-temperature resistance. Detailed Implementation
[0026] The present invention will be further described in detail below with reference to specific embodiments. The embodiments of the present invention provide an anti-oxidation magnesium-aluminum spinel-based composite coating, wherein the magnesium spinel powder has a purity >90% and a particle size ≤5μm; the SiC powder has a purity >98% and a particle size ≤10μm; the aluminum powder has a purity >96wt% and a particle size ≤1μm; and the low-melting-point glass powder has a melting point below 500℃ and a particle size ≤5μm. Example
[0027] Step 1: Mix and dry the raw materials 20 parts of magnesium aluminum spinel powder, 50 parts of SiC powder, 5 parts of metallic aluminum powder and 25 parts of low melting glass powder were put into a ball mill and wet-milled for 1 hour. The mass ratio of material to ball in the ball mill was 1:8. After being ground into fine powder, the powder was dried at 110°C for 24 hours to obtain a premix.
[0028] Step 2: Preparation of Anti-oxidation Magnesium Aluminum Spinel-based Composite Coating The premixed material and Fe-modified silicone resin were stirred at a mass ratio of 1:5 using a magnetic stirrer at 60 rpm for 10 minutes, resulting in a magnesium-aluminum spinel-based composite coating precursor that could be drawn into 9mm wires. The anti-oxidation magnesium-aluminum spinel-based composite coating precursor was then coated onto 316L stainless steel to a thickness of 1mm. The 316L stainless steel coated with the anti-oxidation magnesium-aluminum spinel-based composite coating precursor was dried and cured at 80℃ for 2-3 hours, and then heated to 700℃ in a microwave oven and held for 0.1 hours to obtain the magnesium-aluminum spinel-based composite coating. Example
[0029] Step 1: Mix and dry the raw materials 30 parts of magnesium aluminum spinel powder, 35 parts of SiC powder, 10 parts of metallic aluminum powder and 25 parts of low melting glass powder were put into a ball mill and wet-milled for 5 hours. The mass ratio of material to ball in the ball mill was 5:9. After being ground into fine powder, the powder was dried at 110°C for 24 hours to obtain a premix.
[0030] Step 2: Preparation of Anti-oxidation Magnesium Aluminum Spinel-based Composite Coating The premixed material and La-modified silicone resin were stirred at a mass ratio of 3:11 using a magnetic stirrer at 300 rpm for 50 minutes, resulting in a magnesium-aluminum spinel-based composite coating precursor that could be drawn into 11 mm wires. The anti-oxidation magnesium-aluminum spinel-based composite coating precursor was then coated onto an alumina layer to a thickness of 3 mm. The alumina layer coated with the anti-oxidation magnesium-aluminum spinel-based composite coating precursor was dried and cured at 200℃ for 2-3 hours, and then heated to 900℃ in a microwave oven and held for 1 hour to obtain the magnesium-aluminum spinel-based composite coating. Example
[0031] Step 1: Mix and dry the raw materials 25 parts of magnesium aluminum spinel powder, 40 parts of SiC powder, 5 parts of metallic aluminum powder and 30 parts of low melting glass powder were put into a ball mill and wet-milled for 3 hours. The mass ratio of material to ball in the ball mill was 3:4. After being ground into fine powder, the powder was dried at 110°C for 24 hours to obtain a premix.
[0032] Step 2: Preparation of Anti-oxidation Magnesium Aluminum Spinel-based Composite Coating The premixed material and Cu-modified silicone resin were stirred at a mass ratio of 3:8 using a magnetic stirrer at 180 rpm for 30 minutes, resulting in a magnesium-aluminum spinel-based composite coating precursor that could be drawn into 10 mm wires. The anti-oxidation magnesium-aluminum spinel-based composite coating precursor was then coated onto a magnesium oxide layer to a thickness of 2 mm. The magnesium oxide layer coated with the anti-oxidation magnesium-aluminum spinel-based composite coating precursor was dried and cured at 150℃ for 2-3 hours, and then heated to 800℃ in a microwave oven and held for 0.5 hours to obtain the magnesium-aluminum spinel-based composite coating. Example
[0033] Step 1: Mix and dry the raw materials 30 parts of magnesium aluminum spinel powder, 35 parts of SiC powder, 10 parts of metallic aluminum powder and 25 parts of low melting glass powder were put into a ball mill and wet-milled for 4 hours. The mass ratio of material to ball in the ball mill was 2:7. After being ground into fine powder, the powder was dried at 110°C for 24 hours to obtain a premix.
[0034] Step 2: Preparation of Anti-oxidation Magnesium Aluminum Spinel-based Composite Coating The premixed materials were stirred with Fe-modified silicone resin and La-modified silicone resin at a mass ratio of 2:7 using a magnetic stirrer at 200 rpm for 40 minutes, resulting in a magnesium-aluminum spinel-based composite coating precursor that could be drawn into 10 mm filaments. The oxidation-resistant magnesium-aluminum spinel-based composite coating precursor was then coated onto a silicon oxide layer to a thickness of 1.8 mm. The silicon oxide layer coated with the oxidation-resistant magnesium-aluminum spinel-based composite coating precursor was dried and cured at 180℃ for 2-3 hours, and then heated to 880℃ in a microwave oven and held for 0.6 hours to obtain the magnesium-aluminum spinel-based composite coating.
[0035] The magnesium-aluminum spinel-based composite coating prepared by this patent exhibits excellent antioxidant properties. Compared with other coating methods, this preparation method has the following advantages: the raw materials are non-toxic, harmless, and readily available; the microwave process shortens the production time, thus requiring lower production costs; the preparation process only requires ball milling, drying, stirring, curing, and sintering, making the process simple.
Claims
1. An anti-oxidation magnesium-aluminum spinel-based composite coating, characterized in that: The premix composition, by weight, is: 20-40 parts magnesium aluminum spinel powder, 35-55 parts SiC powder, 5-25 parts metallic aluminum powder, and 25-45 parts low-melting-point glass powder. The metallic aluminum powder has a purity >96wt% and a particle size ≤1μm, and the low-melting-point glass powder has a melting point below 500℃ and a particle size ≤5μm. The premix is added to the modified organosilicon resin, with a mass ratio of premix to modified organosilicon resin of 1-3:3-11. The preparation method includes the following steps: Step 1: Mix and dry the raw materials; Magnesium aluminum spinel powder, SiC powder, metallic aluminum powder and low melting glass powder are put into a ball mill in the above proportion and wet ball milled for 1 to 5 hours. After being ground into fine powder, they are dried at 110°C for 24 hours to obtain a premix. Step 2: Preparation of an anti-oxidation magnesium-aluminum spinel-based composite coating; The premix and modified silicone resin were stirred in a magnetic stirrer at a speed of 60-300 rpm for 10-50 minutes to obtain an anti-oxidation magnesium-aluminum spinel-based composite coating precursor that could be drawn into filaments of 9-11 mm. The anti-oxidation magnesium-aluminum spinel-based composite coating precursor was then coated onto the substrate to a thickness of less than 3 mm. The substrate coated with the anti-oxidation magnesium-aluminum spinel-based composite coating precursor was dried and cured at 80-200℃ for 2-3 hours, and then heated in a microwave oven to 700-900℃ and held for 0.1-1 hours to obtain the magnesium-aluminum spinel-based composite coating. The low-temperature melting characteristics of the low-melting glass powder reacted with the carbon source to generate SiC. The aluminum source underwent ceramic phase transformation, and periclase crystals, SiC crystals, and corundum crystals dissolved in each other to form magnesium-aluminum spinel crystals. The interpenetration and entanglement of the crystals formed during the solid solution process resulted in a multiphase entangled magnesium-aluminum spinel-based composite material.
2. The anti-oxidation magnesium-aluminum spinel-based composite coating according to claim 1, characterized in that: The purity of the magnesium aluminum spinel powder is >90%, and the particle size is ≤5μm.
3. The anti-oxidation magnesium-aluminum spinel-based composite coating according to claim 1, characterized in that: The purity of the SiC powder is >98%, and the particle size is ≤10μm.
4. The anti-oxidation magnesium-aluminum spinel-based composite coating according to claim 1, characterized in that: The modified organosilicon resin is one or more of Fe-modified organosilicon resin, La-modified organosilicon resin, and Cu-modified organosilicon resin, with a solid content >45%.
5. The method for preparing the anti-oxidation magnesium-aluminum spinel-based composite coating according to claim 1, characterized in that: The substrate is an inorganic non-metallic material layer or a metal layer.
6. The method for preparing the anti-oxidation magnesium-aluminum spinel-based composite coating according to claim 1, characterized in that: In step one, the material-to-ball mass ratio during wet ball milling is 1-5:5-9.
Citation Information
Patent Citations
Composite structure rare earth modified tungsten coating and preparation method thereof
CN116590688A
Preparation method of SiC-ZrC composite coating in inner hole of slender metal pipe
CN116590689A
Silicone coating
CN103059725A
Silicon carbide-magnesium aluminate spinel-aluminum composite refractory material
CN111704466A