A low-temperature electrolyte for aqueous zinc ion batteries and its application

By adding 2-trifluoromethyl-2-propanol to the aqueous zinc-ion battery electrolyte and optimizing the ratio of solvents and additives, the problems of coagulation and poor wettability of zinc-ion batteries in low-temperature environments were solved, and higher performance was achieved. Low temperature electrochemical performance and longer cycle life reduce cost and self-discharge rate.

CN118099570BActive Publication Date: 2024-10-15HENAN NORMAL UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410479214.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-22
Publication Date
2024-10-15
Estimated Expiration
2044-04-22

AI Technical Summary

Technical Problem

Aqueous zinc-ion batteries are prone to solidification in low-temperature environments, limiting ion migration and poor electrode wettability, resulting in deterioration of electrochemical performance. The existing technology has the disadvantages of evaporating and flammable organic electrolytes and high-cost, high-concentration electrolytes. .

Method used

Use a small amount of 2-trifluoromethyl-2-propanol as an additive to optimize the ratio of solvents to additives, lower the freezing point of the electrolyte, and adjust the solvation structure of Zn2+ to make it liquid at low temperatures and improve ionic conductivity. rate and deposition uniformity to form an inorganic/organic hybrid electrolyte.

Benefits of technology

At -70~-20℃, the low-temperature electrochemical performance of aqueous zinc-ion batteries is significantly improved, the cycle life is extended, the safety and energy conversion efficiency are improved, and the self-discharge speed and cost are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118099570B_ABST
    Figure CN118099570B_ABST
Patent Text Reader

Abstract

The invention discloses a low-temperature electrolyte for an aqueous zinc ion battery and an application thereof, wherein the low-temperature electrolyte for an aqueous zinc ion battery is composed of a solvent, an additive and a soluble zinc salt, wherein the concentration of the soluble zinc salt in the electrolyte is 0.5 to 3 mol / L, the volume fraction of the additive in the mixed solvent is 1% to 25%, the solvent is pure water, the mixed solvent is a mixed solution of the solvent and the additive, and the additive is 2-trifluoromethyl-2-propanol. The present invention reduces the freezing point of the electrolyte on the one hand by adding an appropriate amount of 2-trifluoromethyl-2-propanol to the electrolyte, and on the other hand, water molecules are confined in a liquid eutectic network, thereby weakening the activity of free water and extending the electrochemical stability window; an organic / inorganic hybrid interface containing F is generated on the surface of a zinc negative electrode to avoid the occurrence of side reactions caused by direct contact between water and Zn.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of aqueous zinc ion battery electrolytes, and in particular relates to an aqueous zinc ion battery low-temperature electrolyte and application thereof. Background Art

[0002] Electrochemical energy storage technology is of great significance for the storage and conversion of renewable natural resources. As an emerging energy device, aqueous zinc ion batteries (AZIBs) are considered to be an ideal candidate for large-scale energy storage technology due to their many advantages such as high abundance, low cost, high safety and high ionic conductivity.

[0003] Aqueous zinc-ion battery electrolytes have a narrow liquid temperature range because they use water as the solvent of the electrolyte. When the temperature drops below 0°C, ordinary aqueous electrolytes tend to solidify due to the high freezing point of water, which limits the flow of ions and the wettability of the electrolyte to the electrodes, resulting in a deterioration of the electrode-electrolyte interface, which in turn leads to a serious deterioration in the electrochemical performance of aqueous zinc-ion batteries. Currently, several strategies have been proposed to inhibit the coagulation of electrolytes: (1) Adding a certain amount of organic additives to the electrolyte. On the one hand, the addition of organic matter breaks the original hydrogen bond network between water molecules and forms new hydrogen bonds with water molecules to form an electrolyte with a low freezing point. On the other hand, by reacting with Zn 2+ Coordination to adjust Zn 2+ The solvation structure of Zn can inhibit the formation of dendrites and side reactions. However, organic electrolytes generally have many disadvantages such as easy evaporation, flammability and environmental unfriendliness. In addition, during the coordination process, Zn 2+ The radius of the solvated structure increases, especially below 0°C, which significantly reduces the ionic conductivity of the battery; (2) Organic matter is grafted onto polymer chains to make hydrogels, but the preparation process is relatively cumbersome and complicated; (3) High-concentration electrolytes are prepared. The increase in concentration can reduce the freezing point and improve the ionic conductivity of the battery at low temperatures. It has higher ionic conductivity than organic molecules, but this solution is expensive and the wettability of the electrolyte is extremely poor. Salting out will occur at low temperatures, resulting in the precipitation of electrolyte salts and the deposition of zinc salts on the positive and negative electrodes, greatly reducing the cycle life of the battery. In addition, high-concentration electrolytes can cause corrosion and side reactions, thereby shortening the battery life. Therefore, it is very necessary to develop low-temperature aqueous zinc-ion battery electrolytes with excellent electrochemical properties at extreme temperatures.

[0004] In extremely cold regions, most energy storage devices cannot operate normally. Therefore, exploring a new aqueous zinc-ion battery electrolyte with low concentration and low freezing point and using the electrolyte to assemble a low-temperature aqueous zinc-ion battery is the focus of expanding its application scenarios. Summary of the invention

[0005] The present invention provides an aqueous zinc ion battery low-temperature electrolyte to solve the problems of coagulation of aqueous zinc ion battery electrolyte under low temperature environment, restricted ion migration, extremely poor wettability of electrolyte to electrode, serious deterioration of discharge performance, etc., wherein a small amount of organic additives are added to the electrolyte, and the ratio of solvent to additives is optimized, so that not only the coagulation point of the electrolyte is reduced, but also the Zn 2+ The solvation shell structure of Zn 2+ It has a faster dissolution behavior and is easier to deposit toward a specific crystal plane. The aqueous zinc ion battery assembled using this electrolyte has excellent low-temperature electrochemical performance at a temperature of -70~-20℃.

[0006] The present invention adopts the following technical scheme to solve the above technical problems. It is a low-temperature electrolyte for aqueous zinc ion batteries, characterized in that the electrolyte consists of a solvent, an additive and a soluble zinc salt, the concentration of the soluble zinc salt in the electrolyte is 0.5-3 mol / L, the volume fraction of the additive in the mixed solvent is 1%-25%, the solvent is pure water, the mixed solvent is a mixed solution of the solvent and the additive, and the additive is 2-trifluoromethyl-2-propanol.

[0007] It is further defined that the soluble zinc salt is one or more of zinc perchlorate, zinc tetrafluoroborate, zinc acetate or zinc nitrate, preferably zinc perchlorate.

[0008] It is further defined that the concentration of the soluble zinc salt in the electrolyte is 2 mol / L.

[0009] It is further defined that the additive accounts for 10% of the volume fraction of the mixed solvent.

[0010] The invention discloses an application of the electrolyte in preparing a low-temperature aqueous zinc ion battery.

[0011] It is further defined that the aqueous zinc ion battery comprises a positive electrode, a negative electrode, a separator and an electrolyte, wherein the positive electrode is Zr 0.02 Nb 0.09 V2O5·1.63H2O (abbreviated as ZNVO) or copper foil, the diaphragm is a glass fiber microporous filter membrane (Whatman Company, UK) GF / D, the negative electrode is a metal zinc sheet, and the operating temperature of this aqueous zinc ion battery is -70~-20℃.

[0012] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0013] 1. In the present invention, the additive 2-trifluoromethyl-2-propanol is fully mixed with the solvent pure water, wherein the addition of 2-trifluoromethyl-2-propanol breaks the original hydrogen bond network between water and water molecules, and 2-trifluoromethyl-2-propanol forms new hydrogen bonds F···H and O···H with water molecules, thereby lowering the freezing point of the electrolyte, making the electrolyte liquid in a low temperature environment, reducing the viscosity of the electrolyte, improving the interface impedance, and inhibiting the occurrence of interface side reactions, thereby effectively improving the low temperature performance of the aqueous zinc ion battery.

[0014] 2. In the present invention, water molecules react with Zn 2+ The double interaction of coordination and hydrogen bond with 2-trifluoromethyl-2-propanol confines it in the liquid eutectic network, thereby weakening the activity of free water, prolonging the electrochemical stability window, and inhibiting the occurrence of hydrogen evolution and oxygen evolution reactions. To a certain extent, it can prevent the occurrence of problems such as flatulence, leakage and explosion in the charge and discharge process of aqueous zinc-ion batteries, thereby improving the safety of aqueous zinc-ion batteries.

[0015] 3. The addition of 2-trifluoromethyl-2-propanol as an additive in the present invention replaces Zn 2+ The position of water molecules in the solvation structure forms a new Zn 2+ The solvated structure has a strong affinity with the specific crystal plane of the Zn metal surface, which reduces the nucleation barrier of Zn metal, promotes the directional deposition of Zn metal, and regulates the 2+ The diffusion behavior of Zn 2+ The surface of the Zn negative electrode is deposited more evenly. 2+ The solvated structure exhibits good desolvation kinetics, making Zn 2+ It has a faster desolvation behavior, regulates the thermodynamic and kinetic properties of the zinc negative electrode, makes Zn deposition uniform, and is less likely to form dendrites.

[0016] 4. The present invention effectively improves the ionic conductivity of the electrolyte at low temperature by adding a suitable amount of the additive 2-trifluoromethyl-2-propanol. The additive contains F groups, which have a good adsorption effect on Zn metal. During the battery cycle, an organic / inorganic hybrid solid electrolyte layer (SEI) containing F can be formed, which isolates the direct contact between H2O and the Zn metal negative electrode, avoids the occurrence of hydrogen and oxygen evolution reactions and corrosion of the Zn metal negative electrode, and regulates the Zn in the aqueous zinc ion battery. 2+ The deposition process of zinc ions can be inhibited, and the formation of dendrites and "dead zinc" can be inhibited, thereby achieving the purpose of improving the low-temperature resistance of aqueous zinc-ion batteries.

[0017] 5. The low-temperature electrolyte provided by the present invention has a simple preparation process, little environmental pollution, is easy to operate, and can effectively solve the problem of poor low-temperature performance of aqueous zinc ion batteries, and is easy to mass produce. 2+ It mainly plays the role of ion transport. The low-temperature resistant 2-trifluoromethyl-2-propanol is used as an additive to form an inorganic / organic mixed low-temperature electrolyte, which not only maintains the high ionic conductivity and high safety of the original aqueous electrolyte, but also improves the reversible reaction of zinc deposition / stripping at the negative electrode, thereby maximizing the low-temperature service life of the aqueous zinc-ion battery.

[0018] 6. 2-Trifluoromethyl-2-propanol in the present invention is an organic substance. Compared with other organic solvents, it has the advantages of good chemical stability, thermal stability and good solubility, and has lower viscosity and surface tension, which makes the ion transmission inside the aqueous zinc ion battery smoother, reduces the self-discharge rate of the battery, and improves the energy conversion efficiency of the battery. (1) 2-Trifluoromethyl-2-propanol has good chemical stability, which can effectively improve the safety performance of the battery and reduce the cost of the battery. Experimental data show that introducing 2-trifluoromethyl-2-propanol into the electrolyte of the aqueous zinc ion battery can significantly improve its low-temperature electrochemical performance; (2) 2-Trifluoromethyl-2-propanol has low volatility, which can effectively inhibit the volatilization of the electrolyte during the operation of the aqueous zinc ion battery and reduce the attenuation of the battery capacity. 2-Trifluoromethyl-2-propanol can be used as an additive in the electrolyte of aqueous zinc ion batteries. Adding an appropriate amount of this organic additive can effectively improve the low-temperature cycle performance and low-temperature cycle service life of the battery; (3) 2-Trifluoromethyl-2-propanol can stabilize the solubility of zinc salts and prevent zinc salts from being deposited on the positive and negative electrodes of the battery, thereby extending the service life of the aqueous zinc ion battery.

[0019] 7. Under low temperature conditions of -60°C, both symmetrical cells and full cells exhibit relatively excellent battery electrochemical performance. The experimental results show that the zinc-zinc symmetrical battery assembled with the electrolyte containing 2-trifluoromethyl-2-propanol has a high electrochemical performance at 0.5 mA cm even at -60°C. -2 0.5mAh cm -2 The aqueous zinc ion full battery (Zn / / ZNVO) assembled with 2-trifluoromethyl-2-propanol electrolyte can maintain a cycle stability of 4000 h at 1A g even at -60 °C. -1 At a current density of 1.5 MW, after 3,000 cycles, the capacity retention rate was 85%. This excellent performance provides new hope for the widespread application of low-temperature aqueous zinc-ion batteries under low-temperature and harsh conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1The electrolyte prepared in Example 1 was assembled into a zinc-zinc symmetrical battery at a temperature of -60°C with a current density of 0.5 mA cm -2 0.5mAh cm -2 Scanning electron microscope image of the zinc metal negative electrode after 30 cycles.

[0021] Figure 2 The electrolyte prepared in Comparative Example 1 was assembled into a zinc-zinc symmetrical battery at a temperature of -60°C with a current density of 0.5 mA cm -2 0.5mAh cm -2 Scanning electron microscope image of the zinc metal negative electrode after 30 cycles.

[0022] Figure 3 The electrolytes prepared in Example 1 and Comparative Examples 1 to 3 were assembled into zinc-zinc symmetrical batteries at a temperature of -60°C with a current density of 0.5 mA cm -2 0.5mAh cm -2 Cycle performance diagram when .

[0023] Figure 4 The electrolytes prepared in Example 1 and Comparative Examples 1 to 3 were assembled into zinc-zinc symmetrical batteries at a temperature of -40°C with a current density of 0.5 mA cm -2 0.5mAh cm -2 Cycle performance diagram when .

[0024] Figure 5 The electrolyte prepared in Example 1 and Comparative Examples 1 to 3 was assembled with ZNVO into an aqueous zinc ion full battery at a temperature of -60°C with a current density of 1A g -1 Cycle performance diagram when .

[0025] Figure 6 The rate performance diagram of the aqueous zinc ion full battery assembled with the electrolyte prepared in Example 1 and Comparative Examples 1 to 3 and ZNVO at a temperature of -60°C.

[0026] Figure 7 The electrolyte prepared in Example 1 and Comparative Example 1 and the copper foil were assembled into an aqueous zinc ion full battery at a temperature of -60°C with a current of 1 mA cm -2 0.5mAh cm -2 Coulomb efficiency diagram when .

[0027] Figure 8 The electrolyte prepared in Example 1 and Comparative Example 1 and the copper foil were assembled into an aqueous zinc ion full battery at a temperature of -60°C and a scan rate of 0.1 mV s -1 CV graph of. DETAILED DESCRIPTION

[0028] The above contents of the present invention are further described in detail below through examples, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples, and all technologies implemented based on the above contents of the present invention belong to the scope of the present invention. Example 1

[0029] A low-temperature electrolyte for zinc ion batteries is provided. Pure water is used as a solvent, 2-trifluoromethyl-2-propanol is used as an additive, the volume fraction of the additive in the mixed solvent is 10%, a certain mass of zinc perchlorate is weighed according to a concentration of 2 mol / L, the zinc perchlorate is dissolved in a mixed solvent of water and 2-trifluoromethyl-2-propanol, and the electrolyte is obtained by stirring and dissolving the mixture into a transparent solution at room temperature. Example 2

[0030] A low-temperature electrolyte for zinc ion batteries is provided. Pure water is used as a solvent, 2-trifluoromethyl-2-propanol is used as an additive, the volume fraction of the additive in the mixed solvent is 25%, a certain mass of zinc perchlorate is weighed according to a concentration of 0.5 mol / L, the zinc perchlorate is dissolved in a mixed solvent of water and 2-trifluoromethyl-2-propanol, and the electrolyte is obtained by stirring and dissolving the mixture into a transparent solution at room temperature. Example 3

[0031] A low-temperature electrolyte for zinc ion batteries is provided. Pure water is used as a solvent, 2-trifluoromethyl-2-propanol is used as an additive, the volume fraction of the additive in the mixed solvent is 1%, a certain mass of zinc perchlorate is weighed according to a concentration of 3 mol / L, the zinc perchlorate is dissolved in a mixed solvent of water and 2-trifluoromethyl-2-propanol, and the electrolyte is obtained by stirring and dissolving the mixture into a transparent solution at room temperature. Example 4

[0032] A low-temperature electrolyte for zinc ion batteries is provided. Pure water is used as a solvent, 2-trifluoromethyl-2-propanol is used as an additive, the volume fraction of the additive in the mixed solvent is 10%, a certain mass of zinc tetrafluoroborate is weighed according to a concentration of 2 mol / L, the zinc tetrafluoroborate is dissolved in a mixed solvent of water and 2-trifluoromethyl-2-propanol, and the electrolyte is obtained by stirring and dissolving the mixture into a transparent solution at room temperature. Example 5

[0033] A low-temperature electrolyte for zinc ion batteries is provided. Pure water is used as a solvent, 2-trifluoromethyl-2-propanol is used as an additive, the volume fraction of the additive in the mixed solvent is 10%, a certain mass of zinc nitrate is weighed according to a concentration of 2 mol / L, the zinc nitrate is dissolved in a mixed solvent of water and 2-trifluoromethyl-2-propanol, and the electrolyte is obtained by stirring and dissolving into a transparent solution at room temperature.

[0034] Comparative Example 1

[0035] A low-temperature electrolyte for zinc ion batteries is provided. Pure water is used as a solvent without any additives. A certain mass of zinc perchlorate is weighed according to a concentration of 2 mol / L, dissolved in the solvent pure water, and stirred at room temperature to dissolve into a transparent solution to obtain the electrolyte.

[0036] Comparative Example 2

[0037] A low-temperature electrolyte for zinc ion batteries is provided. Pure water is used as a solvent, isopropyl ether is used as an additive, the volume fraction of the additive in the mixed solvent is 10%, a certain mass of zinc perchlorate is weighed according to a concentration of 2 mol / L, the zinc perchlorate is dissolved in a mixed solvent of water and isopropyl ether, and the electrolyte is obtained by stirring and dissolving into a transparent solution at room temperature.

[0038] Comparative Example 3

[0039] A low-temperature electrolyte for zinc ion batteries is provided. Pure water is used as a solvent, ethyl trifluoroacetate is used as an additive, the volume fraction of the additive in the mixed solvent is 10%, a certain mass of zinc perchlorate is weighed according to a concentration of 2 mol / L, the zinc perchlorate is dissolved in a mixed solvent of water and ethyl trifluoroacetate, and the electrolyte is obtained by stirring and dissolving the mixture into a transparent solution at room temperature.

[0040] Assembly process of aqueous zinc ion zinc-zinc symmetric battery (Zn / / Zn) / full battery (Zn / / Cu): The electrolytes prepared in Example 1 and Comparative Examples 1 to 3 were assembled into 2032-type button aqueous zinc ion zinc-zinc symmetric battery / full battery at room temperature. The assembly order was positive electrode shell, zinc sheet / copper foil, diaphragm, electrolyte, zinc sheet, gasket, spring and negative electrode shell. The battery was first packaged with a battery packaging machine at room temperature and then allowed to stand for 8 hours. The battery was then transferred to a low-temperature refrigerator at -60°C or -40°C and allowed to stand for 8 hours. The battery was then charged and discharged on a Xinwei charge and discharge tester. The current density of the symmetrical battery was 0.5 mA cm -2 0.5mAh cm -2 .Depend on Figure 3 It can be seen that the symmetrical battery assembled with the mixed electrolyte containing 2-trifluoromethyl-2-propanol has a significantly improved stable cycle time, and can stably cycle for more than 4000 hours at a temperature of -60°C, far exceeding the symmetrical batteries assembled in Comparative Examples 1 to 3. Figure 4 It can be seen that the symmetrical battery assembled with the mixed electrolyte containing 2-trifluoromethyl-2-propanol has a significantly improved stable cycle time, and can stably cycle for more than 1800 hours at a temperature of -40°C, and its performance is better than that of the symmetrical batteries assembled in Comparative Examples 1 to 3. Figure 1 and Figure 2By comparison, it can be seen that the mixed electrolyte containing 2-trifluoromethyl-2-propanol improves the zinc deposition morphology and inhibits hydrogen evolution corrosion, greatly improving the stability of the zinc negative electrode, thereby greatly improving the cycle stability of the aqueous zinc ion battery. The current density of the full battery (Zn / / Cu) is 1mA cm -2 0.5mAh cm -2 ,Depend on Figure 7 It can be seen that the full battery assembled in Example 1 can have a cycle life of up to 2000 cycles and the coulombic efficiency is stable at 100%, which is far higher than the full battery assembled in Comparative Example 1. Figure 8 It can be seen that compared with the Zn / / Cu full battery assembled in Comparative Example 1, Example 1 has a higher nucleation overpotential, and the nucleation overpotential is increased by 17 mV, which is conducive to the formation of refined small-sized nuclei, indicating that zinc dendrites are less likely to form.

[0041] The synthesis process of ZNVO positive electrode: First, weigh 0.364g of V2O5, pour it into a beaker filled with 40mL of deionized water to dissolve, and perform ultrasound for 20 minutes to make it evenly dispersed. Then, add 0.012g of zirconium acetate and 0.051g of niobium oxalate to the solution, first perform ultrasound for 20 minutes, then add 5mL of hydrogen peroxide, stir for 20 minutes, and then transfer the obtained solution to a reactor for hydrothermal reaction at 200℃ for 24h. Then centrifuge the obtained sample, wash it three times with deionized water, then wash it three times with ethanol, and finally dry it in vacuum at 70℃ for 24h to obtain the target sample Zr 0.02 Nb 0.09 V2O5·1.63H2O, abbreviated as ZNVO.

[0042] Assembly process of aqueous zinc ion full battery (Zn / / ZNVO): The prepared ZNVO, conductive carbon (MWCNTs) and binder (PVDF) are mixed in a mass ratio of 60:30:10 to form a fine slurry, which is then coated on a stainless steel mesh to obtain a positive electrode. A zinc sheet is used as the negative electrode, and a glass fiber microporous filter membrane GF / D is used as a diaphragm. The electrolyte prepared in Example 1 and Comparative Examples 1 to 3 is used to assemble a 2032-type button aqueous zinc ion full battery at room temperature. The assembly order is negative electrode shell, zinc sheet, diaphragm, electrolyte, positive electrode, gasket, shrapnel and positive electrode shell. It is first packaged with a battery packaging machine at room temperature and allowed to stand for 8 hours. It is then transferred to a low-temperature refrigerator at -60°C and allowed to stand for 8 hours. The battery is then subjected to charge and discharge tests on a Newway charge and discharge tester. Figure 5 It can be seen that the battery assembled in Example 1 is at a temperature of -60°C and at 1A g -1 At a current density of 0.05A g, after 3000 cycles, the capacity retention rate is as high as 85%, showing excellent low-temperature cycle stability. -1 , 0.1A g-1 , 0.2A g -1 , 0.5A g -1 , 0.8A g -1 , 1A g -1 , 2A g -1 , 3A g -1 , 2A g -1 , 1A g -1 , 0.8A g -1 , 0.5A g -1 , 0.2A g -1 , 0.1A g -1 and 0.05A g -1 The rate performance of the assembled battery was tested at a charge and discharge rate of Figure 6 It can be seen that the battery assembled in Example 1 exhibits excellent low-temperature electrochemical performance when cycled ten times at the above current density at a temperature of -60°C.

[0043] The above embodiments describe the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for illustrating the principles of the present invention. Without departing from the scope of the principles of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of protection of the present invention.

Claims

1. A low-temperature electrolyte for an aqueous zinc ion battery, characterized in that: The electrolyte consists of a solvent, an additive and a soluble zinc salt. The concentration of the soluble zinc salt in the electrolyte is 0.5-3 mol / L, the volume fraction of the additive in the mixed solvent is 1%-25%, the solvent is pure water, the mixed solvent is a mixed liquid of the solvent and the additive, the additive is 2-trifluoromethyl-2-propanol, and the soluble zinc salt is one or more of zinc perchlorate, zinc tetrafluoroborate, zinc acetate or zinc nitrate.

2. The aqueous zinc ion battery low temperature electrolyte according to claim 1, characterized in that: The concentration of the soluble zinc salt in the electrolyte is 2 mol / L.

3. The aqueous zinc ion battery low temperature electrolyte according to claim 1, characterized in that: The volume fraction of the additive in the mixed solvent is 10%.

4. Use of the low-temperature electrolyte for aqueous zinc ion batteries according to any one of claims 1 to 3 in the preparation of low-temperature aqueous zinc ion batteries.

5. The use according to claim 4, characterized in that: The aqueous zinc ion battery comprises a positive electrode, a negative electrode, a separator and an electrolyte, wherein the positive electrode is Zr 0.02 Nb 0.09 V2O5·1.63H2O or copper foil, the diaphragm is a glass fiber microporous filter membrane GF / D, the negative electrode is a metal zinc sheet, and the operating temperature of the aqueous zinc ion battery is -70~-20℃.

Citation Information

Patent Citations

  • Aqueous zinc ion battery additive, electrolyte prepared from aqueous zinc ion battery additive and application of aqueous zinc ion battery additive

    CN114447446A

  • Water-based zinc ion battery electrolyte containing small-molecule dihydric alcohol additive and application of water-based zinc ion battery electrolyte

    CN116365067A

  • Zinc alkaline battery

    JP1990270263A

  • Aqueous electrolyte and battery

    WO2022233342A1