A nondestructive testing method for heat treatment quality of alloy steel castings for mining machinery

Through the method of combining environmentally friendly on-site metallographic coating paper with grinding and polishing treatment, the problem of heat treatment quality inspection of alloy steel castings for mining machinery has been solved, fast, non-destructive and accurate inspection has been achieved, and costs and safety risks have been reduced.

CN118067948BActive Publication Date: 2024-10-11XIAN COAL MINING MACHINERY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410188501.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-20
Publication Date
2024-10-11
Estimated Expiration
2044-02-20

AI Technical Summary

Technical Problem

It is difficult to quickly and non-destructively detect the heat treatment quality of mining machinery alloy steel castings with existing technology, especially when the size is large and the structure is complex, the heat treatment quality cannot be accurately controlled, and common methods use toxic chemicals, resulting in low detection efficiency and problems. Safety hazard.

Method used

Using a method that combines environmentally friendly on-site metallographic coating paper with grinding and polishing treatment, typical areas of alloy steel castings of mining machinery are ground, polished and corroded to obtain the metallographic microstructure. Through on-site replication of the metallographic structure and the original austenitic Replicate the bulk grain boundaries to achieve rapid and non-destructive heat treatment quality inspection.

Benefits of technology

It achieves fast online, non-destructive, efficient and accurate detection, reduces detection costs, avoids damage to parts, improves detection quality, and uses environmentally friendly materials, which is safe and reliable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118067948B_ABST
    Figure CN118067948B_ABST
Patent Text Reader

Abstract

The present invention discloses a nondestructive testing method for the heat treatment quality of alloy steel castings for mining machinery, comprising the following steps: 1. preparing environmentally friendly on-site metallographic coating paper; 2. selecting typical areas on the surface of alloy steel castings for mining machinery, and grinding and etching the typical areas; 3. performing on-site replication of the metallographic structure and on-site replication of the original austenite grain boundary of the area to be inspected; 4. judging the heat treatment quality of alloy steel castings for mining machinery during processing according to the microstructure. The present invention selects typical areas for grinding and etching, uses on-site replication to obtain real and clear grain size, residual cast structure and metallographic microstructure category, judges whether the heat treatment quality of alloy steel castings for mining machinery is qualified, realizes the finalization treatment of the matrix structure without pollution, damage or deformation, effectively realizes the accurate reproduction of the main structure on the metallographic microscope, and has the characteristics of nondestructive testing, accuracy and efficiency, safety and environmental protection, and low cost.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Methodology Area

[0002] The invention belongs to the field of heat treatment quality detection of alloy steel castings for mining machinery, and in particular relates to a nondestructive detection method for heat treatment quality of alloy steel castings for mining machinery.

[0003] Background Methods

[0004] Metallographic analysis and testing is one of the important means of material research and metallurgical machinery products. The metallographic structure determines the quality of heat treatment. At present, on-site metallographic non-destructive analysis methods are the development trend of online detection and organization analysis, especially European countries such as Germany and Italy are at the forefront of research and application of on-site metallographic non-destructive methods. On-site metallographic non-destructive testing and analysis methods are online detection of part performance, which is of great significance in preventing early failure of parts and predicting the life of parts. All countries are committed to exploring and researching this aspect and developing metallographic non-destructive testing and analysis methods.

[0005] With the rapid development of coal mining machinery, many mining machinery are cast due to the complex structure and large size of mining machinery parts. In particular, the rocker arm, traction part, and travel box shell are used as dynamic load parts under harsh alternating load stress conditions. The heat treatment quality of the material has an important impact on its service life. The safe service of alloy steel castings is of great significance to the safe and reliable operation of mining machinery and equipment. Once the cast steel shell fractures and fails, it will not only damage the coal mining shell, but also damage the internal gears, and will also bring huge economic losses and safety hazards. In order to avoid major safety accidents, rapid detection of the internal heat treatment quality of the casting shell has become a scientific problem that the coal mining machinery industry urgently needs to solve. As a coal mining machine alloy steel casting with a more complex stress, it is necessary to strictly control the casting process and heat treatment process quality of the parts and components. At present, the domestic method of determining whether the parts and components meet the requirements is mainly to use the performance of the continuous casting test block to indirectly reflect the intrinsic quality of the parts and components. On the one hand, the detection of the continuous casting test block requires gas cutting, cutting and other processes, which has a long detection cycle and high detection cost. On the other hand, it fails to truly display the intrinsic quality of the casting parts and components. If samples are taken from the main body, the integrity of the parts will be destroyed and the strength of the parts will be affected. Therefore, it is urgent to study the non-destructive testing method of the heat treatment quality of the parts. Due to the different materials and heat treatment quality of coal mine machinery, the methods of on-site sample preparation, etching and lamination are different.

[0006] Mining machinery alloy steel castings are prone to microsegregation and loose dendrites due to the large variety and high content of alloy elements. Conventional on-site metallographic replication methods cannot obtain clear and effective metallographic microstructures. According to the requirements of CB / T3694-1995 and DL / T 652-1998, acetone is generally used in on-site metallographic replication AC paper and replication solvents. This substance is irritating, toxic, flammable and explosive. Excessive contact will cause acute / chronic poisoning and is harmful to the human body. In addition, it is necessary to file with the public security agency when purchasing, and the procurement time is long. In addition, the on-site metallographic replication process of mining machinery casting samples generally takes 60 minutes per piece, and the detection efficiency is low. There is an urgent need for efficient on-site metallographic non-destructive testing methods.

[0007] In summary, there are still problems in how to use the rapid experimental method of on-site nondestructive testing of heat treatment quality to realize the heat treatment structure identification and detection of on-site mining machinery alloy cast steel in the shortest time, significantly reduce destructive testing, shorten the judgment procedure, and quickly and nondestructively judge the key method of the intrinsic quality of heat treatment of castings.

[0008] Therefore, a nondestructive testing method for heat treatment quality of alloy steel castings for mining machinery is needed. Summary of the invention

[0009] The method problem to be solved by the present invention is to provide a non-destructive testing method for the heat treatment quality of mining machinery alloy steel castings in view of the shortcomings of the above-mentioned existing methods. The method selects a typical area on the surface of the mining machinery alloy steel casting during the processing process, performs grinding and polishing and corrosion treatment on each selected typical area to obtain a typical area to be inspected, and then performs on-site metallographic structure replication on each area to be inspected to obtain the metallographic microstructure of the typical position of the mining machinery alloy steel casting, thereby obtaining the organizational status of multiple areas of the mining machinery alloy steel casting, which solves the problem that the mining machinery alloy steel casting cannot accurately control the heat treatment quality of the mining machinery alloy steel casting due to its large size, complex structure, and large wall thickness difference.

[0010] In order to solve the above technical problems, the technical solution provided by the present invention is: a method for nondestructive testing of heat treatment quality of alloy steel castings for mining machinery, characterized in that the method is used to perform on-site nondestructive testing of heat treatment quality of alloy steel castings for mining machinery during processing, comprising the following steps:

[0011] Step 1: Prepare environmentally friendly on-site metallographic coating paper;

[0012] Step 2: During the processing, a typical area is selected from the surface of the mining machinery alloy steel casting, and then the selected typical area is subjected to grinding and polishing and corrosion treatment to obtain an area to be inspected; the mining machinery alloy steel casting is a low-alloy, medium-alloy steel casting or a high-alloy steel casting;

[0013] Step 3: The environmentally friendly on-site metallographic coating paper prepared in step 1 is used to perform on-site metallographic structure replication and on-site replication of the original austenite grain boundary on the area to be inspected obtained in step 2, so as to obtain the microstructure of the typical area of ​​the mining machinery alloy steel casting;

[0014] Step 4: Determine the heat treatment quality of the mining machinery alloy steel castings during processing based on the microstructure obtained in step 3.

[0015] The present invention selects a typical area on the surface of the alloy steel casting of the mining machinery during the processing, performs grinding and polishing treatment and corrosion treatment on each selected typical area to obtain a typical area to be inspected, detects multiple areas of the alloy steel casting of the mining machinery, and then performs on-site metallographic structure replication on each area to be inspected to obtain the metallographic microstructure of the typical position of the alloy steel casting of the mining machinery, thereby obtaining the organizational conditions of multiple areas of the alloy steel casting of the mining machinery, and solves the problem that the alloy steel casting of the mining machinery cannot accurately control the heat treatment quality of the alloy steel casting of the mining machinery due to its large volume, complex structure and large wall thickness difference; the present invention realizes the rapid online, non-destructive, efficient and accurate detection of the metallographic structure of the typical position of the alloy steel casting of the mining machinery, thereby judging the heat treatment quality of different positions of the alloy steel casting of the mining machinery, effectively solving the on-site detection of the metallographic structure of the alloy steel casting of the mining machinery after heat treatment, eliminating the process of machine tool cutting sampling and repair welding of parts, reducing the impact on the quality of parts, shortening the detection cycle, reducing the detection cost, and improving the detection quality.

[0016] The above-mentioned nondestructive testing method for heat treatment quality of alloy steel castings of mining machinery is characterized in that the production process of the environmentally friendly on-site metallographic coating paper in step one is: ethyl cellulose is fully dissolved in anhydrous ethanol and then filtered, and then methyl violet and polyvinyl alcohol are added to the filtrate in sequence and quickly stirred until completely dissolved, and then the upper layer solution is spread by centrifugation, and the environmentally friendly on-site metallographic coating paper is obtained after solidification, and stored in a drying container.

[0017] The above-mentioned non-destructive testing method for heat treatment quality of mining machinery alloy steel castings is characterized in that the grinding and polishing process of the mining machinery alloy steel castings described in step 2 is a low-alloy or medium-alloy steel casting as follows: a polishing machine is used to select wet sandpaper with a mesh number of 200# to 320# for coarse grinding while adding deionized water, and then a wet sandpaper with a mesh number of 400# to 1200# is selected for step-by-step fine grinding while adding deionized water, and then a fluffy polishing cloth and abrasive paste are used for polishing while spraying deionized water intermittently, the diameters of the wet sandpaper and the fluffy polishing cloth are both 20 mm, and the abrasive paste is chromium oxide abrasive paste , alumina grinding paste or artificial diamond polishing agent; when the alloy steel castings of the mining machinery are high-alloy steel castings, the grinding and polishing process is: use an angle grinder, select a nylon polishing sheet and perform coarse grinding while adding deionized water, then select a PVA polishing wheel with a particle size of 280#~1200# and perform fine grinding step by step while adding deionized water, then use a felt wheel and grinding paste to polish while spraying deionized water, the diameters of the nylon polishing sheet, PVA polishing wheel and felt wheel are all 20mm, and the grinding paste is an artificial diamond polishing agent; the diameter of each of the areas to be inspected is 10mm~20mm.In the present invention, the low-alloy and medium-alloy steel castings and the high-alloy steel castings have different grindability and plastic toughness due to the different contents of Cr, Ni, Mo, W and V. To obtain the metallographic detection surface with the same smoothness, the required sample preparation methods are different. Therefore, the present invention controls the specific grinding and polishing processing parameters to enable the low-alloy and medium-alloy steel castings and the high-alloy steel castings to obtain the inspection area with the composite requirements; the present invention first uses the wet sandpaper with a mesh number of 200# to 320# to coarsely grind the low-alloy and medium-alloy steel castings while adding deionized water. The flowing deionized water can timely wash away the grinding chips and the fallen abrasives, thereby reducing the shedding grinding. The rolling action of the particles and the sample surface causes the fixed abrasive particles on the wet sandpaper to be washed away, and the rolling action of the falling abrasive particles and the sample surface is reduced, so that the sharp edges and corners of the fixed abrasive particles on the sandpaper are always in contact with the sample surface, maintaining a good cutting action, and preventing the hard abrasive particles from being embedded in the sample surface to cause an illusion; the present invention selects wet sandpaper with a mesh number of 400# to 1200#, and adds deionized water while fine grinding step by step. As the particle size of the sandpaper becomes smaller and smaller, the contact area between the sandpaper and the sample surface becomes larger, and more heat is generated during the fine grinding process. The flowing deionized water can play a good role in lubrication and cooling, and can prevent the surface from overheating, and the heat generated during grinding is reduced. The generated metal dust is taken away in time by the flowing deionized water, which is beneficial to environmental protection and human health. The present invention adopts a fluffy polishing cloth and abrasive paste to polish while spraying deionized water intermittently. The gaps in the fluffy fabric can store more abrasive paste, and the abrasive paste is partially exposed on the surface to produce a grinding effect. When the fluffy polishing cloth contacts the sample, the pressure should not be too large to avoid increasing the deformation layer. Appropriate deionized water plays a lubricating role to obtain a bright mirror surface. The present invention adopts an angle grinder for high-alloy steel castings of mining machinery, selects nylon polishing sheets for rough grinding while adding deionized water, and due to the high content of alloy elements, the viscosity of high-alloy castings of mining machinery The alloy cast steel is large and has high hardness. An angle grinder with strong grinding force is required to remove the serious deformation layer on the surface of the alloy cast steel. The nylon polishing sheet can grind off the significant deformation layer of the sub-surface layer and reduce the deformation layer formed by the alloy cast steel. The present invention selects a PVA polishing wheel with a particle size of 280#~1200# to grind finely while adding deionized water to further remove the deformation layer. When the high-alloy cast steel is mechanically polished by the PVA polishing wheel, the abrasive is equivalent to a planer and can produce a cutting effect. In addition, a felt wheel and abrasive paste are used to polish while spraying deionized water. The felt wheel can store smaller abrasive paste to obtain a metallographic polishing surface with higher smoothness.

[0018] The above-mentioned nondestructive testing method for heat treatment quality of alloy steel castings for mining machinery is characterized in that the direction of the next grinding and polishing process in step 2 is perpendicular to the direction of the previous grinding and polishing, and the next grinding and polishing is performed after the wear mark of the previous grinding and polishing is eliminated. The present invention ensures the effect of the grinding and polishing process by controlling the direction of each grinding and polishing, thereby ensuring the effect of the obtained metallographic microstructure.

[0019] The above-mentioned nondestructive testing method for heat treatment quality of mining machinery alloy steel castings is characterized in that, when the mining machinery alloy steel castings described in step 2 are low- and medium-alloy steel castings, the process of corrosion treatment is: wiping with absorbent cotton containing hydrochloric acid solution for 20s to 40s, then rinsing with deionized water, then wiping with absorbent cotton containing anhydrous ethanol solution of nitric acid for 10s to 15s, and then rinsing with anhydrous ethanol and drying with hot air; when the mining machinery alloy steel castings are high-alloy steel castings, the process of corrosion treatment is: wiping with absorbent cotton containing hydrochloric acid solution for 10s to 30s, then rinsing with deionized water, then wiping with absorbent cotton containing anhydrous ethanol solution of nitric acid for 5s to 10s, and then rinsing with anhydrous ethanol and drying with hot air; the mass fraction of the hydrochloric acid solution is 5% to 15%, and the mass fraction of nitric acid in the anhydrous ethanol solution of nitric acid is 3% to 4%. The corrosion treatment of low-alloy and medium-alloy steel castings and high-alloy steel castings in the present invention is mainly a process of metallographic structure etching. Due to the difference in phase composition structure between low-alloy and medium-alloy steel castings and high-alloy steel castings, they have different electrode potentials, and many micro-batteries are formed in the etching solution. The phase with a more negative electrode potential is the anode, which dissolves during etching, and these micro-areas on the polishing surface become low-lying and rough. The phase with a positive potential is the cathode and is basically not etched. These micro-areas on the polishing surface remain smooth and flat. Different alloy systems have the same two-phase structure, but different potential differences, and the degree of dissolution of the anode phase is different. Therefore, the chemical etching reagent and method of low-alloy and medium-alloy steel and high-alloy steel for mining machinery are The method is different; the present invention adopts absorbent cotton containing hydrochloric acid solution to wipe the low and medium alloy steel castings for 20s to 40s, so as to further eliminate the deformation layer caused by grinding and polishing, and then rinse with deionized water, and then wipe with absorbent cotton containing anhydrous ethanol solution of nitric acid for 10s to 15s to etch the structure, and then rinse with anhydrous ethanol and blow dry with hot air; the present invention adopts absorbent cotton containing hydrochloric acid solution to wipe the high alloy steel castings for 10s to 30s to eliminate the deformation layer caused by grinding and polishing on the surface of the sample, and then rinse with deionized water, and then wipe with absorbent cotton containing anhydrous ethanol solution of nitric acid for 5s to 10s to etch and display the metallographic structure, and then rinse with anhydrous ethanol and blow dry with hot air.

[0020] The above-mentioned nondestructive testing method for the heat treatment quality of alloy steel castings of mining machinery is characterized in that the process of on-site replication of the metallographic structure in step three is: 1 to 10 drops of solvent are added to the area to be inspected obtained in step two, and then the environmentally friendly on-site metallographic coating paper prepared in step one is spread on the area to be inspected, and pressed to squeeze out excess solvent and bubbles. After standing, the environmentally friendly on-site metallographic coating paper is connected, mounted between two glass slides, and taped with tape, and finally the metallographic structure is observed; the solvent is anhydrous ethanol, the environmentally friendly on-site metallographic coating paper is a square with a side length of 10 mm, the pressing time is 20s to 40s, the standing time is 4min to 15min, and the size of the glass slide is 30mm×100mm. The present invention drips 1 to 10 drops of solvent on the area to be inspected, so as to accurately replicate the tissue morphology, spreads the metallographic replica paper on the area to be inspected, and presses to squeeze out excess solvent and bubbles to prevent false tissues such as bubbles from appearing on the replica paper, takes the metallographic replica paper from one corner with tweezers, places it between two prepared glass slides, presses it tightly and wraps it with transparent tape, so as to facilitate metallographic tissue observation.

[0021] The above-mentioned nondestructive testing method for heat treatment quality of alloy steel castings for mining machinery is characterized in that the production process of the metallographic replica paper is as follows: ethyl cellulose is fully dissolved in anhydrous ethanol and filtered, and then methyl violet and polyvinyl alcohol are sequentially added to the filtrate and stirred rapidly until it is completely dissolved, and then the upper layer solution is spread by centrifugation, and after solidification, the on-site metallographic replica test paper is obtained, and it is cut into 10mm×10mm and stored in a drying container. The present invention uses ethyl cellulose, an alcohol-soluble resin, to fully dissolve in anhydrous ethanol, and then methyl violet and polyvinyl alcohol are sequentially added to the filtrate and stirred rapidly, thereby improving the toughness of the metallographic replica test paper and improving the contrast of the metallographic photograph.

[0022] The above-mentioned non-destructive testing method for heat treatment quality of mining machinery alloy steel castings is characterized in that the process of on-site replication of the original austenite grain boundary in step three is: re-performing secondary grinding and polishing treatment and secondary corrosion treatment on the area to be inspected after the on-site replication of the metallographic structure, and then adopting the same method as the on-site replication of the metallographic structure to carry out on-site replication of the original austenite grain boundary; the secondary grinding and polishing treatment is the same as the grinding and polishing treatment process described in step two, and the process of secondary corrosion treatment when the mining machinery alloy steel casting is a low- or medium-alloy steel casting is: using a low- or medium-alloy steel casting grain boundary corrosion treatment solution to chemically abrade for 2 minutes to 3 minutes, and then rinsing with deionized water Clean, spray anhydrous ethanol, and blow dry with a hair dryer; the low and medium alloy steel casting grain boundary corrosion treatment solution is prepared by picric acid, sodium dodecylbenzene sulfonate and the balance deionized water in a mass ratio of 3.3:1.0:95; the secondary corrosion treatment process of the mining machinery alloy steel casting is a high alloy steel casting: chemically abraded for 5min to 7min using a high alloy steel casting grain boundary corrosion treatment solution, then rinsed with deionized water, sprayed with anhydrous ethanol, and blown dry with a hair dryer; the high alloy steel casting grain boundary corrosion treatment solution is prepared by picric acid, sodium dodecylbenzene sulfonate and the balance deionized water in a mass ratio of 3.3:0.5:95. The present invention re-polishes the typical area by performing a secondary grinding and polishing treatment to ensure that there are no scratches and deformation layers in the typical area, and by performing a secondary corrosion treatment, the effect of on-site replication of the original austenite grain boundary is guaranteed.

[0023] The above-mentioned nondestructive testing method for heat treatment quality of alloy steel castings for mining machinery is characterized in that the items determined in step three are: grain size, residual cast structure and metallographic microstructure category. The present invention performs heat treatment quality testing of alloy steel castings for mining machinery by determining grain size, residual cast structure and metallographic microstructure category.

[0024] Compared with the existing methods, the present invention has the following advantages:

[0025] 1. The present invention selects typical areas on the surface of the alloy steel castings for mining machinery during the processing, performs grinding and polishing treatments and corrosion treatments on each selected typical area to obtain typical areas to be inspected, and then performs on-site metallographic structure replication on each area to be inspected to obtain the metallographic microstructure of the typical position of the alloy steel castings for mining machinery, thereby obtaining the organizational conditions of multiple areas of the alloy steel castings for mining machinery, which solves the problem that the quality of heat treatment of the alloy steel castings for mining machinery cannot be accurately controlled due to their large size, complex structure, and large difference in wall thickness.

[0026] 2. The present invention effectively solves the problem of heat treatment quality detection of cast steel parts, and realizes fast online, non-destructive, efficient and accurate detection of the metallographic structure of typical positions of alloy steel castings of mining machinery, so as to judge the heat treatment quality of alloy steel castings of mining machinery at different positions, eliminating the process of machine tool cutting and sampling of parts and repair welding, reducing the impact on the quality of parts, shortening the detection cycle, reducing the detection cost, and improving the detection quality. It is more efficient than the original physical and chemical dissection destructive method.

[0027] 3. The present invention provides a method for preparing environmentally friendly on-site metallographic coated paper test paper and an on-site environmentally friendly replication method. Anhydrous ethanol is used for replication production and on-site replication, and acetone is not used. The price is significantly lower than acetone, which reduces the detection cost. Acetone is toxic and causes irreversible damage to the respiratory tract and neurons. Anhydrous ethanol is non-toxic to the body and is safer to use.

[0028] 4. The present invention adopts grinding and polishing treatment and corrosion treatment suitable for on-site metallographic replication of alloy steel castings, which meets the necessary conditions for obtaining high-quality metallographic structure.

[0029] 5. The present invention can quickly and accurately determine the heat treatment quality of alloy steel castings for mining machinery based on metallographic microstructure, grain size, and residual cast structure.

[0030] The method scheme of the present invention is further described in detail below through the drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a physical picture of the environmentally friendly on-site metallographic coating paper after the on-site replication of the metallographic structure and the on-site replication of the original austenite grain boundary in step 3 of Example 1 of the present invention.

[0032] Figure 2 This is a metallographic structure of qualified quality obtained after the metallographic structure is replicated on site in Example 1 of the present invention.

[0033] Figure 3 The original austenite grains are of qualified quality obtained by performing on-site replication of the original austenite grain boundaries in Example 1 of the present invention.

[0034] Figure 4 This is a physical picture of the environmentally friendly on-site metallographic coating paper after the on-site replication of the metallographic structure and the on-site replication of the original austenite grain boundary in step 3 of Example 2 of the present invention.

[0035] Figure 5 This is a metallographic structure of unqualified quality obtained after the metallographic structure is replicated on site in Example 2 of the present invention.

[0036] Figure 6 These are original austenite grains of unqualified quality obtained by performing on-site replication of original austenite grain boundaries in Example 2 of the present invention.

[0037] Figure 7 This is a physical picture of the environmentally friendly on-site metallographic coating paper after the on-site replication of the metallographic structure and the on-site replication of the original austenite grain boundary in step 3 of Example 3 of the present invention.

[0038] Figure 8 This is a metallographic structure of qualified quality obtained after the metallographic structure is replicated on site in Example 3 of the present invention.

[0039] Fig. 9 These are original austenite grains of qualified quality obtained by performing on-site replication of original austenite grain boundaries in Example 3 of the present invention.

[0040] Fig.10 This is a physical picture of the environmentally friendly on-site metallographic coating paper after the on-site metallographic structure replication and the on-site replication of the original austenite grain boundary in step 3 of embodiment 4 of the present invention.

[0041] Fig.11 This is a metallographic structure of unqualified quality obtained after the metallographic structure is replicated on site in Example 4 of the present invention.

[0042] Fig.12 These are original austenite grains of unqualified quality obtained by performing on-site replication of original austenite grain boundaries in Example 4 of the present invention.

[0043] Fig.13 This is a physical picture of the environmentally friendly on-site metallographic coating paper after the on-site metallographic structure replication and the on-site replication of the original austenite grain boundary in step 3 of Example 5 of the present invention.

[0044] Fig.14 This is a metallographic structure of qualified quality obtained after the metallographic structure is replicated on site in Example 5 of the present invention.

[0045] Fig.15 These are the original austenite grains of qualified quality obtained by performing on-site replication of the original austenite grain boundaries in Example 5 of the present invention. DETAILED DESCRIPTION

[0046] Example 1

[0047] This embodiment includes the following steps:

[0048] Step 1: Dissolve 15g of ethyl cellulose in 200mL of anhydrous ethanol and filter. Then, add 0.05g of methyl violet and 10g of polyvinyl alcohol to the filtrate in sequence and stir rapidly for 10min until it is completely dissolved. Then, spread the upper layer of solution by centrifugation. After solidification, obtain the on-site metallographic replica test paper, cut it into 10mm×10mm, and store it in a drying container.

[0049] Step 2: Select a typical area on the surface of the ZG25MnF low alloy steel casting of the mining machinery in the positive return + tempering state, and then perform grinding and polishing and corrosion treatment on the selected typical area to obtain the area to be inspected; the grinding and polishing process is: use a polishing machine to select a wet sandpaper with a diameter of 20mm and a mesh number of 200#, and coarsely grind it while adding deionized water at a pressure of 0.05MPa, and then select a wet sandpaper with a diameter of 20mm and a mesh number of 400#, 800# and 1200#, and grind it step by step while adding deionized water at a pressure of 0.05MPa, and then select Use a fluffy polishing cloth and a synthetic diamond polishing agent to polish while spraying deionized water intermittently at a pressure of 0.05MPa. During the polishing process, the direction of the next polishing is perpendicular to the direction of the previous polishing. After the wear mark of the previous polishing is eliminated, the next polishing is performed. The diameter of the area to be inspected is 15mm. The process of the corrosion treatment is: wipe with absorbent cotton containing a 10% hydrochloric acid solution by mass for 30s, then rinse with deionized water, then wipe with absorbent cotton containing an anhydrous ethanol solution of 4% nitric acid by mass for 15s, and then rinse with anhydrous ethanol and blow dry with hot air;

[0050] Step 3, add 5 drops of anhydrous ethanol to the area to be inspected obtained in step 2, then spread the environmental protection on-site metallographic coating paper prepared in step 1 on the area to be inspected, and press to squeeze out excess anhydrous ethanol and bubbles, pick up the environmental protection on-site metallographic coating paper after standing, install it between two glass slides, and stick it with tape to obtain the metallographic replica paper after the metallographic structure on-site replication, re-perform secondary grinding and secondary corrosion treatment on the area to be inspected after the metallographic structure on-site replication, and then adopt the same method as the metallographic structure on-site replication to perform the original austenite grain boundary on-site replication to obtain the metallographic replica paper after the original austenite grain boundary on-site replication, and finally compare the metallographic replica paper after the metallographic structure on-site replication and the original austenite The metallographic replica paper after the on-site replication of the grain boundary is observed to obtain the metallographic microstructure of the mining machinery alloy steel casting; the length × width of the metallographic replica paper is 10mm × 10mm, the pressing time is 30s, the standing time is 12min, and the size of the slide is 30mm × 100mm; the secondary grinding and polishing process is the same as the grinding and polishing process described in step 2, and the secondary corrosion process is: chemically abrading for 2.5min using a solution prepared by picric acid, sodium dodecylbenzene sulfonate and the remainder deionized water in a mass ratio of 3.3:1.0:95, then rinsing with deionized water, spraying with anhydrous ethanol, and drying with a hair dryer;

[0051] Step 4: Determine the heat treatment quality of the mining machinery alloy steel castings according to the metallographic microstructure obtained in step 3; the items to be determined are: grain size, residual cast structure and metallographic microstructure category.

[0052] Figure 1This is a physical picture of the environmental protection on-site metallographic coating paper after the on-site metallographic structure replication and the on-site replication of the original austenite grain boundary in step 3 of this embodiment. Figure 1 It can be seen that the three test papers on the left are environmentally friendly on-site metallographic coating papers after on-site replication of the metallographic structure, the test paper in the middle and the two test papers on the right are environmentally friendly on-site metallographic coating papers after on-site replication of the original austenite grain boundary. In this embodiment, the metallographic structure of the ZG25MnF low-alloy steel casting in the normalizing + tempering state was replicated on-site, and the environmentally friendly on-site metallographic coating paper clamped in the slide was obtained.

[0053] Figure 2 This is the qualified metallographic structure obtained after the metallographic structure is replicated on site in this embodiment. Figure 2 It can be seen that the metallographic structure of the ZG25MnF low alloy steel casting in the normalized + tempered state of this embodiment is clearly visible, the organizational boundary is clear, and the organizational identification is convenient. The metallographic structure is small block ferrite + pearlite + bainite, which meets the production detection requirements.

[0054] Figure 3 The original austenite grains of qualified quality are obtained by in-situ replication of the original austenite grain boundaries in this embodiment. Figure 3 It can be seen that the original austenite grains of the ZG25MnF low alloy steel casting in the normalized + tempered state of this embodiment are fine, and the grain boundaries are clearly visible, which meets the production inspection requirements.

[0055] Example 2

[0056] This embodiment includes the following steps:

[0057] Step 1: Dissolve 15g of ethyl cellulose in 200mL of anhydrous ethanol and filter. Then, add 0.05g of methyl violet and 10g of polyvinyl alcohol to the filtrate in sequence and stir rapidly for 10min until it is completely dissolved. Then, spread the upper layer of solution by centrifugation. After solidification, obtain the on-site metallographic replica test paper, cut it into 10mm×10mm, and store it in a drying container.

[0058] Step 2: Select a typical area on the surface of a ZG40Cr low alloy steel casting for mining machinery in a normalized + tempered state, and then perform grinding and polishing and corrosion treatment on the selected typical area to obtain a test area; the grinding and polishing process is as follows: use a polishing machine to select a wet sandpaper with a diameter of 20 mm and a mesh number of 280#, and coarsely grind it while adding deionized water at a pressure of 0.05MPa, and then select a wet sandpaper with a diameter of 20 mm and a mesh number of 400#, 600# and 1200#, and gradually finely grind it while adding deionized water at a pressure of 0.05MPa, and then select Use a fluffy polishing cloth and chromium oxide polishing paste to polish while spraying deionized water intermittently at a pressure of 0.05MPa. During the polishing process, the direction of the next polishing is perpendicular to the direction of the previous polishing. After the wear marks of the previous polishing are eliminated, the next polishing is performed. The diameter of the area to be inspected is 10mm. The process of the corrosion treatment is: wipe with absorbent cotton containing 5% hydrochloric acid solution by mass for 40s, then rinse with deionized water, then wipe with absorbent cotton containing 4% nitric acid by mass in anhydrous ethanol solution for 10s, then rinse with anhydrous ethanol and blow dry with hot air;

[0059] Step 3, add 1 drop of anhydrous ethanol to the area to be inspected obtained in step 2, then spread the environmental protection on-site metallographic coating paper prepared in step 1 on the area to be inspected, and press to squeeze out excess anhydrous ethanol and bubbles, pick up the environmental protection on-site metallographic coating paper after standing, install it between two glass slides, and stick it with tape to obtain the metallographic replica paper after the metallographic structure on-site replication, re-perform secondary grinding and polishing and secondary corrosion treatment on the area to be inspected after the metallographic structure on-site replication, and then adopt the same method as the metallographic structure on-site replication to perform the original austenite grain boundary on-site replication to obtain the metallographic replica paper after the original austenite grain boundary on-site replication, and finally compare the metallographic replica paper after the metallographic structure on-site replication and the original austenite grain boundary on-site replication. The metallographic replica paper after the on-site replication of the helium grain boundary is used for observation to obtain the metallographic microstructure of the mining machinery alloy steel casting; the length × width of the metallographic replica paper is 10mm × 10mm, the pressing time is 20s, the standing time is 4min, and the length × width of the slide is 30mm × 100mm; the secondary grinding and polishing process is the same as the grinding and polishing process described in step 2, and the secondary corrosion process is: chemically abrading for 3min with a solution prepared by picric acid, sodium dodecylbenzene sulfonate and the remainder deionized water in a mass ratio of 3.3:1.0:95, then rinsing with deionized water, spraying with anhydrous ethanol, and drying with a hair dryer;

[0060] Step 4: Determine the heat treatment quality of the mining machinery alloy steel castings according to the metallographic microstructure obtained in step 3; the items to be determined are: grain size, residual cast structure and metallographic microstructure category.

[0061] Figure 4This is a physical picture of the environmental protection on-site metallographic coating paper after the on-site metallographic structure replication and the on-site replication of the original austenite grain boundary in step 3 of this embodiment. Figure 4 It can be seen that the two test papers on the left are environmentally friendly on-site metallographic coating papers after on-site replication of the metallographic structure, and the three test papers on the right are environmentally friendly on-site metallographic coating papers after on-site replication of the original austenite grain boundaries. In this embodiment, the metallographic structure of the ZG40Cr low-alloy steel casting in the normalizing + tempering state was replicated on-site, and the environmentally friendly on-site metallographic coating papers clamped in the slide were obtained.

[0062] Figure 5 The metallographic structure obtained after the metallographic structure on-site replication in this embodiment is of unqualified quality. Figure 5 It can be seen that the metallographic structure of the ZG40Cr low alloy steel casting in the normalized + tempered state of this embodiment is primary dendritic ferrite + pearlite, and there is residual cast structure, which needs to be re-heat treated.

[0063] Figure 6 The original austenite grains of this embodiment are obtained by performing on-site replication of the original austenite grain boundaries and are of unqualified quality. Figure 6 It can be seen from the figure that the original austenite grains of the ZG40Cr low alloy steel casting in the normalized + tempered state of this embodiment have mixed crystal phenomenon and coarse original cast grains, which need to be re-heat treated.

[0064] Example 3

[0065] This embodiment includes the following steps:

[0066] Step 1: Dissolve 15g of ethyl cellulose in 200mL of anhydrous ethanol and filter. Then, add 0.05g of methyl violet and 10g of polyvinyl alcohol to the filtrate in sequence and stir rapidly for 10min until it is completely dissolved. Then, spread the upper layer of solution by centrifugation. After solidification, obtain the on-site metallographic replica test paper, cut it into 10mm×10mm, and store it in a drying container.

[0067] Step 2: Select a typical area on the surface of the ZG35CrMoF alloy steel casting of the mining machinery in the normalized + tempered state, and then grind and polish the selected typical area and corrode it to obtain the area to be inspected; the grinding and polishing process is as follows: use a polishing machine to select a 30mm diameter and 320# mesh wet sandpaper for rough grinding and add deionized water at a pressure of 0.05MPa, and then select a 30mm diameter and 400#, 600#, 800# and 1200# mesh wet sandpaper for fine grinding step by step and add deionized water at a pressure of 0.05MPa. water, and then use a fluff polishing cloth and alumina polishing paste to polish while spraying deionized water intermittently at a pressure of 0.05MPa. During the polishing process, the direction of the next polishing is perpendicular to the direction of the previous polishing, and the next polishing is performed after the wear mark of the previous polishing is eliminated; the diameter of the area to be inspected is 20mm; the process of the corrosion treatment is: wipe with absorbent cotton containing 15% hydrochloric acid solution by mass for 20s, then rinse with deionized water, then wipe with absorbent cotton containing 3% nitric acid by mass in anhydrous ethanol solution for 12s, and then rinse with anhydrous ethanol and blow dry with hot air;

[0068] Step 3, add 10 drops of anhydrous ethanol to each area to be inspected obtained in step 2, then spread the environmental protection on-site metallographic coating paper prepared in step 1 on the area to be inspected, and press to squeeze out excess anhydrous ethanol and bubbles, pick up the environmental protection on-site metallographic coating paper after standing, install it between two glass slides, and stick it with tape to obtain the metallographic replica paper after the metallographic structure on-site replication, re-perform secondary grinding and polishing and secondary corrosion treatment on the area to be inspected after the metallographic structure on-site replication, and then adopt the same method as the metallographic structure on-site replication to perform the original austenite grain boundary on-site replication to obtain the metallographic replica paper after the original austenite grain boundary on-site replication, and finally perform the metallographic replica paper and The metallographic replica paper after the on-site replication of the original austenite grain boundary is observed to obtain the metallographic microstructure of the mining machinery alloy steel casting; the length × width of the metallographic replica paper is 10mm × 10mm, the pressing time is 40s, the standing time is 15min, and the size of the slide is 30mm × 100mm; the secondary grinding and polishing process is the same as the grinding and polishing process described in step 2, and the secondary corrosion process is: chemically abrading for 2min using a solution prepared by picric acid, sodium dodecylbenzene sulfonate and the remainder deionized water in a mass ratio of 3.3:1.0:95, then rinsing with deionized water, spraying with anhydrous ethanol, and drying with a hair dryer;

[0069] Step 4: Determine the heat treatment quality of the mining machinery alloy steel castings according to the metallographic microstructure obtained in step 3; the items to be determined are: grain size, residual cast structure and metallographic microstructure category.

[0070] Figure 7This is a physical picture of the environmental protection on-site metallographic coating paper after the on-site metallographic structure replication and the on-site replication of the original austenite grain boundary in step 3 of this embodiment. Figure 7 It can be seen that the two test papers on the left are environmentally friendly on-site metallographic coating papers after on-site replication of the metallographic structure, and the three test papers on the right are environmentally friendly on-site metallographic coating papers after on-site replication of the original austenite grain boundary. In this embodiment, the metallographic structure of the ZG35CrMoF medium alloy steel casting in the normalizing + tempering state was replicated on-site, and the environmentally friendly on-site metallographic coating paper clamped in the slide was obtained.

[0071] Figure 8 This is the qualified metallographic structure obtained after the metallographic structure is replicated on site in this embodiment. Figure 8 It can be seen that the metallographic structure of the alloy steel casting in the normalized + tempered state ZG35CrMoF of this embodiment is clearly visible, the organizational boundary is clear, and the organizational identification is convenient. The metallographic structure is uniform and fine block ferrite + pearlite, which meets the production detection requirements.

[0072] Fig. 9 The original austenite grains of qualified quality are obtained by in-situ replication of the original austenite grain boundaries in this embodiment. Fig. 9 It can be seen that the original austenite grains of the ZG35CrMoF alloy steel casting in the normalizing + tempering state of this embodiment are fine, and the grain boundaries are clearly visible, which meets the production inspection requirements.

[0073] Example 4

[0074] This embodiment includes the following steps:

[0075] Step 1: Dissolve 15g of ethyl cellulose in 200mL of anhydrous ethanol and filter. Then, add 0.05g of methyl violet and 10g of polyvinyl alcohol to the filtrate in sequence and stir rapidly for 10min until it is completely dissolved. Then, spread the upper layer of solution by centrifugation. After solidification, obtain the on-site metallographic replica test paper, cut it into 10mm×10mm, and store it in a drying container.

[0076] Step 2: Select a typical area on the surface of the ZG32CrF alloy steel casting of the mining machinery in the normalized + tempered state, and then grind and polish the selected typical area and corrode the selected typical area to obtain the area to be inspected; the grinding and polishing process is: use a polishing machine to select a 20mm diameter and 200# mesh wet sandpaper for rough grinding and add deionized water at a pressure of 0.05MPa, and then select a 20mm diameter and 400#, 600#, 1000# and 1200# mesh wet sandpaper for fine grinding step by step and add deionized water at a pressure of 0.05MPa. , and then use a fluffy polishing cloth and artificial diamond polishing agent to polish while spraying deionized water intermittently at a pressure of 0.05MPa. During the grinding and polishing treatment, the direction of the next grinding and polishing is perpendicular to the direction of the previous grinding and polishing, and the next grinding and polishing is performed after the wear marks of the previous grinding and polishing are eliminated; the diameter of the area to be inspected is 15mm; the process of the corrosion treatment is: wipe with absorbent cotton containing 10% hydrochloric acid solution by mass for 30s, then rinse with deionized water, then wipe with absorbent cotton containing 4% nitric acid by mass in anhydrous ethanol solution for 15s, and then rinse with anhydrous ethanol and blow dry with hot air;

[0077] Step 3, add 5 drops of anhydrous ethanol to each area to be inspected obtained in step 2, then spread the environmental protection on-site metallographic coating paper prepared in step 1 on the area to be inspected, and press to squeeze out excess anhydrous ethanol and bubbles, pick up the environmental protection on-site metallographic coating paper after standing, install it between two glass slides, and stick it with tape to obtain the metallographic replica paper after the metallographic structure on-site replication, re-perform secondary grinding and polishing and secondary corrosion treatment on the area to be inspected after the metallographic structure on-site replication, and then adopt the same method as the metallographic structure on-site replication to perform the original austenite grain boundary on-site replication to obtain the metallographic replica paper after the original austenite grain boundary on-site replication, and finally compare the metallographic replica paper after the metallographic structure on-site replication and the original austenite grain boundary on-site replication. The metallographic replica paper after the on-site replication of the helium grain boundary is used for observation to obtain the metallographic microstructure of the mining machinery alloy steel casting; the length × width of the metallographic replica paper is 10mm × 10mm, the pressing time is 30s, the standing time is 10min, and the size of the slide is 30mm × 100mm; the secondary grinding and polishing process is the same as the grinding and polishing process described in step 2, and the secondary corrosion process is: chemically abrading for 2.5min using a solution prepared by picric acid, sodium dodecylbenzene sulfonate and the remainder deionized water in a mass ratio of 3.3:1.0:95, then rinsing with deionized water, spraying with anhydrous ethanol, and drying with a hair dryer;

[0078] Step 4: Determine the heat treatment quality of the mining machinery alloy steel castings according to the metallographic microstructure obtained in step 3; the items to be determined are: grain size, residual cast structure and metallographic microstructure category.

[0079] Fig.10This is a physical picture of the environmental protection on-site metallographic coating paper after the on-site metallographic structure replication and the on-site replication of the original austenite grain boundary in step 3 of this embodiment. Fig.10 It can be seen that the two test papers on the left are environmentally friendly on-site metallographic coating papers after on-site replication of the metallographic structure, and the two test papers on the right are environmentally friendly on-site metallographic coating papers after on-site replication of the original austenite grain boundaries. In this embodiment, the metallographic structure of the ZG32CrF medium alloy steel casting in the normalizing + tempering state was replicated on-site, and the environmentally friendly on-site metallographic coating paper clamped in the slide was obtained.

[0080] Fig.11 This is the qualified metallographic structure obtained after the metallographic structure is replicated on site in this embodiment. Fig.11 It can be seen that the metallographic structure of the ZG32CrF alloy steel casting in the normalized + tempered state of this embodiment is primary austenite grain boundary distributed ferrite and a small amount of acicular ferrite growing into the crystal + intracrystalline needle-shaped and blocky ferrite + pearlite, and there is residual cast structure, which needs to be re-heat treated.

[0081] Fig.12 The original austenite grains of qualified quality are obtained by in-situ replication of the original austenite grain boundaries in this embodiment. Fig.12 It can be seen that the original austenite grains of the ZG32CrF alloy steel casting in the normalizing + tempering state of this embodiment have mixed crystal phenomenon and coarse original cast grains, which need to be re-heat treated.

[0082] Example 5

[0083] This embodiment includes the following steps:

[0084] Step 1: Dissolve 15g of ethyl cellulose in 200mL of anhydrous ethanol and filter. Then, add 0.05g of methyl violet and 10g of polyvinyl alcohol to the filtrate in sequence and stir rapidly for 10min until it is completely dissolved. Then, spread the upper layer of solution by centrifugation. After solidification, obtain the on-site metallographic replica test paper, cut it into 10mm×10mm, and store it in a drying container.

[0085] Step 2: Select a typical area on the surface of a ZG25MnF8 high-alloy steel casting for mining machinery in a normalized + tempered + quenched and tempered state, and then perform grinding and polishing and corrosion treatment on the selected typical area to obtain an area to be inspected; the grinding and polishing process is as follows: use an angle grinder to select a nylon polishing sheet with a diameter of 20 mm and add deionized water at a pressure of 0.05 MPa, then select a PVA polishing wheel with a diameter of 20 mm and a particle size of 280#, 400#, 800#, and 1200#, and perform step-by-step fine grinding while adding deionized water at a pressure of 0.05 MPa, and then A felt wheel with a diameter of 20 mm and an artificial diamond polishing agent are used to polish while spraying deionized water at a pressure of 0.05 MPa intermittently. During the polishing treatment, the direction of the next polishing is perpendicular to the direction of the previous polishing, and the next polishing is performed after the wear mark of the previous polishing is eliminated; the diameter of the area to be inspected is 15 mm; the process of the corrosion treatment is: wipe with absorbent cotton containing a mass fraction of 10% hydrochloric acid solution for 20 seconds, then rinse with deionized water, then wipe with absorbent cotton containing a mass fraction of 4% nitric acid anhydrous ethanol solution for 8 seconds, and then rinse with anhydrous ethanol and blow dry with hot air;

[0086] Step 3, add 1 to 10 drops of anhydrous ethanol to each area to be inspected obtained in step 2, then spread the environmental protection on-site metallographic coating paper prepared in step 1 on the area to be inspected, and press to squeeze out excess anhydrous ethanol and bubbles, pick up the environmental protection on-site metallographic coating paper after standing, install it between two glass slides, and stick it with tape to obtain the metallographic replica paper after the metallographic structure on-site replication, re-perform secondary grinding and polishing and secondary corrosion treatment on the area to be inspected after the metallographic structure on-site replication, and then adopt the same method as the metallographic structure on-site replication to perform the original austenite grain boundary on-site replication to obtain the metallographic replica paper after the original austenite grain boundary on-site replication, and finally perform the metallographic replica paper after the metallographic structure on-site replication The metallographic replica paper after the on-site replication of the original austenite grain boundary is observed to obtain the metallographic microstructure of the mining machinery alloy steel casting; the length × width of the metallographic replica paper is 10mm × 10mm, the pressing time is 30s, the standing time is 8min, and the size of the slide is 30mm × 100mm; the secondary grinding and polishing process is the same as the grinding and polishing process described in step 2, and the secondary corrosion process is: chemically abrading for 6min with a solution prepared by picric acid, sodium dodecylbenzene sulfonate and the remainder deionized water in a mass ratio of 3.3:0.5:95, then rinsing with deionized water, spraying with anhydrous ethanol, and drying with a hair dryer;

[0087] Step 4: Determine the heat treatment quality of the mining machinery alloy steel castings according to the metallographic microstructure obtained in step 3; the items to be determined are: grain size, residual cast structure and metallographic microstructure category.

[0088] Fig.13This is a physical picture of the environmental protection on-site metallographic coating paper after the on-site metallographic structure replication and the on-site replication of the original austenite grain boundary in step 3 of this embodiment. Fig.13 It can be seen that the test paper on the left and the two test papers in the middle are environmentally friendly on-site metallographic coating papers after on-site replication of the metallographic structure, and the two test papers on the right are environmentally friendly on-site metallographic coating papers after on-site replication of the original austenite grain boundaries. In this embodiment, the metallographic structure of the ZG25MnF8 high-alloy steel casting in the normalizing + tempering + quenching and tempering state was replicated on-site, and the environmentally friendly on-site metallographic coating paper clamped in the slide was obtained.

[0089] Fig.14 This is the qualified metallographic structure obtained after the metallographic structure is replicated on site in this embodiment. Fig.14 It can be seen that the metallographic structure of the ZG25MnF8 high alloy steel casting in the normalizing + tempering + quenching and tempering state of this embodiment is clearly visible, the organizational boundary is clear, and the organizational identification is convenient. The metallographic structure is fine and uniform tempered troostite, which meets the production detection requirements.

[0090] Fig.15 The original austenite grains of qualified quality are obtained by in-situ replication of the original austenite grain boundaries in this embodiment. Fig.15 It can be seen that the original austenite grains of the ZG25MnF8 high alloy steel casting in the normalized + tempered + quenched and tempered state of this embodiment have fine grains and clearly visible grain boundaries, which meets the production inspection requirements.

[0091] Example 6

[0092] The difference between this embodiment and embodiment 5 is that the corrosion treatment process is: wiping with absorbent cotton containing 5% hydrochloric acid solution by mass for 30 seconds, then rinsing with deionized water, then wiping with absorbent cotton containing 3% nitric acid by mass in anhydrous ethanol solution for 10 seconds, then rinsing with anhydrous ethanol and drying with hot air;

[0093] The process of the secondary corrosion treatment is: chemically abrading for 5 minutes using a high alloy cast steel grain boundary corrosion treatment solution.

[0094] Example 7

[0095] The difference between this embodiment and embodiment 5 is that the corrosion treatment process is: wiping with absorbent cotton containing 15% hydrochloric acid solution by mass for 10 seconds, then rinsing with deionized water, then wiping with absorbent cotton containing 4% nitric acid by mass in anhydrous ethanol solution for 5 seconds, then rinsing with anhydrous ethanol and drying with hot air;

[0096] The process of the secondary corrosion treatment is: chemically abrading for 7 minutes using a high alloy cast steel grain boundary corrosion treatment solution.

[0097] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent changes made to the above embodiments according to the essence of the method of the present invention still fall within the protection scope of the method of the present invention.

Claims

1. A non-destructive testing method for heat treatment quality of alloy steel castings for mining machinery, It is characterized in that The method is used for on-site nondestructive testing of the heat treatment quality of alloy steel castings of mining machinery during processing, and comprises the following steps: Step 1, prepare environmental protection site metallographic coating paper; the preparation process of the environmental protection site metallographic coating paper is: 15g ethyl cellulose is fully dissolved in 200mL anhydrous ethanol and filtered, then 0.05g methyl violet and 10g polyvinyl alcohol are added to the filtrate in sequence and quickly stirred until completely dissolved, then the upper layer solution is spread by centrifugation, and the environmental protection site metallographic coating paper is obtained after solidification, and stored in a drying container Step 2: During the processing, a typical area is selected from the surface of the alloy steel casting of the mining machinery, and then the selected typical area is subjected to grinding and polishing treatment and corrosion treatment to obtain the area to be inspected; the alloy steel casting of the mining machinery is a low-alloy or medium-alloy steel casting or a high-alloy steel casting; when the alloy steel casting of the mining machinery is a low-alloy or medium-alloy steel casting, the grinding and polishing process is as follows: using a polishing machine, selecting wet sandpaper with a mesh number of 200# to 320#, rough grinding while adding deionized water, and then selecting wet sandpaper with a mesh number of 400# to 1200#, step by step, fine grinding while adding deionized water The wet sandpaper and the fluff polishing cloth are both 20 mm in diameter, and the abrasive paste is chromium oxide abrasive paste, aluminum oxide abrasive paste or artificial diamond polishing agent; when the alloy steel castings of the mining machinery are low-alloy and medium-alloy steel castings, the corrosion treatment process is as follows: wipe with absorbent cotton containing hydrochloric acid solution for 20s to 40s, then rinse with deionized water, then wipe with absorbent cotton containing anhydrous ethanol solution of nitric acid for 10s to 15s, then rinse with anhydrous ethanol and blow dry with hot air; Step 3, the area to be inspected obtained in step 2 is subjected to on-site metallographic structure replication and on-site replication of the original austenite grain boundary in turn by using the environmentally friendly on-site metallographic coating paper prepared in step 1 to obtain the microstructure of the typical area of ​​the alloy steel casting for mining machinery; the process of on-site replication of the original austenite grain boundary is as follows: the area to be inspected after the on-site replication of the metallographic structure is subjected to secondary grinding and polishing and secondary corrosion treatment, and then the on-site replication of the original austenite grain boundary is carried out by the same method as the on-site replication of the metallographic structure; the secondary grinding and polishing is the same as the grinding and polishing process described in step 2, and the process of secondary corrosion treatment when the alloy steel casting for mining machinery is a low- and medium-alloy steel casting is as follows: a low- and medium-alloy steel casting grain boundary corrosion treatment solution is used for chemical abrasion for 2 minutes to 3 minutes, and then it is rinsed with deionized water, sprayed with anhydrous ethanol, and then washed with water. Blow dry with a hair dryer; the low and medium alloy steel casting grain boundary corrosion treatment solution is prepared by picric acid, sodium dodecylbenzene sulfonate and the balance deionized water in a mass ratio of 3.3:1.0:95; the process of the metallographic structure on-site replication is: add 1 to 10 drops of solvent to the area to be inspected obtained in step 2, then spread the environmental protection on-site metallographic coating paper prepared in step 1 on the area to be inspected, and press to squeeze out excess solvent and bubbles, connect the environmental protection on-site metallographic coating paper after standing, install it between two glass slides, and stick it with tape, and finally observe the metallographic structure; the solvent is anhydrous ethanol, the environmental protection on-site metallographic coating paper is a square with a side length of 10mm, the pressing time is 20s to 40s, the standing time is 4min to 15min, and the size of the glass slide is 30mm×100mm; Step 4: Determine the heat treatment quality of the alloy steel castings for mining machinery during processing according to the microstructure obtained in step 3; the items for determination are: grain size, residual cast structure and metallographic microstructure category.

2. A nondestructive testing method for heat treatment quality of alloy steel castings for mining machinery according to claim 1, It is characterized in that When the alloy steel castings of the mining machinery described in step 2 are high-alloy steel castings, the grinding and polishing process is as follows: use an angle grinder, select a nylon polishing sheet and perform coarse grinding while adding deionized water, then select a PVA polishing wheel with a particle size of 280#~1200# and perform fine grinding step by step while adding deionized water, and then use a felt wheel and abrasive paste to polish while spraying deionized water, the diameters of the nylon polishing sheet, PVA polishing wheel and felt wheel are all 20mm, and the abrasive paste is an artificial diamond polishing agent; the diameter of each of the areas to be inspected is 10mm~20mm.

3. A nondestructive testing method for heat treatment quality of alloy steel castings for mining machinery according to claim 1, It is characterized in that During the grinding and polishing process in step 2, the direction of the next grinding and polishing is perpendicular to the direction of the previous grinding and polishing, and the next grinding and polishing is performed after the grinding marks of the previous grinding and polishing are eliminated.

4. A nondestructive testing method for heat treatment quality of alloy steel castings for mining machinery according to claim 1, It is characterized in that When the alloy steel castings of the mining machinery described in step 2 are high-alloy steel castings, the corrosion treatment process is: wipe with absorbent cotton containing hydrochloric acid solution for 10s to 30s, then rinse with deionized water, then wipe with absorbent cotton containing anhydrous ethanol solution of nitric acid for 5s to 10s, then rinse with anhydrous ethanol and blow dry with hot air; the mass fraction of the hydrochloric acid solution is 5% to 15%, and the mass fraction of nitric acid in the anhydrous ethanol solution of nitric acid is 3% to 4%.

5. A nondestructive testing method for heat treatment quality of alloy steel castings for mining machinery according to claim 1, It is characterized in that When the alloy steel castings for mining machinery described in step three are high-alloy steel castings, the process of secondary corrosion treatment is as follows: chemically abrade for 5 minutes to 7 minutes using a high-alloy cast steel grain boundary corrosion treatment solution, then rinse with deionized water, spray with anhydrous ethanol, and blow dry with a hair dryer; the high-alloy cast steel grain boundary corrosion treatment solution is prepared with picric acid, sodium dodecylbenzene sulfonate and the remainder deionized water in a mass ratio of 3.3:0.5:95.

Citation Information

Cited By

  • Replication detection method for surface density of hard alloy parts of nuclear power equipment

    CN122238394A