Method and device for preparing back contact heterojunction solar cell
By using chemical vapor deposition method and laser ablation technology to deposit multi-layer films in back-contact heterojunction solar cells, and using inkjet printing and screen printing technology to prepare isolation structures, the complex process and low efficiency in the existing technology are solved. The problem of this has achieved efficient mass production of back-junction contact heterojunction solar cells.
Patent Information
- Application Number
- CN202410201846.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-23
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-02-23
AI Technical Summary
The existing back contact heterojunction solar cells have complex preparation processes and high equipment materials requirements, resulting in low conversion efficiency and difficult to mass production.
Chemical vapor deposition method and laser ablation technology are used to deposit multi-layer films on the back of the silicon wafer, and metal electrodes are prepared by inkjet printing and screen printing technology to form an isolation structure to avoid leakage, simplify the process flow and reduce silicon wafer damage.
It improves the conversion efficiency of solar cells, simplifies the preparation process, reduces the requirements of equipment and materials, and achieves efficient mass production of back-junction and back-contact heterojunction solar cells.
Smart Images

Figure CN118073480B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparation of heterojunction solar cells, and in particular to a preparation method and a device for a back-contact heterojunction solar cell. Background Art
[0002] Back-contact heterojunction solar cells are considered to have the highest efficiency structure among crystalline silicon single-junction solar cells because there is no metal grid blocking the front and amorphous silicon thin film is introduced on the back for efficient surface passivation. It is the only crystalline silicon single-junction cell technology that has the potential to achieve mass production efficiencies exceeding 28%.
[0003] However, despite its potential for ultra-high conversion efficiency, since both the positive and negative electrodes are on the back, the need to prepare positive and negative electrodes with interdigitated spacing has become a difficulty in the preparation process.
[0004] At present, some people have proposed to use multiple mask exposure and development methods to prepare back-junction and back-contact heterojunction solar cells, and have achieved a conversion efficiency of 26.7% in the laboratory. However, this technology is too cumbersome, has very high requirements for equipment and materials, and has a low preparation yield, so it cannot become a mass production process. Summary of the invention
[0005] The present invention aims to at least improve one of the technical problems existing in the prior art. To this end, the present invention provides a method for preparing a back-contact heterojunction solar cell and a device thereof.
[0006] The method for preparing a back-contact heterojunction solar cell according to the first embodiment of the present invention comprises the following steps:
[0007] Step S1, obtaining a double-sided polished and clean silicon wafer, double-sided polishing the surface of the silicon wafer with an alkali or acid solution to remove the cutting damage layer on the surface of the silicon wafer, and then cleaning the silicon wafer with an acid and an alkali solution respectively to remove organic pollutants on the surface of the silicon wafer and remove metal ion pollutants, and finally immersing the silicon wafer in a hydrofluoric acid aqueous solution to remove the oxide layer on the surface of the silicon wafer and drying to obtain a double-sided polished and clean silicon wafer;
[0008] Step S2, using chemical vapor deposition to sequentially deposit three layers of thin films, namely, an intrinsic amorphous silicon thin film, a silicon oxide (or silicon nitride) thin film, and a boron-doped silicon thin film, on the back side of the silicon wafer;
[0009] Step S3, using a short-wavelength nanosecond or picosecond laser with a wavelength less than 500nm to partially ablate the backside boron-doped silicon film, and the silicon oxide underneath reflects the excess laser energy to avoid damaging the amorphous silicon of the substrate;
[0010] Step S4, cleaning the surface of the silicon wafer after ablation, placing the silicon wafer in a wet cleaning device and cleaning the surface of the silicon wafer with an alkaline solution and an acid solution respectively;
[0011] Step S5, depositing a boron-doped silicon film on the back side of the silicon wafer by chemical vapor deposition;
[0012] Step S6, using a short-wave nanosecond or picosecond laser with a wavelength less than 500 nm to groove an area outside the first groove area on the back side of the silicon wafer, which is defined as a second groove area, wherein the second groove area is not connected to the first groove area, and the middle interval of 1um to 30um is a non-grooved area;
[0013] Step S7, cleaning the grooved silicon wafer with a hydrofluoric acid aqueous solution to remove the natural silicon oxide on the front and back sides of the silicon wafer; removing the silicon oxide film in the second grooved area, leaking the intrinsic amorphous silicon in the second grooved area, and finally drying;
[0014] Step S8, spraying a layer of mask material in the first slotted area by inkjet printing; the mask material needs to be easily cleaned by acid or organic matter, and the main purpose of the mask material is to protect the boron-doped silicon film in the first slotted area, and the spraying width is 1um to 30um wider than the first slotted area.
[0015] Step S9, depositing a phosphorus-doped silicon film on the back side of the silicon wafer using a chemical vapor deposition method;
[0016] Step S10: Clean the silicon wafer with an acidic aqueous solution to remove the mask material of the first slotted area on the back of the silicon wafer, and expose the boron-doped silicon film; then clean the silicon wafer with a hydrofluoric acid aqueous solution to remove the natural oxide layer on the front and back sides; at this time, a cross structure of a phosphorus-doped N-type silicon film and a boron-doped P-type silicon film has been formed on the back side, and there is also a layer of silicon oxide film between the P-type film and the N-type film to isolate them, so that the P and N films are not directly connected, completely eliminating the possibility of leakage, which is a prerequisite for obtaining a solar cell with high conversion efficiency;
[0017] Step S11, using chemical vapor deposition to sequentially deposit four layers of thin films, namely, intrinsic amorphous silicon, phosphorus-doped silicon thin film, silicon nitride thin film, and silicon oxynitride thin film, on the front side of the silicon wafer;
[0018] Step S12, depositing a transparent conductive film on the back of the silicon wafer by magnetron sputtering or reactive plasma deposition; the film can be an indium-containing conductive oxide or an indium-free conductive oxide, with a film thickness of 30nm to 300nm and a film refractive index of 1.7 to 3.0.
[0019] The main function of this film is to increase the surface conductivity of the silicon film, increase the back reflection of long-wave incident light, and reduce the contact resistance of the metal interface.
[0020] Step S13, using laser to isolate and scribe the transparent conductive film, wherein the scribe position is between the phosphorus-doped silicon film and the boron-doped silicon film prepared previously, in order to cut off the lateral conduction between the two films, thereby avoiding leakage and reducing the conversion efficiency of the solar cell;
[0021] Step S14, screen printing technology is used to print conductive paste on the back of the battery to form a metal electrode. The conductive paste can be silver paste, copper paste, silver-coated copper paste, carbon paste and other conductive pastes. The electrode includes a main grid and a secondary grid. The width of each electrode grid line cannot be greater than the width of the phosphorus-doped silicon film or the boron-doped silicon film under the grid line to avoid leakage; and the metal electrode above the phosphorus-doped silicon film cannot be connected to the grid line electrode above the boron-doped silicon film, which is also to avoid short circuits and reduce the conversion efficiency of solar cells. The width of the grid line electrode on the phosphorus-doped silicon film is 5um~95um, the width of the electrode above the boron-doped silicon film is 10um~290um, and the height of the grid line electrode is 1um~30um; The method of preparing the grid line electrode can be screen printing or inkjet printing conductive paste technology. The phosphorus-doped film area is the negative electrode of the back-contact heterojunction solar cell, and the boron-doped silicon film area is the positive electrode of the back-contact heterojunction solar cell (where the positive and negative electrodes are strictly prohibited from being connected to each other), and a back-contact heterojunction solar cell is obtained.
[0022] According to the method for preparing a back-contact heterojunction solar cell according to the embodiment of the present invention, the structure of a high-efficiency back-contact heterojunction solar cell can be designed, and a simple process for preparing a high-efficiency cell is proposed; the cell structure prepared by the embodiment of the present invention uses a silicon oxide film to completely isolate the N region and the P region, eliminating the possibility of leakage and greatly improving the cell efficiency; the embodiment of the present invention simultaneously prepares a front-side texturing and a back-side polishing structure, the front-side texturing can fully reduce the surface reflectivity, and the back-side polishing is greatly beneficial to the surface passivation effect, thus fully balancing the photoelectric performance of the solar cell and further improving the cell conversion efficiency. In the embodiment of the present invention, only intrinsic amorphous silicon is deposited on the back side at the beginning and the surface is protected, thus avoiding the situation in which the subsequent grooving, clearing and etching, and then cleaning of the groove cannot be cleaned due to the surface tension of the liquid.
[0023] The embodiment of the present invention is simpler than the traditional three-step mask lithography method, and also reduces one laser process, reduces damage to the silicon wafer, and improves the conversion efficiency of the battery; the application of the technology of the present invention can more efficiently mass-produce back-junction back-contact heterojunction solar cells.
[0024] In a possible implementation manner of the first aspect, in step S2, specifically,
[0025] The first layer of intrinsic amorphous silicon film has a thickness of 3nm to 15nm and a refractive index range of 3.5 to 4.5, and is used to passivate dangling bonds on the surface of the silicon wafer and reduce the surface defect state density;
[0026] The second silicon oxide film is any one of aluminum oxide, silicon nitride, and silicon oxynitride, with a film thickness of 10nm to 200nm and a refractive index range of 1.4 to 3.0, and is used to protect the underlying amorphous silicon layer from subsequent etching by an alkaline solution;
[0027] The third layer of boron-doped silicon film is an amorphous silicon film or a boron-doped microcrystalline silicon film with a film thickness of 10nm to 100nm and a refractive index range of 2.2 to 4.5. It is used to protect silicon oxide (aluminum oxide, silicon nitride, silicon oxynitride and other films) from being etched by acidic solutions.
[0028] In a possible implementation manner of the first aspect, step S4 specifically includes:
[0029] In step S41, potassium hydroxide solution is first used to texture the silicon wafer. At this time, the front side of the silicon wafer is transformed from the polished surface into a pyramid-structured texture surface, which is used to reduce the surface reflectivity of the silicon wafer. Since the back side is protected by a boron-doped silicon film and a silicon oxide film, both of which are resistant to alkali corrosion, the back side morphology and structure will not change.
[0030] Step S42, using hydrofluoric acid aqueous solution to clean the silicon wafer, the front silicon will not react with hydrofluoric acid, so the pyramid structure will not change, and the back boron-doped silicon film will not react with hydrofluoric acid, but the silicon oxide film leaked under the laser ablation area will react with hydrofluoric acid, so it will be etched away, so that the intrinsic amorphous silicon film leaks out of the groove; but the intrinsic amorphous silicon film does not react with the hydrofluoric acid aqueous solution, so it is not affected;
[0031] Step S43, using a dilute potassium hydroxide solution to clean the silicon wafer. The dilute alkali solution will slightly round the pyramid tip and the bottom of the pyramid, which is more conducive to subsequent surface passivation and improves battery efficiency. The boron-doped silicon film on the back is not etched by the alkali, while the phosphorus-doped silicon film in the groove will be etched by the alkali, and the intrinsic amorphous silicon will also be etched by the alkali, so the silicon surface is left in the groove.
[0032] Step S44, using hydrofluoric acid aqueous solution to clean the silicon wafer, remove the silicon oxide on the front and back sides of the silicon wafer and in the grooves, and finally dry it.
[0033] In a possible implementation of the first aspect, the boron-doped silicon film in step S5 is any one of an amorphous silicon film, a microcrystalline silicon film or a microcrystalline silicon oxide film, the thickness of the boron-doped silicon film is 3nm to 40nm, and the refractive index ranges from 2.0 to 4.8; the purpose is to form a PN junction with an N-type substrate silicon wafer.
[0034] In a possible implementation of the first aspect, in step S6, the laser wavelength is between 200nm and 500nm, the laser type is one of nanosecond laser, femtosecond laser or picosecond laser, the frequency is 10E12Hz to 10E19Hz, and the laser slot width is 10um to 100um. For this type of laser, the absorption coefficient of the boron-doped silicon film is much larger than that of the silicon oxide film, and the silicon oxide film also has a strong reflectivity for the laser in this band, and can reflect more than 80% of the residual laser energy. Therefore, most of the laser energy is absorbed by the boron-doped silicon film, so that the local boron-doped silicon film is instantly vaporized and leaks out of the silicon oxide film underneath; if other types of lasers are used, they will penetrate the silicon oxide and damage the passivation effect of the intrinsic amorphous silicon, which will lead to a decrease in the battery conversion efficiency.
[0035] In a possible implementation of the first aspect, the phosphorus-doped silicon film in step S9 is any one of an amorphous silicon film, a microcrystalline silicon film or a microcrystalline silicon oxide film, and the thickness of the phosphorus-doped silicon film is 4nm to 30nm, and the refractive index ranges from 2.2 to 4.5; it is used to further provide a field passivation effect of the phosphorus-doped silicon film and improve the battery conversion efficiency.
[0036] In a possible implementation manner of the first aspect, in step S11, specifically,
[0037] The first layer of intrinsic amorphous silicon film has a thickness of 4nm to 10nm and a refractive index range of 3.5 to 4.4, and is used to passivate dangling bonds on the surface of the silicon wafer and reduce the surface defect state density;
[0038] The second phosphorus-doped silicon film is any one of an amorphous silicon film, a microcrystalline silicon film, and a microcrystalline silicon oxide film, with a film thickness of 4nm to 30nm and a refractive index range of 2.2 to 4.5, and is used to provide a field passivation effect for the surface and improve the battery conversion efficiency;
[0039] The third layer of silicon nitride film has a thickness of 10 nm to 80 nm and a refractive index ranging from 1.5 to 3.5;
[0040] The fourth layer of silicon oxynitride film has a thickness of 30 to 100 nm and a refractive index range of 1.5 to 3.0. The third layer of silicon nitride film and the fourth layer of silicon oxynitride film are used to form a double-layer anti-reflection film structure to further reduce the reflectivity of the silicon wafer surface.
[0041] In a possible implementation of the first aspect, in step S13, the width of the laser scribing is 1um to 20um, the laser wavelength is between 200nm and 500nm, and the frequency is 10E12Hz to 10E19Hz, which can better isolate the lateral conduction between the two thin films and avoid leakage current that reduces the conversion efficiency of the solar cell.
[0042] In a possible implementation manner of the first aspect, the type of laser is any one of nanosecond laser, femtosecond laser or picosecond laser.
[0043] According to the second aspect of the present invention, a device for preparing a back-contact heterojunction solar cell is provided, wherein the device executes the above-mentioned method for preparing a back-contact heterojunction solar cell to prepare a heterojunction solar cell. The device for preparing a back-contact heterojunction solar cell based on the method for preparing a back-contact heterojunction solar cell of the present invention effectively utilizes the convenience of laser ablation for preparing graphic patterns, and also uses an inkjet mask method to reduce the disadvantage of multiple laser ablation causing intrinsic amorphous silicon passivation failure, and finally introduces an efficient and simple process technology route, which is expected to promote the large-scale mass production of high-efficiency back-junction back-contact heterojunction solar cells.
[0044] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0046] Figure 1 is a flow chart of a method for preparing a back-contact heterojunction solar cell according to an embodiment of the present invention;
[0047] Figure 2 Schematic diagram of the preparation process stages of a back-contact heterojunction solar cell according to an embodiment of the present invention. DETAILED DESCRIPTION
[0048] The embodiments of the present invention are described in detail below. The embodiments described with reference to the accompanying drawings are exemplary. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0049] It should be noted that when an element is referred to as being "fixed to" another element, it may be directly on the other element or there may be an intermediate element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be an intermediate element at the same time.
[0050] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.
[0051] The terms "first", "second", "third", etc. in the specification and claims of the present application and the drawings are used to distinguish different objects rather than to describe a specific order. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions. For example, a series of steps or units are included, or optionally, steps or units not listed are included, or optionally, other steps or units inherent to these processes, methods, products or devices are included.
[0052] Only the part relevant to the present application is shown in the accompanying drawings, but not all of the content. Before discussing the exemplary embodiments in more detail, it should be mentioned that some exemplary embodiments are described as processing or methods depicted as flow charts. Although the flow chart describes each operation (or step) as a sequential process, many of the operations therein can be implemented in parallel, concurrently or simultaneously. In addition, the order of each operation can be rearranged. When its operation is completed, the process can be terminated, but it can also have additional steps not included in the accompanying drawings. The process can correspond to a method, function, procedure, subroutine, subprogram, etc.
[0053] The terms "component", "module", "system", "unit", etc. used in this specification are used to represent computer-related entities, hardware, firmware, a combination of hardware and software, software, or software in execution. For example, a unit can be, but is not limited to, a process running on a processor, a processor, an object, an executable file, an execution thread, a program, and / or distributed between two or more computers. In addition, these units can be executed from various computer-readable media having various data structures stored thereon. Units can communicate through local and / or remote processes, for example, based on signals having one or more data packets (e.g., data from a second unit interacting with another unit in a local system, a distributed system, and / or a network. For example, the Internet interacts with other systems via signals).
[0054] Example 1
[0055] See also Figure 1 and Figure 2 As shown, this embodiment provides a method for preparing a back-contact heterojunction solar cell, which includes the following steps:
[0056] Step S1, prepare a double-sided polished and clean silicon wafer, use an alkali or acid solution to double-sided polish the surface of the silicon wafer to remove the cutting damage layer on the surface of the silicon wafer, then use an acid and alkali solution to clean the silicon wafer respectively, the purpose is to remove organic pollutants on the surface of the silicon wafer and remove metal ion pollutants, finally immerse the silicon wafer in a hydrofluoric acid aqueous solution to remove the oxide layer on the surface of the silicon wafer and dry it to obtain a double-sided polished and clean silicon wafer, such as Figure 2 As shown in (a);
[0057] Step S2, using chemical vapor deposition to sequentially deposit three layers of thin films, namely, an intrinsic amorphous silicon film, a silicon oxide (or silicon nitride) film, and a boron-doped silicon film, on the back of the silicon wafer. Figure 2 As shown in (b), the first layer of intrinsic amorphous silicon film has a thickness of 3 nm to 15 nm and a refractive index range of 3.5 to 4.5, and is used to passivate dangling bonds on the surface of the silicon wafer and reduce the surface defect state density;
[0058] The second silicon oxide film is any one of aluminum oxide, silicon nitride, and silicon oxynitride, with a film thickness of 10nm to 200nm and a refractive index range of 1.4 to 3.0, and is used to protect the underlying amorphous silicon layer from subsequent etching by an alkaline solution;
[0059] The third layer of boron-doped silicon film is an amorphous silicon film or a boron-doped microcrystalline silicon film, with a film thickness of 10nm to 100nm and a refractive index range of 2.2 to 4.5, and is used to protect silicon oxide (aluminum oxide, silicon nitride, silicon oxynitride and other films) from being etched by acidic solutions;
[0060] Step S3, using a short-wavelength nanosecond or picosecond laser with a wavelength less than 500nm to partially ablate the backside boron-doped silicon film, the silicon oxide underneath reflects the excess laser energy to avoid damaging the amorphous silicon of the substrate, such as Figure 2 As shown in (c);
[0061] Step S4, cleaning the surface of the silicon wafer after ablation, placing the silicon wafer in a wet cleaning device and cleaning the surface of the silicon wafer with an alkaline solution and an acid solution respectively, such as Figure 2 As shown in (d), it includes:
[0062] Step S41, first use potassium hydroxide solution to texture the silicon wafer, at this time the front side of the silicon wafer is formed into a pyramid-structured texture surface by the polished surface; it is used to reduce the surface reflectivity of the silicon wafer; wherein the back side is protected by a boron-doped silicon film and a silicon oxide film, both of which are resistant to alkali corrosion, so the back side morphology and structure will not change.
[0063] Step S42, using hydrofluoric acid aqueous solution to clean the silicon wafer, the front silicon will not react with hydrofluoric acid, so the pyramid structure will not change, and the back boron-doped silicon film will not react with hydrofluoric acid, but the silicon oxide film leaked under the laser ablation area will react with hydrofluoric acid, so it will be etched away, so that the intrinsic amorphous silicon film leaks out of the groove; but the intrinsic amorphous silicon film does not react with the hydrofluoric acid aqueous solution, so it is not affected;
[0064] Step S43, using a dilute potassium hydroxide solution to clean the silicon wafer. The dilute alkali solution will slightly round the pyramid tip and the bottom of the pyramid, which is more conducive to subsequent surface passivation and improves battery efficiency. The boron-doped silicon film on the back is not etched by the alkali, while the phosphorus-doped silicon film in the groove will be etched by the alkali, and the intrinsic amorphous silicon will also be etched by the alkali, so the silicon surface is left in the groove.
[0065] Step S44, using hydrofluoric acid aqueous solution to clean the silicon wafer, remove the silicon oxide on the front and back sides of the silicon wafer and in the grooves, and finally dry it.
[0066] Step S5, depositing a boron-doped silicon film on the back of the silicon wafer by chemical vapor deposition, such as Figure 2 As shown in (e);
[0067] Step S6, using a short-wave nanosecond or picosecond laser with a wavelength less than 500nm to groove the area outside the first groove area on the back of the silicon wafer, which is defined as the second groove area, and the second groove area and the first groove area are not connected to each other, and the middle interval of 1um to 30um is a non-grooved area, such as Figure 2 As shown in (f);
[0068] Step S7, cleaning the grooved silicon wafer with a hydrofluoric acid aqueous solution to remove the natural silicon oxide on the front and back sides of the silicon wafer; removing the silicon oxide film in the second grooved area, leaking the intrinsic amorphous silicon in the second grooved area, and finally drying. Figure 2 As shown in (g);
[0069] Step S8, spraying a layer of mask material in the first slotted area by inkjet printing; the mask material needs to be easily cleaned by acid or organic matter, and the main purpose of the mask material is to protect the boron-doped silicon film in the first slotted area. The spraying width is 1um to 30um wider than the first slotted area. Figure 2As shown in (h) in .
[0070] Step S9, using chemical vapor deposition to deposit a phosphorus-doped silicon film on the back of the silicon wafer, such as Figure 2 As shown in (i);
[0071] Step S10: Clean the silicon wafer with an acidic aqueous solution to remove the mask material of the first slotted area on the back of the silicon wafer, and expose the boron-doped silicon film; then use a hydrofluoric acid aqueous solution to clean the silicon wafer to remove the natural oxide layer on the front and back sides; at this time, a cross structure of a phosphorus-doped N-type silicon film and a boron-doped P-type silicon film has been formed on the back side, and there is a layer of silicon oxide film between the P-type film and the N-type film to isolate the P and N films, so that the P and N films are not directly connected, completely eliminating the possibility of leakage, which is a prerequisite for obtaining high conversion efficiency solar cells, such as Figure 2 As shown in (j);
[0072] Step S11, using chemical vapor deposition method to sequentially deposit four layers of thin films, namely, intrinsic amorphous silicon, phosphorus-doped silicon thin film, silicon nitride thin film and silicon oxynitride thin film, on the front side of the silicon wafer. Figure 2 As shown in (k), the first layer of intrinsic amorphous silicon film has a thickness of 4 nm to 10 nm and a refractive index range of 3.5 to 4.4, which is used to passivate dangling bonds on the surface of the silicon wafer and reduce the surface defect state density;
[0073] The second phosphorus-doped silicon film is any one of an amorphous silicon film, a microcrystalline silicon film, and a microcrystalline silicon oxide film, with a film thickness of 4nm to 30nm and a refractive index range of 2.2 to 4.5, and is used to provide a field passivation effect for the surface and improve the battery conversion efficiency;
[0074] The third layer of silicon nitride film has a thickness of 10 nm to 80 nm and a refractive index ranging from 1.5 to 3.5;
[0075] The fourth layer of silicon oxynitride film has a thickness of 30 to 100 nm and a refractive index range of 1.5 to 3.0. The third layer of silicon nitride film and the fourth layer of silicon oxynitride film are used to form a double-layer anti-reflection film structure to further reduce the reflectivity of the silicon wafer surface.
[0076] Step S12, depositing a transparent conductive film on the back of the silicon wafer by magnetron sputtering or reactive plasma deposition; the film can be a conductive oxide containing indium or a conductive oxide not containing indium, the film thickness is 30nm to 300nm, and the film refractive index is between 1.7 and 3.0, such as Figure 2 As shown in (l) in .
[0077] The main function of this film is to increase the surface conductivity of the silicon film, increase the back reflection of long-wave incident light, and reduce the contact resistance of the metal interface.
[0078] Step S13, using laser to isolate and scribe the transparent conductive film, wherein the scribe position is between the phosphorus-doped silicon film and the boron-doped silicon film prepared previously, in order to cut off the lateral conduction between the two films, to avoid leakage and reduce the conversion efficiency of the solar cell, such as Figure 2 As shown in (m);
[0079] Step S14, using screen printing technology to print conductive paste on the back of the battery to form a metal electrode. The conductive paste can be silver paste, copper paste, silver-coated copper paste, carbon paste and other conductive pastes. The electrode includes a main grid and a secondary grid. The width of each electrode grid line cannot be greater than the width of the phosphorus-doped silicon film or the boron-doped silicon film under the grid line to avoid leakage; and the metal electrode above the phosphorus-doped silicon film cannot be connected to the grid line electrode above the boron-doped silicon film, also to avoid short circuits and reduce the conversion efficiency of the solar cell. The width of the grid line electrode on the phosphorus-doped silicon film is 5um~95um, the width of the electrode above the boron-doped silicon film is 10um~290um, and the height of the grid line electrode is 1um~30um; The method of preparing the grid line electrode can be screen printing or inkjet printing conductive paste technology. The phosphorus-doped film area is the negative electrode of the back-contact heterojunction solar cell, and the boron-doped silicon film area is the positive electrode of the back-contact heterojunction solar cell (where the positive and negative electrodes are strictly prohibited from being connected to each other), so as to obtain a back-contact heterojunction solar cell, such as Figure 2 As shown in (n) in .
[0080] According to the method for preparing a back-contact heterojunction solar cell according to the embodiment of the present invention, the structure of a high-efficiency back-contact heterojunction solar cell can be designed, and a simple process for preparing a high-efficiency cell is proposed; the cell structure prepared by the embodiment of the present invention uses a silicon oxide film to completely isolate the N region and the P region, eliminating the possibility of leakage and greatly improving the cell efficiency; the embodiment of the present invention simultaneously prepares a front-side texturing and a back-side polishing structure, the front-side texturing can fully reduce the surface reflectivity, and the back-side polishing is greatly beneficial to the surface passivation effect, thus fully balancing the photoelectric performance of the solar cell and further improving the cell conversion efficiency. In the embodiment of the present invention, only intrinsic amorphous silicon is deposited on the back side at the beginning and the surface is protected, thus avoiding the situation in which the subsequent grooving, clearing and etching, and then cleaning of the groove cannot be cleaned due to the surface tension of the liquid.
[0081] The embodiment of the present invention is simpler than the traditional three-step mask lithography method, and also reduces one laser process, reduces damage to the silicon wafer, and improves the conversion efficiency of the battery; the application of the technology of the present invention can more efficiently mass-produce back-junction back-contact heterojunction solar cells.
[0082] It should be noted that the boron-doped silicon film in step S5 is any one of an amorphous silicon film, a microcrystalline silicon film or a microcrystalline silicon oxide film, the thickness of the boron-doped silicon film is 3nm to 40nm, and the refractive index ranges from 2.0 to 4.8; the purpose is to form a PN junction with an N-type substrate silicon wafer.
[0083] It should be noted that in step S6, the laser wavelength is between 200nm and 500nm, the laser type is one of nanosecond laser, femtosecond laser or picosecond laser, the frequency is 10E12Hz to 10E19Hz, and the laser slot width is 10um to 100um. For this type of laser, the absorption coefficient of the boron-doped silicon film is much larger than that of the silicon oxide film, and the silicon oxide film also has a strong reflectivity for the laser in this band, and can reflect more than 80% of the residual laser energy. Therefore, most of the laser energy is absorbed by the boron-doped silicon film, causing the local boron-doped silicon film to instantly vaporize and leak out the silicon oxide film underneath; if other types of lasers are used, they will penetrate the silicon oxide and damage the passivation effect of the intrinsic amorphous silicon, which will lead to a decrease in the battery conversion efficiency.
[0084] It should be noted that the phosphorus-doped silicon film in step S9 is any one of an amorphous silicon film, a microcrystalline silicon film or a microcrystalline silicon oxide film, and the thickness of the phosphorus-doped silicon film is 4nm to 30nm, and the refractive index ranges from 2.2 to 4.5; it is used to further provide a field passivation effect of the phosphorus-doped silicon film and improve the battery conversion efficiency.
[0085] It should be noted that in step S13, the width of the laser scribing is 1um to 20um, the laser wavelength is between 200nm and 500nm, the laser type is any one of nanosecond laser, femtosecond laser or picosecond laser, and the frequency is 10E12Hz to 10E19Hz, which can better isolate the lateral conduction between the two layers of film and avoid leakage to reduce the conversion efficiency of the solar cell.
[0086] Example 2
[0087] The present embodiment provides a device for preparing a back-contact heterojunction solar cell, wherein the device executes the above-mentioned method for preparing a back-contact heterojunction solar cell to prepare a heterojunction solar cell. The preparation device of the method for preparing a back-contact heterojunction solar cell based on the embodiment of the present invention effectively utilizes the convenience of laser ablation to prepare graphic patterns, and also uses an inkjet mask method to reduce the disadvantage of intrinsic amorphous silicon passivation failure caused by multiple laser ablation, and finally introduces an efficient and simple process technology route, which is expected to promote the large-scale mass production of high-efficiency back-junction back-contact heterojunction solar cells.
[0088] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention.
[0089] In the description of the present invention, it is to be understood that the terms “center”, “longitudinal”, “lateral”, “length”, “width”, “thickness”, “up”, “down”, “front”, “back”, “left”, “right”, “vertical”, “horizontal”, “top”, “bottom”, “inside”, “outside”, “clockwise”, “counterclockwise”, “axial”, “radial”, “circumferential”, etc., indicating orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation to the invention.
[0090] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example.
[0091] Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all the embodiments. Mentioning "embodiment" in this article means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present embodiment application. The appearance of this phrase in various positions in the specification is not necessarily the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It can be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0092] Although the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the claims and their equivalents.
Claims
1. A method for preparing a back-contact heterojunction solar cell, characterized in that: The steps include: Step S1, preparing a double-sided polished and clean silicon wafer, polishing the surface of the silicon wafer to remove the cutting damage layer, then cleaning, removing the surface oxide layer and drying to obtain a double-sided polished and clean silicon wafer; Step S2, depositing an intrinsic amorphous silicon film, a silicon oxide film and a boron-doped silicon film on the back of the silicon wafer in sequence; Step S3, using a laser with a wavelength less than 500 nm to ablate the back side boron-doped silicon film; Step S4, cleaning the surface of the silicon wafer after ablation; Step S5, depositing a boron-doped silicon film on the back side of the silicon wafer; Step S6, groove the area outside the first groove area on the back side of the silicon wafer, which is defined as a second groove area, wherein a non-grooved area of 1 um to 30 um is spaced between the second groove area and the first groove area; Step S7, cleaning the grooved silicon wafer to remove the natural silicon oxide on the front and back sides of the silicon wafer; at the same time, removing the silicon oxide film in the second grooved area, leaking the intrinsic amorphous silicon in the second grooved area, and drying; Step S8, spraying a layer of mask material in the first grooved area of the silicon wafer; Step S9, depositing a phosphorus-doped silicon film on the back side of the silicon wafer; Step S10: cleaning the silicon wafer, removing the mask material in the first grooved area on the back side of the silicon wafer, exposing the boron-doped silicon film, and then cleaning the silicon wafer; Step S11, depositing intrinsic amorphous silicon, phosphorus-doped silicon film, silicon nitride film and silicon oxynitride film in sequence on the front side of the silicon wafer; Step S12, depositing a transparent conductive film on the back of the silicon wafer; Step S13, isolating and scribing the transparent conductive film, wherein the scribing position is between the prepared phosphorus-doped silicon film and the boron-doped silicon film; Step S14, printing a conductive paste on the back of the battery to form a metal electrode, wherein the phosphorus-doped thin film area is the negative electrode of the back-contact heterojunction solar cell, and the boron-doped silicon thin film area is the positive electrode of the back-contact heterojunction solar cell, to obtain a back-contact heterojunction solar cell.
2. The method for preparing a back-contact heterojunction solar cell according to claim 1, characterized in that: In step S2, specifically, The thickness of the first layer of intrinsic amorphous silicon film is 3nm to 15nm, and the refractive index ranges from 3.5 to 4.5; The second silicon oxide film is silicon oxynitride, with a film thickness of 10nm to 200nm and a refractive index ranging from 1.4 to 3.0; The third boron-doped silicon film is an amorphous silicon film or a boron-doped microcrystalline silicon film, with a film thickness of 10 nm to 100 nm and a refractive index ranging from 2.2 to 4.
5.
3. The method for preparing a back-contact heterojunction solar cell according to claim 1, characterized in that: The step S4 specifically includes: Step S41, using potassium hydroxide solution to texture the silicon wafer, at this time, the front side of the silicon wafer is transformed from the polished surface to a textured surface with a pyramid structure; Step S42, cleaning the silicon wafer with a hydrofluoric acid aqueous solution; Step S43, cleaning the silicon wafer with a dilute potassium hydroxide solution; Step S44, using hydrofluoric acid aqueous solution to clean the silicon wafer, remove the silicon oxide on the front and back sides of the silicon wafer and in the grooves, and finally dry it.
4. The method for preparing a back-contact heterojunction solar cell according to claim 1, characterized in that: The boron-doped silicon film in step S5 is any one of an amorphous silicon film and a microcrystalline silicon film, and the boron-doped silicon film has a thickness of 3 nm to 40 nm and a refractive index range of 2.0 to 4.
8.
5. The method for preparing a back-contact heterojunction solar cell according to claim 1, characterized in that: In step S3, the laser wavelength is between 200nm and 500nm, the laser type is any one of nanosecond laser, femtosecond laser or picosecond laser, the frequency is 10E12Hz to 10E19Hz, and the laser slot width is 10um to 100um.
6. The method for preparing a back-contact heterojunction solar cell according to claim 1, characterized in that: The phosphorus-doped silicon film in step S9 is any one of an amorphous silicon film and a microcrystalline silicon film. The phosphorus-doped silicon film has a thickness of 4 nm to 30 nm and a refractive index range of 2.2 to 4.
5.
7. The method for preparing a back-contact heterojunction solar cell according to claim 1, characterized in that: In step S11, specifically, The thickness of the first layer of intrinsic amorphous silicon film is 4nm to 10nm, and the refractive index ranges from 3.5 to 4.4; The second phosphorus-doped silicon film is any one of an amorphous silicon film and a microcrystalline silicon film, the film thickness is 4nm to 30nm, and the refractive index ranges from 2.2 to 4.5; The third layer of silicon nitride film has a thickness of 10 nm to 80 nm and a refractive index ranging from 1.5 to 3.5; The fourth silicon oxynitride film has a thickness of 30 to 100 nm and a refractive index ranging from 1.5 to 3.
0.
8. The method for preparing a back-contact heterojunction solar cell according to claim 1, characterized in that: In step S13, laser is used to isolate and scribe the transparent conductive film, the width of the laser scribe is 1 um to 20 um, the laser wavelength is between 200 nm and 500 nm, and the frequency is 10E12 Hz to 10E19 Hz.
9. The method for preparing a back-contact heterojunction solar cell according to claim 8, characterized in that: The type of laser is any one of nanosecond laser, femtosecond laser or picosecond laser.