A method for preparing a flame retardant electrolyte for sodium ion battery

Conductive additives are prepared by the reaction of modified diethyl phosphate and acrylic acid, and combined with sodium sulfate, sodium fluoroborate and polyethylene glycol to form an electrolyte with high conductivity and flame retardant properties, solving the organics in sodium ion batteries Solution combustion and flame retardants reduce conductivity issues, achieving safe and efficient battery operation.

CN117477026BActive Publication Date: 2024-11-26ANHUI NANDU HUATUO NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311742015.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-18
Publication Date
2024-11-26
Estimated Expiration
2043-12-18

AI Technical Summary

Technical Problem

The use of organic solutions as solvents for existing sodium ion batteries poses a risk of combustion and explosion, and adding flame retardants to the electrolyte will reduce conductivity and increase costs.

Method used

The conductive additives are prepared by reacting modified diethyl phosphate, acrylic acid, toluene and initiator, and combined with sodium sulfate, sodium fluoroborate and polyethylene glycol to form a flame retardant electrolyte, through the processing of diethyl chlorophosphate and Modification of hydroxyethyl ester improves the conductivity and stability of the electrolyte.

Benefits of technology

It achieves high conductivity and good flame retardant properties of sodium ion battery electrolyte, reduces combustion risks, is suitable for a wide temperature range, and avoids combustion of the battery during operation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004613373480000021
    Figure BDA0004613373480000021
  • Figure BDA0004613373480000031
    Figure BDA0004613373480000031
  • Figure BDA0004613373480000032
    Figure BDA0004613373480000032
Patent Text Reader

Abstract

The invention discloses a method for preparing a flame-retardant electrolyte for sodium ion batteries, and belongs to the technical field of electrolyte processing. The invention is used to solve the technical problem that the combustion performance and conductivity of the electrolyte of the sodium ion battery in the prior art need to be further improved. A method for preparing a flame-retardant electrolyte for a sodium ion battery comprises the following steps: adding modified diethyl phosphate, acrylic acid, toluene and an initiator to a three-necked flask and stirring, raising the temperature of the three-necked flask to 75-85°C, keeping the temperature for reaction for 20-23h, and post-processing to obtain a conductive additive; adding sodium sulfate, sodium fluoroborate and deionized water to a nitrogen-protected three-necked flask and stirring evenly to obtain a mixed solution one. The present invention cooperates with the synthesized conductive additive, sodium sulfate, polyethylene glycol and solvent water, so that the flame-retardant electrolyte is not only non-flammable, but also has a wide temperature range and ultra-high conductivity, and is suitable for use in sodium ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electrolyte processing, and in particular to a method for preparing a flame retardant electrolyte for a sodium ion battery. Background Art

[0002] As the global demand for renewable energy continues to increase and traditional oil resources are decreasing, sodium-ion batteries, as a new type of high-energy-density energy storage device, have attracted much attention from researchers. Sodium-ion batteries have the advantages of high energy density, low cost, and abundant resources, and are widely considered to be a potential energy storage solution to replace lithium-ion batteries.

[0003] The electrolyte of sodium ion batteries in the prior art usually uses organic solutions such as acetone nitrile, diethylene glycol, etc. as solvents, but these organic solutions not only have a low ignition point, but also easily cause battery combustion or even explosion in abnormal conditions such as overcharging, overdischarging, and short circuit, which poses a great safety risk. In order to improve the combustion performance of sodium ion batteries, the flame retardant effect of the electrolyte is currently mainly achieved by adding phosphorus flame retardants, fluorine flame retardants, silicon flame retardants, etc. to the electrolyte. However, while these flame retardants improve the flame retardancy of the electrolyte, they will have a negative impact on other properties of the electrolyte, such as reduced conductivity and decreased ion mobility. In addition, the addition of these flame retardants will also increase the cost of the electrolyte.

[0004] In view of the technical defects in this aspect, a solution is now proposed. Summary of the invention

[0005] The object of the present invention is to provide a method for preparing a flame retardant electrolyte for a sodium ion battery, which is used to solve the technical problems that the prior art uses an organic solution as a solvent for the electrolyte, resulting in the risk of combustion and explosion of the sodium ion battery, and that adding a flame retardant to the electrolyte reduces the conductivity of the electrolyte and other conductive properties.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A method for preparing a flame retardant electrolyte for a sodium ion battery comprises the following steps:

[0008] S1. Add modified diethyl phosphate, acrylic acid, toluene and initiator into a three-necked flask and stir. Raise the temperature of the three-necked flask to 75-85° C. and keep the temperature for 20-23 hours. Post-treat to obtain a conductive additive.

[0009] The synthetic reaction principle of conductive additives is:

[0010]

[0011] S2, adding sodium sulfate, sodium fluoroborate and deionized water into a three-necked flask protected by nitrogen and stirring evenly to obtain a mixed solution 1 for standby use;

[0012] S3, adding the conductive additive and deionized water into a three-necked flask protected by nitrogen and stirring evenly to obtain a mixed solution 2;

[0013] S4. Add mixed solution 2, mixed solution 1 and polyethylene glycol into a beaker and mix well to obtain a flame retardant electrolyte.

[0014] Furthermore, in step S1, the dosage ratio of modified diethyl phosphate and acrylic acid is 2 mol:1 mol, the dosage ratio of modified diethyl phosphate, toluene and initiator is 1 g:5 mL:0.02 g, the initiator is azobisisobutyronitrile, and the post-treatment operation includes: after the reaction is completed, toluene is evaporated under reduced pressure, deionized water is added to a three-necked flask, stirred and dispersed at room temperature for 30-50 minutes, 10 wt% sodium hydroxide is slowly added dropwise to the three-necked flask, the system pH is adjusted to 7, and the solvent is evaporated under reduced pressure to obtain a conductive additive.

[0015] Furthermore, in step S2, the dosage ratio of sodium sulfate, sodium fluoroborate and deionized water is 1.5g:1g:30mL; in step S3, the dosage ratio of the conductive additive and deionized water is 1g:30mL; in step S4, the volume ratio of mixed solution 1, mixed solution 2 and polyethylene glycol is 3:3:4, and the polyethylene glycol is polyethylene glycol-400.

[0016] Further, diethyl chlorophosphate is processed by the following steps:

[0017] A1, adding anhydrous ethanol to a three-necked flask protected by nitrogen and stirring, lowering the temperature of the three-necked flask to -5-0°C, adding dichlorophosphine oxide dropwise to the three-necked flask, and after the addition is complete, keeping the temperature for reaction for 2-3 hours, and naturally raising the temperature of the three-necked flask to room temperature, keeping the temperature for reaction for 2-3 hours, and post-treating to obtain intermediate I;

[0018] The synthetic reaction principle of intermediate I is:

[0019]

[0020] A2. Add sulfonyl chloride and acetone into a three-necked flask protected by nitrogen and stir. At room temperature, add the intermediate I solution dropwise into the three-necked flask. After the addition is complete, stir and react at room temperature for 2-3 hours. Post-treat to obtain diethyl chlorophosphate.

[0021] The synthetic reaction principle of diethyl chlorophosphate is:

[0022]

[0023] Furthermore, in step A1, the dosage ratio of anhydrous ethanol and dichlorophosphine is 5 mL:2 g, and the post-treatment operation includes: after the reaction is completed, vacuum distillation is performed, the internal pressure of the three-necked flask is reduced to 1-1.2 kPa, and the fraction in the temperature range of 68-72 ° C is collected to obtain intermediate I; in step A2, the dosage ratio of sulfonyl chloride, acetone and intermediate I solution is 1 g:3 mL:2 g, and the intermediate I solution is composed of intermediate I and acetone in a weight ratio of 1:1. The post-treatment operation includes: after the reaction is completed, vacuum distillation is performed, the internal pressure of the three-necked flask is reduced to 1-1.2 kPa, and the fraction in the temperature range of 53-55 ° C is collected to obtain diethyl chlorophosphate.

[0024] Furthermore, the preparation method of modified diethyl phosphate is as follows: hydroxyethyl acrylate, anhydrous ether and a catalyst are added to a three-necked flask protected by nitrogen and stirred, the temperature of the three-necked flask is lowered to -5-0°C, diethyl chlorophosphate is slowly added dropwise to the three-necked flask, after the addition is completed, the reaction is kept warm for 2-3 hours, the temperature of the three-necked flask is naturally heated to room temperature, the reaction is kept warm for 20-22 hours, and the modified diethyl phosphate is obtained by post-treatment.

[0025] The synthetic reaction principle of modified diethyl phosphate is:

[0026]

[0027] Furthermore, the dosage ratio of the hydroxyethyl acrylate and diethyl chlorophosphate is 1 mol:1 mol, the dosage ratio of the hydroxyethyl acrylate, anhydrous ether and catalyst is 1 g:10 mL:0.6, the catalyst is composed of triethylamine and cuprous chloride in a dosage ratio of 10 mL:0.3 g, and the post-treatment operation includes: after the reaction is completed, suction filtration, after the filter cake is washed with purified water, the washing liquid and the filtrate are combined to obtain a filtrate, the filtrate is washed twice with 5wt% sodium hydroxide and then washed three times with purified water at 5-8°C, the organic phase is dried with anhydrous magnesium sulfate for 3-5 hours, suction filtration, the filtrate is transferred to a rotary evaporator with a water bath temperature of 45-50°C, and the solvent is evaporated to obtain modified diethyl phosphate.

[0028] The present invention has the following beneficial effects:

[0029] The flame retardant electrolyte of the present invention is prepared by driving an addition reaction between anhydrous ethanol and dichlorophosphine oxide to generate an intermediate I, which is then reacted with sulfonyl chloride, and the hydrogen on the phosphorus of the intermediate I is replaced by chlorine to generate diethyl chlorophosphate. The diethyl chlorophosphate is then subjected to a substitution addition reaction with hydroxyethyl acrylate to prepare a modified diethyl phosphate with olefin double bond modification. The modified diethyl phosphate and acrylic acid are subjected to an acid-base neutralization reaction with sodium hydroxide to prepare a conductive additive. The conductive additive contains a large amount of sodium carboxylate and diethyl phosphate, and the sodium carboxylate can form hydrogen bonds and ions with water molecules. The sub-bond makes sodium carboxylate dissolve in water, and it cooperates with sodium sulfate and sodium fluoroborate to ionize and hydrolyze in the aqueous solution to generate a large number of sodium ions, fluoroborate ions, and sulfate ions, thereby improving the conductivity of the aqueous solution. The solubility of diethyl phosphate in water is low, so that the conductive additive is in a gel state in the aqueous solution. It cooperates with polyethylene glycol-400 to maintain the dispersion stability of the system, increase the boiling point of the electrolyte, and reduce the freezing point of the electrolyte, so that the electrolyte can be used in a wide temperature range. The electrolyte uses deionized water as a solvent, which makes it have good flame retardancy and avoids combustion during the operation of the battery. DETAILED DESCRIPTION

[0030] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Example 1

[0032] A method for preparing a flame-retardant electrolyte for a sodium ion battery in this embodiment comprises the following steps:

[0033] S1. Preparation of diethyl chlorophosphate

[0034] Weigh: 50 mL of anhydrous ethanol is added to a three-necked flask protected by nitrogen and stirred. The temperature of the three-necked flask is lowered to -5°C. 20 g of phosphine oxychloride is added dropwise to the three-necked flask. After the addition is completed, the reaction is kept warm for 2 hours. The temperature of the three-necked flask is naturally raised to room temperature. The reaction is kept warm for 2 hours. The pressure inside the three-necked flask is reduced to 1 kPa by vacuum distillation. The fraction in the temperature range of 68-72°C is collected to obtain intermediate I;

[0035] Add intermediate I and acetone in a weight ratio of 1:1 into a beaker and mix well to obtain an intermediate I solution for later use;

[0036] Weigh: 10 g of sulfonyl chloride and 30 mL of acetone are added into a three-necked flask protected by nitrogen and stirred. At room temperature, 20 g of the intermediate I solution is added dropwise into the three-necked flask. After the addition is complete, stir and react at room temperature for 2 h. Perform vacuum distillation to reduce the internal pressure of the three-necked flask to 1 kPa, and collect the fraction in the temperature range of 53-55 ° C to obtain diethyl chlorophosphate.

[0037] S2. Preparation of modified diethyl chlorophosphate

[0038] Add triethylamine and cuprous chloride in a ratio of 10 mL:0.3 g into a beaker and mix well to obtain a catalyst for later use;

[0039] Weigh: 11.6 g of hydroxyethyl acrylate, 116 mL of anhydrous ether and 6 g of catalyst, add them to a three-necked flask protected by nitrogen and stir, lower the temperature of the three-necked flask to -5°C, slowly add 17.3 g of diethyl chlorophosphate to the three-necked flask, after the addition is complete, keep warm for 2 hours, the temperature of the three-necked flask naturally rises to room temperature, keeps warm for 20 hours, filter, wash the filter cake with purified water, combine the washing liquid and the filtrate to obtain a filtrate, wash the filtrate twice with 5wt% sodium hydroxide and then wash three times with 5°C purified water, dry the organic phase with anhydrous magnesium sulfate for 3 hours, filter, transfer the filtrate to a rotary evaporator with a water bath temperature of 45°C, evaporate the solvent to obtain modified diethyl phosphate.

[0040] S3. Preparation of conductive additives

[0041] Weigh: 50.4 g of modified diethyl phosphate, 7.2 g of acrylic acid, 252 mL of toluene and 1 g of azobisisobutyronitrile, add into a three-necked flask and stir, raise the temperature of the three-necked flask to 75°C, keep warm for 20 hours, evaporate the toluene under reduced pressure, add deionized water into the three-necked flask, stir and disperse at room temperature for 30 minutes, slowly add 10 wt% sodium hydroxide into the three-necked flask, adjust the system pH to 7, evaporate the solvent under reduced pressure to obtain a conductive additive.

[0042] S4. Preparation of mixed solution 1

[0043] Sodium sulfate, sodium fluoroborate and deionized water were added into a nitrogen-protected three-necked flask at a ratio of 1.5 g:1 g:30 mL and stirred evenly to obtain a mixed solution 1.

[0044] S5. Preparation of mixed solution II

[0045] The conductive additive and deionized water were added into a nitrogen-protected three-necked flask at a ratio of 1 g:30 mL and stirred evenly to obtain a mixed solution II.

[0046] S6. Preparation of flame retardant electrolyte

[0047] Add mixed solution 2, mixed solution 1 and polyethylene glycol-400 into a beaker in a volume ratio of 3:3:4 and mix well to obtain a flame retardant electrolyte.

[0048] Example 2

[0049] A method for preparing a flame-retardant electrolyte for a sodium ion battery in this embodiment comprises the following steps:

[0050] S1. Preparation of diethyl chlorophosphate

[0051] Weigh: 50 mL of anhydrous ethanol is added to a three-necked flask protected by nitrogen and stirred. The temperature of the three-necked flask is lowered to -3°C. 20 g of phosphine oxychloride is added dropwise to the three-necked flask. After the addition is complete, the reaction is kept warm for 2.5 hours. The temperature of the three-necked flask is naturally raised to room temperature. The reaction is kept warm for 2.5 hours. The pressure inside the three-necked flask is reduced to 1.1 kPa by vacuum distillation. The fraction in the temperature range of 68-72°C is collected to obtain intermediate I;

[0052] Add intermediate I and acetone in a weight ratio of 1:1 into a beaker and mix well to obtain an intermediate I solution for later use;

[0053] Weigh: 10 g of sulfonyl chloride and 30 mL of acetone are added into a three-necked flask protected by nitrogen and stirred. At room temperature, 20 g of the intermediate I solution is added dropwise into the three-necked flask. After the addition is complete, stir and react at room temperature for 2.5 h. Distill under reduced pressure until the internal pressure of the three-necked flask is reduced to 1.1 kPa. Collect the fraction in the temperature range of 53-55 ° C to obtain diethyl chlorophosphate.

[0054] S2. Preparation of modified diethyl chlorophosphate

[0055] Add triethylamine and cuprous chloride in a ratio of 10 mL:0.3 g into a beaker and mix well to obtain a catalyst for later use;

[0056] Weigh: 11.6 g of hydroxyethyl acrylate, 116 mL of anhydrous ether and 6 g of catalyst, add them to a three-necked flask protected by nitrogen and stir, lower the temperature of the three-necked flask to -3°C, slowly add 17.3 g of diethyl chlorophosphate to the three-necked flask, after the addition is complete, keep warm for 2.5 hours, the temperature of the three-necked flask naturally rises to room temperature, keep warm for 21 hours, filter, wash the filter cake with purified water, combine the washing liquid and the filtrate to obtain a filtrate, wash the filtrate twice with 5wt% sodium hydroxide and then wash three times with 7°C purified water, dry the organic phase with anhydrous magnesium sulfate for 4 hours, filter, transfer the filtrate to a rotary evaporator with a water bath temperature of 47°C, evaporate the solvent to obtain modified diethyl phosphate.

[0057] S3. Preparation of conductive additives

[0058] Weigh: 50.4 g of modified diethyl phosphate, 7.2 g of acrylic acid, 252 mL of toluene and 1 g of azobisisobutyronitrile, add into a three-necked flask and stir, raise the temperature of the three-necked flask to 80°C, keep warm for 21.5 hours, evaporate the toluene under reduced pressure, add deionized water into the three-necked flask, stir and disperse at room temperature for 40 minutes, slowly drop 10 wt% sodium hydroxide into the three-necked flask, adjust the system pH to 7, evaporate the solvent under reduced pressure to obtain a conductive additive.

[0059] S4. Preparation of mixed solution 1

[0060] Sodium sulfate, sodium fluoroborate and deionized water were added into a nitrogen-protected three-necked flask at a ratio of 1.5 g:1 g:30 mL and stirred evenly to obtain a mixed solution 1.

[0061] S5. Preparation of mixed solution II

[0062] The conductive additive and deionized water were added into a nitrogen-protected three-necked flask at a ratio of 1 g:30 mL and stirred evenly to obtain a mixed solution II.

[0063] S6. Preparation of flame retardant electrolyte

[0064] Add mixed solution 2, mixed solution 1 and polyethylene glycol-400 into a beaker in a volume ratio of 3:3:4 and mix well to obtain a flame retardant electrolyte.

[0065] Example 3

[0066] A method for preparing a flame-retardant electrolyte for a sodium ion battery in this embodiment comprises the following steps:

[0067] S1. Preparation of diethyl chlorophosphate

[0068] Weigh: 50 mL of anhydrous ethanol is added to a three-necked flask protected by nitrogen and stirred. The temperature of the three-necked flask is reduced to 0°C. 20 g of phosphine oxychloride is added dropwise to the three-necked flask. After the addition is completed, the reaction is kept warm for 3 hours. The temperature of the three-necked flask is naturally raised to room temperature. The reaction is kept warm for 3 hours. The pressure inside the three-necked flask is reduced to 1.2 kPa by vacuum distillation. The fraction in the temperature section of 72°C is collected to obtain intermediate I;

[0069] Add intermediate I and acetone in a weight ratio of 1:1 into a beaker and mix well to obtain an intermediate I solution for later use;

[0070] Weigh: 10 g of sulfonyl chloride and 30 mL of acetone, add them into a three-necked flask protected by nitrogen and stir. Under room temperature, add 20 g of intermediate I solution dropwise into the three-necked flask. After the addition is complete, stir and react at room temperature for 3 h. Perform vacuum distillation to reduce the internal pressure of the three-necked flask to 1.2 kPa. Collect the fraction in the temperature zone of 55 ° C to obtain diethyl chlorophosphate.

[0071] S2. Preparation of modified diethyl chlorophosphate

[0072] Add triethylamine and cuprous chloride in a ratio of 10 mL:0.3 g into a beaker and mix well to obtain a catalyst for later use;

[0073] Weigh: 11.6 g of hydroxyethyl acrylate, 116 mL of anhydrous ether and 6 g of catalyst, add them to a three-necked flask protected by nitrogen and stir, lower the temperature of the three-necked flask to 0°C, slowly add 17.3 g of diethyl chlorophosphate to the three-necked flask, and after the addition is complete, keep warm for 3 hours. The temperature of the three-necked flask naturally rises to room temperature and keeps warm for 22 hours. Filter by suction, wash the filter cake with purified water, combine the washing liquid with the filtrate to obtain a filtrate, wash the filtrate twice with 5wt% sodium hydroxide and then wash three times with purified water at 5-8°C, dry the organic phase with anhydrous magnesium sulfate for 5 hours, filter by suction, transfer the filtrate to a rotary evaporator with a water bath temperature of 50°C, evaporate the solvent, and obtain modified diethyl phosphate.

[0074] S3. Preparation of conductive additives

[0075] Weigh: 50.4 g of modified diethyl phosphate, 7.2 g of acrylic acid, 252 mL of toluene and 1 g of azobisisobutyronitrile, add into a three-necked flask and stir, raise the temperature of the three-necked flask to 85°C, keep warm for 23 hours, evaporate the toluene under reduced pressure, add deionized water into the three-necked flask, stir and disperse at room temperature for 50 minutes, slowly drop 10 wt% sodium hydroxide into the three-necked flask, adjust the system pH to 7, evaporate the solvent under reduced pressure to obtain a conductive additive.

[0076] S4. Preparation of mixed solution 1

[0077] Sodium sulfate, sodium fluoroborate and deionized water were added into a nitrogen-protected three-necked flask at a ratio of 1.5 g:1 g:30 mL and stirred evenly to obtain a mixed solution 1.

[0078] S5. Preparation of mixed solution II

[0079] The conductive additive and deionized water were added into a nitrogen-protected three-necked flask at a ratio of 1 g:30 mL and stirred evenly to obtain a mixed solution II.

[0080] S6. Preparation of flame retardant electrolyte

[0081] Add mixed solution 2, mixed solution 1 and polyethylene glycol-400 into a beaker in a volume ratio of 3:3:4 and mix well to obtain a flame retardant electrolyte.

[0082] Comparative Example 1

[0083] The difference between this comparative example and Example 1 is that step S2 is eliminated and modified diethyl phosphate is not added in step S3.

[0084] Comparative Example 2

[0085] The difference between this comparative example and Example 1 is that step S3 is omitted and no conductive additive is added in step S5.

[0086] Comparative Example 3

[0087] The difference between this comparative example and Example 1 is that polyethylene glycol is not added in step S5.

[0088] Performance Test:

[0089] The combustion performance, heat resistance and electrical conductivity of the flame retardant electrolyte prepared in Examples 1-3 and Comparative Examples 1-3 were tested, wherein the heat resistance was measured by measuring the freezing point and boiling point of the sample under the international standard atmospheric pressure, the electrical conductivity was measured by using a conductivity meter of model DDS-307A to test the conductivity of the sample at 25°C, and the combustion performance was measured by adding the sample to a test container, keeping it in close contact with an open flame for 10 seconds, then removing the open flame and observing the continuous burning time of the sample. The specific test results are shown in the following table:

[0090]

[0091] Data Analysis:

[0092] Comparative analysis of the data in the above table shows that the flame retardant electrolyte prepared by the present invention uses purified water as a solvent, and the synthetic conductive additive is combined with other additives to reduce the freezing point of the flame retardant electrolyte to -43.2°C, increase the boiling point to 196.3°C, and achieve a conductivity of 16.6 mS·cm -1 , and is non-flammable, and all test data are better than those of the comparative example, indicating that the flame-retardant electrolyte prepared by the present invention has a wide temperature range and ultra-high conductivity, and is suitable for use in sodium ion batteries.

[0093] The above contents are merely examples and explanations of the structure of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

[0094] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0095] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for preparing a flame retardant electrolyte for a sodium ion battery, characterized in that: The following steps are involved: S1. Add modified diethyl phosphate, acrylic acid, toluene and initiator into a three-necked flask and stir. Raise the temperature of the three-necked flask to 75-85° C. and keep the temperature for 20-23 hours. Post-treat to obtain a conductive additive. S2, adding sodium sulfate, sodium fluoroborate and deionized water into a three-necked flask protected by nitrogen and stirring evenly to obtain a mixed solution 1 for standby use; S3, adding the conductive additive and deionized water into a three-necked flask protected by nitrogen and stirring evenly to obtain a mixed solution 2; S4, adding mixed solution 2, mixed solution 1 and polyethylene glycol into a beaker and mixing evenly to obtain a flame retardant electrolyte; The preparation method of modified diethyl phosphate is as follows: hydroxyethyl acrylate, anhydrous ether and a catalyst are added into a three-necked flask protected by nitrogen and stirred, the temperature of the three-necked flask is lowered to -5-0°C, diethyl chlorophosphate is slowly added dropwise into the three-necked flask, after the addition is completed, the temperature is kept warm for 2-3 hours, the temperature of the three-necked flask is naturally heated to room temperature, the temperature is kept warm for 20-22 hours, and the modified diethyl phosphate is obtained by post-treatment.

2. The method for preparing a flame-retardant electrolyte for a sodium ion battery according to claim 1, characterized in that: In step S1, the dosage ratio of modified diethyl phosphate and acrylic acid is 2 mol:1 mol, the dosage ratio of modified diethyl phosphate, toluene and initiator is 1 g:5 mL:0.02 g, the initiator is azobisisobutyronitrile, and the post-treatment operation includes: after the reaction is completed, toluene is distilled off under reduced pressure, deionized water is added to the three-necked flask, stirred and dispersed at room temperature for 30-50 minutes, 10 wt% sodium hydroxide is slowly added dropwise to the three-necked flask, the system pH is adjusted to 7, and the solvent is distilled off under reduced pressure to obtain a conductive additive.

3. The method for preparing a flame-retardant electrolyte for a sodium ion battery according to claim 1, characterized in that: In step S2, the dosage ratio of sodium sulfate, sodium fluoroborate and deionized water is 1.5g:1g:30mL; in step S3, the dosage ratio of the conductive additive and deionized water is 1g:30mL; in step S4, the volume ratio of the mixed solution 1, the mixed solution 2 and the polyethylene glycol is 3:3:4, and the polyethylene glycol is polyethylene glycol-400.

4. The method for preparing a flame-retardant electrolyte for a sodium ion battery according to claim 1, characterized in that: Diethyl chlorophosphate is obtained by the following steps: A1, adding anhydrous ethanol to a three-necked flask protected by nitrogen and stirring, lowering the temperature of the three-necked flask to -5-0°C, adding dichlorophosphine oxide dropwise to the three-necked flask, and after the addition is complete, keeping the temperature for reaction for 2-3 hours, and naturally raising the temperature of the three-necked flask to room temperature, keeping the temperature for reaction for 2-3 hours, and post-treating to obtain intermediate I; A2. Add sulfonyl chloride and acetone into a three-necked flask protected by nitrogen and stir. At room temperature, add the intermediate I solution dropwise into the three-necked flask. After the addition is complete, stir and react at room temperature for 2-3 hours. Post-treat to obtain diethyl chlorophosphate.

5. The method for preparing a flame-retardant electrolyte for a sodium ion battery according to claim 4, characterized in that: In step A1, the usage ratio of anhydrous ethanol and phosphine oxychloride is 5 mL:2 g, and the post-treatment operation includes: after the reaction is completed, vacuum distillation is performed, the internal pressure of the three-necked flask is reduced to 1-1.2 kPa, and the fraction in the temperature section of 68-72° C. is collected to obtain intermediate I; in step A2, the usage ratio of sulfonyl chloride, acetone and intermediate I solution is 1 g:3 mL:2 g, and the intermediate I solution is composed of intermediate I and acetone in a weight ratio of 1:1, and the post-treatment operation includes: after the reaction is completed, vacuum distillation is performed, the internal pressure of the three-necked flask is reduced to 1-1.2 kPa, and the fraction in the temperature section of 53-55° C. is collected to obtain diethyl chlorophosphate.

6. The method for preparing a flame-retardant electrolyte for a sodium ion battery according to claim 1, characterized in that: The usage ratio of the hydroxyethyl acrylate and diethyl chlorophosphate is 1 mol:1 mol, and the usage ratio of the hydroxyethyl acrylate, anhydrous ether and catalyst is 1 g:10 mL: 0.6, the catalyst is composed of triethylamine and cuprous chloride in a dosage ratio of 10mL:0.3g, and the post-treatment operation includes: After the reaction is completed, the reaction is filtered, the filter cake is washed with purified water, the washing liquid and the filtrate are combined to obtain a filtrate, the filtrate is washed twice with 5wt% sodium hydroxide and then three times with purified water at 5-8°C, the organic phase is dried over anhydrous magnesium sulfate for 3-5h, filtered, and the filtrate is transferred to a rotary evaporator with a water bath temperature of 45-50°C, and the solvent is evaporated to obtain modified diethyl phosphate.