A metal organic framework composite membrane and its preparation method and application

By loading a metal-organic framework composite membrane of NH2-Fe-Co-MIL-88B and CaO2 particles on a PVDF membrane, the problem of excessive residual H2O2 when MOF nanozymes degrade aflatoxins is solved, achieving efficient and safe aflatoxin removal. Degradation improves the safety and recyclability of food handling.

CN118079679BActive Publication Date: 2024-10-01NAN JING SHI FAN DA XUE CHANG ZHOU HE CHENG SHENG WU XUE CHAN YE YAN JIU YUAN YOU XIAN GONG SI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410206636.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-26
Publication Date
2024-10-01
Estimated Expiration
2044-02-26

AI Technical Summary

Technical Problem

When the existing technology uses MOF nanozymes to degrade aflatoxin, it may lead to excessive residual H2O2, affecting food and human health.

Method used

A metal-organic framework composite membrane is used, including NH2-Fe-Co-MIL-88B nanoparticles and CaO2 particles supported by a PVDF membrane, which is prepared by ultrasonic dispersion and non-solvent-induced phase separation to form a membrane catalytic reaction with efficient degradation of aflatoxins. device to avoid excessive H2O2 residue.

Benefits of technology

It achieves a 95% aflatoxin degradation rate, avoids the damage of food nutrition by H2O2, improves recyclability and stability, and reduces the risk of heavy metal pollution and secondary pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118079679B_ABST
    Figure CN118079679B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of toxin removal in food, and discloses a metal organic framework composite membrane and a preparation method and application thereof, comprising a PVDF membrane and metal organic framework NH2-Fe-Co-MIL-88B nanoparticles and CaO2 particles loaded on the PVDF membrane; wherein the mass ratio of NH2-Fe-Co-MIL-88B:CaO2:PVDF is (0.1-2):(1-15):15; the metal organic framework composite membrane can be used to degrade aflatoxins in food, especially AFB1 and AFM1 in milk; NH2-Fe-Co-MIL-88B and CaO2 are added to the composite membrane at the same time, and compared with a traditional removal method, the composite membrane can efficiently degrade aflatoxins in milk into non-toxic and harmless small molecules by in-situ controllable generation of H2O2 and combining with NH2-Fe-Co-MIL-88B with peroxidase-like activity, and can achieve an efficient degradation rate of 95%, while avoiding the damage of H2O2 required for peroxidase-like activity to food nutrition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of toxin removal in food, and in particular to a metal organic framework composite membrane and a preparation method and application thereof. Background Art

[0002] Aflatoxins are carcinogenic biological toxins produced by Aspergillus flavus and Aspergillus parasiticus, among which AFB1 is the most toxic and carcinogenic. AFB1 is also highly chemically and thermally stable, and is widely found in agricultural products such as corn and peanuts and their processed products. It may also derive new aflatoxins, such as AFM1. When animals such as cattle eat feed containing AFB1, related biological reactions occur in the body to produce AFM1, which accumulates in milk and causes health hazards to humans.

[0003] Traditional methods for degrading aflatoxin include ozone treatment, ultraviolet degradation, and fermentation degradation by fungi or bacteria, which usually require high conditions and energy consumption, and the degradation efficiency is not ideal. Nanozymes have received more and more attention and applications due to their excellent catalytic activity, stability and versatility. There are many applications of nanozyme-based peroxidase-like catalysis for the treatment of organic pollutants in wastewater, but there is almost no treatment of food, especially liquid food. After nanozymes enter the aqueous solution, due to their nanopowder characteristics, they will be easy to aggregate and difficult to recover, which may lead to reduced catalytic activity and secondary pollution. Due to the characteristics of peroxidase, the addition of H2O2 will also cause excessive residual H2O2 to affect human health. The catalyst is fixed on the membrane to form a membrane catalytic reactor through catalytic membrane technology, which does not require particle separation and recovery. PVDF membrane has been widely used as a membrane with high mechanical strength, thermal stability, chemical corrosion resistance and hydrophobicity. Peroxidase Fe / Co-MIL-88B (NH2) is a highly efficient degradation enzyme, but since hydrogen peroxide needs to be added, its use in the food field may destroy nutrients such as protein in food. For this reason, we proposed a new strategy for controllable in situ generation of H2O2 in combination with nanozymes. CaO2 is used to provide MOF nanozymes with stable and controllable H2O2 to degrade aflatoxin, avoiding the damage that excessive H2O2 may cause to food and human health. Summary of the invention

[0004] The purpose of the present invention is to provide a metal organic framework composite membrane and a preparation method and application thereof, so as to solve the problem that excessive H2O2 residue may be caused when MOF nanozymes are used to degrade aflatoxin in the prior art.

[0005] In order to solve the above technical problems, the present invention specifically provides the following technical solutions:

[0006] A metal organic framework composite membrane, comprising a PVDF membrane and metal organic framework NH2-Fe-Co-MIL-88B nanoparticles and CaO2 particles loaded on the PVDF membrane;

[0007] Among them, the mass ratio of NH2-Fe-Co-MIL-88B:CaO2:PVDF is (0.1-2):(1-15):15.

[0008] Furthermore, the CaO2 particles surround the NH2-Fe-Co-MIL-88B nanoparticles.

[0009] Furthermore, the mass ratio of NH2-Fe-Co-MIL-88B:CaO2:PVDF is 0.5:10:15.

[0010] Furthermore, the thickness of the composite film is 200 μm.

[0011] The present invention also provides a method for preparing the metal organic framework composite film, comprising the following steps:

[0012] Step 1, ultrasonically dispersing NH2-Fe-Co-MIL-88B nanoparticles and CaO2 particles in DMF solvent to obtain a suspension;

[0013] Step 2, adding PVDF powder into the suspension to obtain a casting liquid;

[0014] Step 3: coating the casting liquid on the flat substrate to obtain a composite film on the surface of the flat substrate, and washing the composite film with ultrapure water to remove residual solvent.

[0015] Furthermore, the NH2-Fe-Co-MIL-88B is prepared by the following method: FeCl3﹒6H2O, Co(NO3)2﹒6H2O, and H2(NH2)BDC are dissolved in DMF in a mass ratio of 82:90:53:3181, stirred for 30-60 minutes, reacted at 118-122°C for 22-26 hours, naturally cooled to room temperature, collected the powdered product and washed it with DMF, and dried at 60°C for 8-10 hours to obtain NH2-Fe-Co-MIL-88B.

[0016] Furthermore, in step 2, after adding the PVDF powder to the suspension, mechanical stirring is performed at 45-55°C for 3-5 hours to form a casting liquid, and the casting liquid is degassed at a constant temperature for 4-6 hours to eliminate bubbles.

[0017] The above metal organic framework composite membrane can be used to degrade aflatoxin in food.

[0018] Preferably, the aflatoxins are AFB1 and AFM1.

[0019] Preferably, the food is milk.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] (1) NH2-Fe-Co-MIL-88B and CaO2 are added to the composite membrane of the present invention at the same time. Compared with the traditional removal method, the composite membrane of the present invention can efficiently degrade aflatoxin in milk into non-toxic and harmless small molecules by in-situ controllable generation of H2O2 and combining it with NH2-Fe-Co-MIL-88B with peroxidase-like activity, and can achieve an efficient degradation rate of 95%, while avoiding the damage of H2O2 required for peroxidase-like activity to food nutrition.

[0022] (2) The present invention uses a non-solvent induced phase separation method (NIPS) to prepare a metal organic framework composite membrane, directly fusing NH2-Fe-Co-MIL-88B nanoparticles, CaO2 particles and PVDF into a membrane, thus overcoming the problem of easy detachment of the traditional membrane load.

[0023] (3) Compared with the removal method using only MOF nanopowder, the present invention improves the recyclability by adding PVDF membrane, and at the same time blocks the possible escape of metal ions, thereby avoiding the generation of heavy metal pollution and possible secondary pollution.

[0024] (4) The PVDF-based composite membrane prepared by the present invention has excellent stability and repeatability as well as a lightweight volume, and can function in most environments, greatly expanding the application scenarios of the composite membrane. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the implementation methods of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the implementation methods or the description of the prior art. Obviously, the drawings in the following description are only exemplary, and for ordinary technicians in this field, other implementation drawings can be derived from the provided drawings without creative work.

[0026] Figure 1 This is the SEM image of NH2-Fe-Co-MIL-88B powder in Example 1 of the present invention.

[0027] Figure 2 are SEM images of the original PVDF membrane (a, b, c) and the finally synthesized NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane (d, e, f) in Example 1 of the present invention;

[0028] Figure 3is a representation diagram of Example 1 of the present invention;

[0029] Among them, (a) is the FT-IR of NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane, PVDF, NH2-Fe-Co-MIL-88B and CaO2; (b) is the XRD of NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane and PVDF; (c) is the XPS of NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane and PVDF.

[0030] Figure 4 is a physical property diagram of the NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane and the PVDF membrane in Example 1 and Comparative Example 3;

[0031] Among them, (a) and (c) are the surface wettability and mechanical properties of PVDF membranes; (b) and (d) are the surface wettability and mechanical properties of composite membranes.

[0032] Figure 5 This is a diagram of optimized degradation conditions for the metal organic framework composite membrane provided by the present invention;

[0033] Among them, (a) represents different CaO2 contents, (b) represents different MOF contents, (c) represents different aflatoxin concentrations, and (d) represents different pH values.

[0034] Figure 6 This is a graph showing the degradation results of Aspergillus flavus by NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane, CaO2 / PVDF composite membrane, NH2-Fe-Co-MIL-88B / PVDF composite membrane and PVDF membrane prepared in Example 1, Comparative Example 1, Comparative Example 2 and Comparative Example 3.

[0035] Figure 7 This is the LC-MS result of the degradation products of AFB1 degraded by the NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane in Example 1.

[0036] Figure 8 This is the LC-MS result of the degradation products of AFM1 degraded by the NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane in Example 1.

[0037] Fig. 9 These are the results of the cytotoxicity experiment for the safety evaluation of the NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane in Example 1.

[0038] Fig.10This is the stability test of the NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane in Example 1.

[0039] Fig.11 This is the repeatability test of the NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane in Example 1.

[0040] Fig.12 This is the actual test result of the NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane in milk in Example 1. DETAILED DESCRIPTION

[0041] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] The following first describes the concepts involved in the present application in conjunction with the accompanying drawings. It should be noted that the following description of each concept is only to make the content of the present application easier to understand, and does not limit the scope of protection of the present application; at the same time, the embodiments and features in the embodiments of the present application can be combined with each other in the absence of conflict. The present application will be described in detail with reference to the accompanying drawings and in conjunction with the embodiments.

[0043] NH2-Fe-Co-MIL-88B is a highly efficient degradation enzyme, but it requires the addition of hydrogen peroxide. Therefore, its use in the food field may destroy nutrients such as protein in food. Therefore, the present invention proposes a new idea, in which the catalyst is fixed on the membrane to form a membrane catalytic reactor, with PVDF membrane as the matrix, and CaO2 is used to provide stable and controllable H2O2 for MOF nanozyme to degrade aflatoxin, and combined with NH2-Fe-Co-MIL-88B with peroxidase-like activity, it can be applied to the food field.

[0044] Specifically, the present invention discloses a metal organic framework composite membrane, including a PVDF membrane and metal organic framework NH2-Fe-Co-MIL-88B nanoparticles and CaO2 particles loaded on the PVDF membrane;

[0045] Among them, the mass ratio of NH2-Fe-Co-MIL-88B:CaO2:PVDF is (0.1-2):(1-15):15.

[0046] Preferably, the mass ratio of NH2-Fe-Co-MIL-88B:CaO2:PVDF is 0.5:10:15.

[0047] The CaO2 particles surround the NH2-Fe-Co-MIL-88B nanoparticles.

[0048] The thickness of the composite film is 200 μm.

[0049] The metal organic framework composite film is specifically prepared by the following steps:

[0050] Step 1, ultrasonically dispersing NH2-Fe-Co-MIL-88B nanoparticles and CaO2 particles in DMF solvent to obtain a suspension;

[0051] Step 2, adding PVDF powder into the suspension to obtain a casting liquid;

[0052] Step 3: coating the casting liquid on the flat substrate to obtain a composite film on the surface of the flat substrate, and washing the composite film with ultrapure water to remove residual solvent.

[0053] The NH2-Fe-Co-MIL-88B is prepared as follows: FeCl3﹒6H2O, Co(NO3)2﹒6H2O, and H2(NH2)BDC (2-aminoterephthalic acid) are dissolved in DMF in a mass ratio of 82:90:53:3181, stirred for 30-60 minutes, reacted at 118-122°C for 24 hours, naturally cooled to room temperature, the powdered product was collected and washed with DMF, and dried at 55-65°C for 8-10 hours to obtain NH2-Fe-Co-MIL-88B.

[0054] In step 2, after adding the PVDF powder to the suspension, mechanical stirring is performed at 15-55°C for 3-5 hours to form a casting liquid, and the casting liquid is degassed at a constant temperature for 4-6 hours to eliminate bubbles.

[0055] In the above steps 1 and 2, the mass ratio of NH2-Fe-Co-MIL-88B:CaO2:PVDF is (0.1-2):(1-15):15. DMF is only used as a solvent in this process and does not participate in the reaction. Therefore, the amount used can achieve the dissolution of the reactants.

[0056] The above metal organic framework composite membrane can be used to degrade aflatoxin in food.

[0057] Preferably, the aflatoxins AFB1 and AFM1 are present, especially in milk.

[0058] The following is a detailed explanation with specific examples:

[0059] Example 1: NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane

[0060] (1) Preparation of NH2-Fe-Co-MIL-88B nanoparticles

[0061] NH2-Fe-Co-MIL-88B was synthesized by solvothermal method. 0.82g FeCl3﹒6H2O, 0.90g Co(NO3)2﹒6H2O and 0.53g H2(NH2)BDC were weighed and dissolved in 31.81g DMF, stirred for 60min, and then poured into a 100mL Teflon reactor and reacted at 120℃ for 24h. After the reaction, it was naturally cooled to room temperature, and the collected powder material was washed with DMF 5 times, collected by centrifugation, and dried at 60℃ for 8h.

[0062] (2) Preparation of NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane

[0063] The NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane was prepared by non-solvent induced phase separation (NIPS). The specific experiment is as follows: First, 0.1g NH2-Fe-Co-MIL-88B and 2g CaO2 in powder form were uniformly dispersed in 15 mL DMF solvent by ultrasonic vibration for 10 minutes to prevent serious aggregation of particles in the system. Then 3g PVDF powder was added and dissolved in the above solution, and mechanically stirred at 50°C for 4 hours to form a casting liquid. Finally, the casting liquid was degassed at a constant temperature for 4 hours to eliminate bubbles, and then the casting liquid was applied to a glass plate with a film applicator to obtain the NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane. The formed composite membrane was immersed in ultrapure water, washed with ultrapure water every 12 hours on the first day to remove residual solvent, and then stored in deionized water for use.

[0064] Comparative Example 1: CaO2 / PVDF composite membrane

[0065] The preparation method of NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane is the same as that described in Example 1, except that NH2-Fe-Co-MIL-88B is not added.

[0066] The specific experiment is as follows: First, put 2g of powdered CaO2 into 15mL DMF solvent and disperse it evenly with ultrasonic vibration for 10min to prevent serious aggregation of particles in the system. Then add 3g of PVDF powder and dissolve it in the above solution, and mechanically stir it at 50℃ for 4h to form a casting liquid. Finally, the casting liquid is degassed at a constant temperature for 4h to eliminate bubbles, and then the casting liquid is applied to a glass plate with a film applicator. The formed film is immersed in deionized water, and it is washed with deionized water every 12h on the first day to remove residual solvent, and then it is stored in deionized water for standby use.

[0067] Comparative Example 2: NH2-Fe-Co-MIL-88B / PVDF composite membrane

[0068] NH2-Fe-Co-MIL-88B / CaO as described in Example 1 2 / The preparation method of PVDF composite membrane is different in that no CaO2 is added.

[0069] The specific experiment is as follows: First, 0.1g NH2-Fe-Co-MIL-88B powder is uniformly dispersed in 17mL DMF solvent by ultrasonic vibration for 10min to prevent serious aggregation of particles in the system. Then 3g PVDF (15%) powder is added and dissolved in the above solution, and mechanically stirred at 50℃ for 4h to form a casting liquid. Finally, the casting liquid is degassed at a constant temperature for 4h to eliminate bubbles, and then the casting liquid is applied to a glass plate with a film applicator. The formed membrane is immersed in deionized water, washed with deionized water every 12h on the first day to remove residual solvent, and then stored in deionized water for standby use.

[0070] Comparative Example 3: PVDF membrane

[0071] The NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane was prepared as described in Example 1, except that NH2-Fe-Co-MIL-88B and CaO2 were not added.

[0072] The specific experiment is as follows: 3g PVDF (15%) powder was added and dissolved in 17mL DMF solution, and mechanically stirred at 50℃ for 4h to form a casting liquid. Finally, the casting liquid was degassed at a constant temperature for 4h to eliminate bubbles, and then the casting liquid was applied to a glass plate with a film applicator. The formed membrane was immersed in deionized water, washed with deionized water every 12h on the first day to remove residual solvent, and then stored in deionized water for use.

[0073] Test Example 1

[0074] SEM of NH2-Fe-Co-MIL-88B powder in Test Example 1.

[0075] SEM images of the PVDF membrane (ac) and the NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane (df) in Test Example 1.

[0076] FT-IR (a) of NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane, PVDF, NH2-Fe-Co-MIL-88B and CaO2 in test example 1, XRD (b) of NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane and PVDF, XPS (c) of NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane and PVDF.

[0077] pass Figure 1 and Figure 2 It can be found that the composite membrane has undergone a significant change in morphology compared to the original PVDF membrane. The relatively dense structure has become a reticular porous structure. At the same time, the presence of NH2-Fe-Co-MIL-88B can be clearly seen in the electron microscope image of the composite membrane, indicating that NH2-Fe-Co-MIL-88B is successfully loaded on the membrane. At the same time, in the cross-sectional electron microscope image of the membrane, in addition to NH2-Fe-Co-MIL-88B, the presence of CaO2 particles can also be seen, further proving the successful synthesis of the composite membrane.

[0078] The functional groups of different membranes were observed by FT-IR. As shown in the figure, the composite membrane has a peak at 1427 cm −1 and 1642 cm −1 The two peaks that appear in the range are due to the asymmetric and symmetric vibrations of the carboxyl group. The vibration of the carbon-carbon bond is at 1600 cm −1 -1400 cm −1 At 1159 cm −1 and 831 cm −1 At 478 cm −1 The peak at 890 cm-1 refers to the Fe-O vibration band generated when iron binds to the organic ligand of terephthalic acid. −1 The absorption peak at is attributed to Ca 2+ The functional group analysis is consistent with the existence of MIL-88B, which shows that NH2-Fe-Co-MIL-88B and CaO2 are successfully loaded on the membrane.

[0079] like Figure 3As shown, the original PVDF membrane and the composite membrane were analyzed by XRD. As can be seen from the figure, the original PVDF membrane and the composite membrane have diffraction peaks at 20.5° and 42.7°, which are typical peaks of PVDF and illustrate the semi-crystalline structure of PVDF. At the same time, there are diffraction peaks at 29.5°, 31.7°, 35.6° and 45.4° on the composite membrane, indicating the presence of a crystalline structure in the membrane, which may be caused by the right shift of the diffraction peak of NH2-Fe-Co-MIL-88B.

[0080] The elemental composition and chemical structure of the composite membrane were analyzed by XPS. In the full spectrum, it can be seen that compared with the original PVDF membrane, the composite membrane contains Fe, Co, and Ca elements, indicating the successful synthesis of the composite membrane.

[0081] Test Example 2

[0082] The physical properties such as surface wettability and mechanical properties of the NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane (b, d) in Example 1 and the PVDF membrane (a, c) in Comparative Example 3 were tested respectively.

[0083] In order to test the change of surface wettability of the composite membrane, static contact angle (CA) tests were carried out on the original PVDF membrane and NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane. Figure 4 It can be seen that the contact angle of the original PVDF membrane is 116.3°, and the contact angle of the NNH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane is 116.7°. The change in the contact angle is not large, indicating that the membrane is hydrophobic, and appropriate hydrophobicity helps to maintain the stability of the membrane in the water system. The surface roughness of the membrane determines the size of the static contact angle. The surface of the membrane is relatively smooth, so the contact angle is larger.

[0084] The mechanical properties of the original PVDF membrane and the composite membrane were tested respectively. The tensile strength, elongation at break and elastic modulus of the PVDF membrane were 2.42MPa, 99.27% ​​and 35.5MPa respectively. The elongation at break of the composite membrane with the addition of NH2-Fe-Co-MIL-88B composite membrane was 294.98%, which increased by nearly 3 times. At the same time, the tensile strength was 5.43MPa, which also increased by nearly two times. However, the elastic modulus decreased by half to 15.81MPa. It can be seen that the flexibility of the prepared composite membrane has been significantly improved compared with the PVDF membrane, but the stiffness has decreased.

[0085] Test Example 3

[0086] In order to find out the most suitable ratio and degradation conditions of synthetic membrane, the following experiments were designed:

[0087] The degradation reaction was carried out in a 50 mL centrifuge tube at room temperature. 2 NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membranes with different composition ratios, AFB1 concentration of 1 mg / L, added to 20 mL of ultrapure water, the membrane was immersed in 20 mL of AFB1 (1 mg / L) water, degraded for 60 minutes, and 0.5 mL was weighed and filtered within a certain period of time, and the AFB1 concentration was detected by liquid chromatography (HPLC). The removal rate R was calculated using the following equation:

[0088]

[0089] Where C0 and C t (mg / L) represent the concentration of AFB1 in the aqueous solution at the initial time and the concentration of AFB1 in the aqueous solution at the end of the reaction, respectively.

[0090] The experimental results are as follows Figure 5As shown in the figure, the degradation rate of NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane under different conditions was observed by controlling the variable method. The changes in CaO2 content, NH2-Fe-Co-MIL-88B content, aflatoxin concentration and pH value were tested respectively. As can be seen from Figure a, with the increase of CaO2 content in the composite membrane, the final degradation rate also gradually increased, but with the increase of CaO2 content in the composite membrane synthesis system (including DMF dosage) from 10% to 15%, the degradation rate of aflatoxin basically did not change. This shows that saturation has been reached when the CaO2 content reaches 10%, which may be the optimal content under limited membrane volume. Figure b shows the degradation rate changes affected by different NH2-Fe-Co-MIL-88B contents in the composite membrane. It can be seen that the final degradation rates are basically the same, reaching about 95%. There are certain differences in degradation rate. As the content of MOF in the composite membrane increases, the degradation rate increases accordingly. When the content of MOF in the composite membrane synthesis system reaches more than 0.5%, the difference is not very large. Since the hydrogen peroxide provided by CaO2 is limited, the change in degradation rate is weakened. Figure c shows the degradation rate change of different aflatoxin concentrations. It can be seen that with the increase of concentration, the degradation rate gradually decreases. Figure d is the degradation rate of aflatoxin by the composite membrane under different pH conditions. It is observed that the degradation rate of NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane is the highest in neutral environment, followed by alkaline environment. In acidic environment, especially strong acid environment, the degradation rate decreases rapidly, and aflatoxin is basically not degraded at pH 3. This shows that NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane has good adaptability to neutral and alkaline environments, while acidic environment will affect the degradability of NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane, which may be caused by excessive H + Affects the enzyme-like activity of MOF.

[0091] Test Example 4

[0092] In order to evaluate the degradation performance of different membranes on AFB1, the following experiments were designed:

[0093] The degradation reaction was carried out in a 50 mL centrifuge tube at room temperature. 1 cm 2The NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane, CaO2 / PVDF composite membrane, NH2-Fe-Co-MIL-88B / PVDF composite membrane and PVDF membrane, the concentration of AFB1 is 1mg / L, added to 20mL of ultrapure water, the membrane is immersed in 20mL of AFB1 (1mg / L) water, degraded for 60min, and 0.5mL is weighed and filtered within a certain period of time to detect the AFB1 concentration by liquid chromatography (HPLC). The removal rate R is calculated using the following equation:

[0094]

[0095] Where C0 and C t (mg / L) represent the concentration of AFB1 in the aqueous solution at the initial time and the concentration of AFB1 in the aqueous solution at the end of the reaction, respectively.

[0096] The experimental results are as follows Figure 6 As shown in the figure, the membranes synthesized by different materials were used to observe the effect of the materials on the degradation of aflatoxin. The materials of the synthetic membranes were single PVDF, PVDF+MOF, PVDF+CaO2 and PVDF+CaO2+MOF. The degradation rate of aflatoxin by the membranes synthesized by different materials showed that the PVDF membrane and PVDF+MOF composite membrane had basically no effect on the degradation of aflatoxin, and the degradation rate of the PVDF+CaO2 composite membrane was only about 30%, which may be because the generated hydrogen peroxide had a certain degradation effect on aflatoxin. When the PVDF+CaO2+MOF composite membrane was added, the degradation rate reached 95%, indicating that the combination of CaO2 and MOF can effectively play a degradation role.

[0097] Test Example 5

[0098] In order to further evaluate the degradation products of NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane, the following experiments were designed:

[0099] After the reaction in the NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane reaction system was completed, 1 mL of the reaction solution was filtered and packaged for use in liquid chromatography-mass spectrometry (LC-MS).

[0100] LC-MS test results are as follows Figure 7 and Figure 8 As shown, it can be seen that the final degradation products of AFB1 and AFM1 are small molecules. Through the catalysis of the membrane, AFB1 undergoes changes in the furan ring and methoxy group to eventually produce small molecules.

[0101] Test Example 6

[0102] To evaluate the safety of NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane, cytotoxicity was conducted and the following experiments were designed:

[0103] The cell toxicology experiment was carried out by 3-(4,5-dimethylthiazol-2-yl)-2,5-diphenyltetrazolium bromide (MTT) colorimetry, and HepG2 cells were selected as the experimental subjects to determine the cell viability. HepG2 cells were transplanted into 48-well plates and cultured in a carbon dioxide incubator for 24 h. Then, membrane samples of different areas (0.1, 0.3, 0.5, 1, 1.5, 2 cm 2 ) was added to a 48-well plate (200uL) and continued to be cultured for 24h. After the culture was completed, the supernatant was extracted, 90uL of fresh culture medium and 10uL of MTT solution (5mg / mL) were added, and incubated for 4h. After the end, the supernatant was taken and 100uL of DMSO was added to each well. Then the plate was placed on a low-speed shaker for 10min to ensure that the crystals were completely dissolved. Finally, the absorbance of each well was measured at 490nm using a microplate reader.

[0104] like Fig. 9 As shown in the figure, under different composite membrane areas, the cell survival rate always remains above 70%. This shows that the composite membrane has low toxicity and will not cause harm to the human body. In the degradation products, it can be found that the lactone ring of the product is basically destroyed, and non-toxic small molecule products are generated. This further proves the safety of NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane for use in food.

[0105] Test Example 7

[0106] The stability and repeatability of NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane were tested. Fig.10 and 11 As shown in the figure, in the 15-day stability test, the composite membrane showed good stability, and the degradation rate remained above 75% after 15 days. The decrease in degradation rate may be caused by the decrease in the CaO2 content in the composite membrane as the reaction proceeds, resulting in a decrease in the production of H2O2. In the recyclable test, it can be seen from the figure that the degradation rate is still above 80% after 5 cycles, indicating that the recyclability of the membrane is good. The reason for the decrease in degradation rate may be that the substrate adsorbed on the membrane is not cleaned cleanly, and there is a certain loss in the calcium peroxide content. Overall, the composite membrane has excellent stability and can be stably used in actual scenarios.

[0107] Test Example 8

[0108] In order to verify the actual application performance of NH2-Fe-Co-MIL-88B / CaO2 / PVDF composite membrane in milk, the following experiments were designed:

[0109] Weigh 20g of aflatoxin M1-free milk, place it in a 50mL centrifuge tube, centrifuge at 8000r / min at -4℃ for 15min, remove the upper fat layer, and add the toxin. 2 Composite membrane, degradation for 60 min, 4 mL of milk was mixed with 0.4 g of sodium chloride and 12 mL of ethyl acetate on a shaker at 300 r / min for 10 min. The mixture was centrifuged at 8000 r / min for 10 min to separate the organic layer. 6 mL of the supernatant was evaporated under nitrogen flow (40 °C) and then redissolved in 1 mL of a mixed solution of 15% acetonitrile / H2O (v / v) and 0.1% formic acid. The concentration after degradation was detected after filtering with 0.22 μm.

[0110] like Fig.12 As shown in the figure, the degradation rate of aflatoxin M1 in milk with the composite membrane was 85%, which is much higher than the existing method of removing aflatoxin in milk while ensuring safety. This further proves that the composite membrane has reliable applicability under actual conditions.

[0111] It should be noted that the terms used in this application are only for describing specific embodiments, rather than limiting the scope of this application. As shown in the specification of this application, unless the context clearly indicates an exception, the words "one", "a", "a kind of" and / or "the" do not specifically refer to the singular, but may also include the plural. The terms "include", "comprise" or any other variant thereof are intended to cover non-exclusive inclusion, so that the process, method or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method or device. In the absence of further restrictions, the elements defined by the statement "include one..." do not exclude the presence of other identical elements in the process, method or device including the elements.

[0112] It should also be noted that the terms "center", "up", "down", "left", "right", "vertical", "horizontal", "inside", "outside", etc., indicating the orientation or position relationship, are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application. Unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", etc. should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be an indirect connection through an intermediate medium, or it can be a connection between the two elements. For those of ordinary skill in the art, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0113] The embodiments and / or implementation methods described above are only used to illustrate the preferred embodiments and / or implementation methods for realizing the technology of the present invention, and are not intended to limit the implementation methods of the technology of the present invention in any form. Any technical personnel in this field may make slight changes or modifications to other equivalent embodiments without departing from the scope of the technical means disclosed in the content of the present invention, but they should still be regarded as technologies or embodiments that are essentially the same as the present invention.

[0114] This article uses specific examples to illustrate the principles and implementation methods of this application. The description of the above embodiments is only used to help understand the method and its core ideas of this application. The above is only the preferred implementation method of this application. It should be pointed out that due to the limitations of textual expression and the objective existence of infinite specific structures, ordinary technicians in this technical field can make several improvements, modifications or changes without departing from the principles of this application, and can also combine the above technical features in an appropriate manner; these improvements, modifications, changes or combinations, or the direct application of the concept and technical solution of the invention to other occasions without improvement, should be regarded as the scope of protection of this application.

Claims

1. A metal organic framework composite membrane, characterized in that: It includes a PVDF membrane and metal organic framework NH2-Fe-Co-MIL-88B nanoparticles and CaO2 particles loaded on the PVDF membrane; Among them, the mass ratio of NH2-Fe-Co-MIL-88B:CaO2:PVDF is (0.1-2): (1-15): 15; The metal organic framework composite film is prepared by the following steps: Step 1, ultrasonically dispersing NH2-Fe-Co-MIL-88B nanoparticles and CaO2 particles in DMF solvent to obtain a suspension; Step 2, adding PVDF powder into the suspension to obtain a casting liquid; Step 3, coating the casting liquid on the flat substrate to obtain a composite film on the surface of the flat substrate, and washing the composite film with ultrapure water to remove residual solvent; Wherein, the metal organic framework NH2-Fe-Co-MIL-88B nanoparticles are prepared by the following method: FeCl3﹒6H2O, Co(NO3)2﹒6H2O and H2(NH2)BDC were dissolved in DMF in a mass ratio of 82:90:53:3181, stirred for 30-60 minutes, reacted at 118-122°C for 22-26 hours, cooled naturally to room temperature, the powdered product was collected and washed with DMF, and dried at 55-65°C for 8-10 hours to obtain NH2-Fe-Co-MIL-88B.

2. The metal organic framework composite membrane according to claim 1, characterized in that: The CaO2 particles surround the NH2-Fe-Co-MIL-88B nanoparticles.

3. The metal organic framework composite membrane according to claim 1, characterized in that: The mass ratio of NH2-Fe-Co-MIL-88B:CaO2:PVDF is 0.5:10:

15.

4. The metal organic framework composite membrane according to claim 1, characterized in that: The thickness of the composite film is 200 μm.

5. The metal organic framework composite membrane according to claim 1, characterized in that: In step 2, after adding the PVDF powder to the suspension, mechanical stirring is performed at 45 to 55° C. for 3 to 5 hours to form a casting liquid, and the casting liquid is degassed at a constant temperature for 4 to 6 hours to eliminate bubbles.

6. A use of the metal organic framework composite membrane according to any one of claims 1 to 5, characterized in that: Used to degrade aflatoxins in food.

7. The use according to claim 6, characterized in that: The aflatoxins are AFB1 and AFM1.