Intensive Ultra-High Strength Hot-Rolled Coil Continuous Heat Treatment Line and its Process Method

By using an intensive, ultra-high strength hot-rolled coil continuous heat treatment line, and combining a continuous heating furnace with a variety of cooling nozzles, the problems of poor strip shape and uneven performance during the traditional hot-rolled steel strip quenching process have been solved, achieving efficient steel strip quenching and improved production efficiency.

CN118109679BActive Publication Date: 2026-11-17武汉钢铁有限公司
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311788688.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-25
Publication Date
2026-11-17
Estimated Expiration
2043-12-25

AI Technical Summary

Technical Problem

Traditional hot-rolled steel strip quenching processes suffer from problems such as poor strip shape, substandard surface quality, and uneven performance, and have low production efficiency, especially for steel plates with inconsistent thickness.

Method used

An intensive, ultra-high strength hot-rolled coil continuous heat treatment line is adopted, including equipment such as uncoilers, shearers, straighteners, shot blasting machines, heating furnaces, quenching machines, and stackers. Through a combination of continuous atmosphere-protected heating furnaces and multiple cooling nozzles, continuous quenching and efficient cooling of steel strips are achieved, ensuring uniform heat exchange in different areas.

Benefits of technology

It enables continuous quenching of steel strips of different thicknesses, avoids poor plate shape and performance inhomogeneity, improves production efficiency and equipment utilization, and realizes the "coil-plate" production mode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118109679B_ABST
    Figure CN118109679B_ABST
Patent Text Reader

Abstract

This invention discloses an intensive, continuous heat treatment line for ultra-high strength hot-rolled coils and its process method. The line includes an uncoiler, a No. 1 shear, a straightener, a No. 2 shear, a shot blasting machine, a heating furnace, a quenching machine, a shaper, a laser cutter, and a stacker, arranged sequentially along the treatment path. The heating furnace is a continuous atmosphere-protected furnace with a roller-bottom structure for top and bottom heating, divided into several temperature control zones along its length. The quenching machine uses flat nozzles and slit nozzles in its high-temperature zone at the front, and round-hole nozzles in its low-temperature zone at the middle and rear. Both the flat nozzles and slit nozzles are segmented along the width of the steel strip, symmetrically distributed on the left and right sides and top and bottom, with independent control of water flow in each segment. The round-hole nozzles are not segmented along the width of the steel strip. This invention provides high production line utilization efficiency and avoids issues such as poor strip shape, substandard surface quality, and uneven performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of heat treatment of hot-rolled steel strip, specifically to an intensive continuous heat treatment line for ultra-high strength hot-rolled coils and its process. Background Technology

[0002] With the development of industrial technology, the demand for hot-rolled ultra-high strength steel in the steel industry has been increasing year by year. As the core of improving the strength of hot-rolled steel strip, the heat treatment technology of hot-rolled steel strip has become of paramount importance.

[0003] Currently, in the industry, hot-rolled steel strips with a thickness of 3mm or more are generally produced into ultra-high-strength steel plates using offline heat treatment. Typically, the strips are first cut into plates of a certain length, followed by shot blasting, heating, quenching, and tempering. During quenching, a roller-type water quenching method is mainly used, equipped with high-pressure round nozzles or high-pressure slit spraying. The quenching plate shape is optimized by adjusting the water-to-water ratio and the strip speed. The steel plate moves at high speed, the production line is long, the floor space is large, and there are production intervals between plates. Production in single-plate form results in low production line utilization efficiency.

[0004] Furthermore, traditional quenching machines utilize slit-jet or high-pressure water jetting methods to bring water at different pressures into contact with the surface of the hot steel plate, enhancing heat transfer and rapidly cooling the heated steel plate to room temperature. However, slit-jet systems require extremely high precision in the slit size, making it difficult to ensure uniform slit dimensions along the width of the plate. This results in differences in heat transfer across different areas of the steel plate's width. Additionally, water accumulation in the middle of the upper surface of the steel plate along its width makes it difficult to control the plate shape at thin gauges and low speeds. While high-pressure water nozzles are arranged in a staggered pattern, there are still large areas of direct impact and non-impact zones, leading to significant differences in heat transfer between the two areas. These factors directly result in significant structural and thermal stresses in the hot-rolled steel plate during quenching, leading to poor plate shape, substandard surface quality, and uneven performance. Summary of the Invention

[0005] The purpose of this invention is to provide an intensive, continuous heat treatment line for ultra-high strength hot-rolled coils and its process method. This invention has high production line utilization efficiency and avoids phenomena such as poor plate shape, substandard surface quality, and uneven performance.

[0006] The technical solution adopted in this invention is: An intensive, ultra-high strength hot-rolled coil continuous heat treatment line includes an uncoiler, a No. 1 shear, a straightener, a No. 2 shear, a shot blasting machine, a heating furnace, a quenching machine, a strip shaper, a laser cutting machine, and a stacker, arranged sequentially along the processing path. The heating furnace is a continuous atmosphere-protected heating furnace with a roller bottom structure for top and bottom heating. It is divided into several temperature control zones along the length of the furnace, with the upper and lower areas of the steel strip passing through the line being separate temperature control zones. The quenching machine is equipped with several sets of pinch rollers and various symmetrical cooling nozzles. The high-temperature zone at the front uses flat nozzle groups and slit nozzle groups, while the low-temperature zone at the middle and rear uses round-hole nozzle groups. Both the flat nozzle groups and slit nozzle groups are segmented and controlled along the width of the steel strip, symmetrically distributed on the left and right sides and top and bottom. The water flow rate of each segment is independently adjustable. The round-hole nozzles are not segmented along the width of the steel strip.

[0007] Preferably, the combustion system of the heating furnace includes burners, radiant tubes and control valves, metering devices and safety shut-off devices, and provides indirect heating through self-preheating burners installed inside the radiant tubes.

[0008] Preferably, the outlet of the heating furnace and the first set of pinch roller conveyors of the quenching machine are connected in a compact manner, with the distance between them kept within 1000mm.

[0009] Preferably, the water supply pressure of each section of the cooling nozzle is 6 to 9 bar.

[0010] Preferably, the angle between the jet stream of the flat nozzle group and the direction of movement of the steel belt is 10° to 60°, the angle between the jet stream of the slit nozzle group and the direction of movement of the steel belt is 5° to 30°, the slit size of the slit nozzle group on the upper surface of the steel belt is 1.5 to 3 mm, the slit size of the slit nozzle group on the lower surface of the steel belt is 2.0 to 3.5 mm, and the slit size of the slit nozzle group on the upper surface is 0.1 to 0.4 mm smaller than that of the slit nozzle group on the lower surface, and the angle between the jet stream of the round hole nozzle group and the direction of movement of the steel belt is 20° to 80°.

[0011] Preferably, both the flat nozzle assembly and the slit nozzle assembly are divided into 3 to 5 sections along the width of the steel strip, with the middle section being 800 mm wide and the left and right side sections being 200 to 450 mm long.

[0012] Preferably, the tail end of the quenching machine is equipped with a hot air dryer for blowing away moisture from the outer surface of the steel strip.

[0013] Preferably, the second to fourth sets of pinch rollers of the quenching machine are grooved rollers with annular grooves on their surface, while the first set of pinch rollers and other rollers are flat rollers.

[0014] The above-mentioned integrated ultra-high strength hot-rolled coil continuous heat treatment line process is as follows: For ultra-high strength hot-rolled coils with thicknesses ranging from 3mm to 25mm, the strip is first fed to an uncoiler, which automatically uncoils the coil. The strip head is then cut off by a shearing machine (No. 1), followed by straightening by a straightening machine and shot blasting by a shot blasting machine before entering the heating furnace. The strip passes through the heating furnace at a uniform speed of 6–40 m / min. The heating furnace controls the heating of the strip according to its thickness and speed, ensuring that the temperature reaches above the austenitizing temperature after passing through the furnace at a uniform speed. Immediately after exiting the furnace, the strip enters a quenching machine, ensuring its temperature remains above Ac3 by 30°C. During quenching in the quenching machine, the flat nozzle group and slit nozzle group in the high-temperature zone rapidly cool the strip to below the Ms point at a cooling rate of 60–120°C / s. The round-hole nozzle group in the low-temperature zone reduces the cooling rate, allowing the strip to cool further. The martensitic transformation is completed at a cooling rate of 40–80 °C / s, and the steel strip is cooled to room temperature to ensure no quenching backheating. The flow rate of the cooling nozzles and the flow ratio between the upper and lower sides are controlled according to the steel grade and specifications of the steel strip. The flow ratio between the upper and lower sides in each section of the high-temperature zone is 0.65–0.90, and the flow ratio between the upper and lower sides in each section of the low-temperature zone is 0.80–0.95. Then, the shape meter detects the shape of the quenched steel strip and feeds back the relevant shape information to the quenching machine control system for real-time adjustment of the flow rate of each group and section of the cooling nozzles. After the steel strip passes through the shape meter, the cutting head of the laser cutting machine moves along the roller conveyor with the steel strip and simultaneously performs a fixed-length transverse cut on the quenched steel strip. Finally, the steel strip enters the stacker for stacking and marking. After the stacked plates are bundled, they are hoisted off the line and sent to the finished product warehouse.

[0015] Preferably, a waiting position for a vacuum suction cup is set at the exit of the shot blasting machine. Under normal circumstances, the steel strip passes through the No. 2 shearing machine without being cut. In an emergency, after the steel strip is straightened by the straightening machine, the No. 2 shearing machine cuts the steel strip to a fixed length. After being shot blasted by the shot blasting machine, the steel strip is stacked and removed from the production line by the vacuum suction cup.

[0016] The beneficial effects of this invention are: This invention addresses the issue of single hot-rolled steel coils not being cut into plates after uncoiling, straightening, and shot blasting. The steel strip continuously enters the heating furnace for quenching, and the cooling rate can be controlled by adjusting the cooling water flow rate. This allows for quenching of steel strips with thicknesses ranging from 3mm to 25mm. The quenched high-strength steel is then cross-cut and stacked, achieving a "coil-to-plate" production model with high production line utilization efficiency. In this invention, the quenching machine integrates multiple cooling nozzles, which are segmented and controllable along the width of the steel strip. This ensures symmetrical and controllable heat exchange in different areas along the strip's width, avoiding issues such as poor strip shape, substandard surface quality, and uneven performance. It enables continuous quenching of hot-rolled steel coils of different thicknesses, solving the production interval problem inherent in traditional ultra-high-strength steel single-plate heat treatment, shortening production line length, and improving production efficiency and equipment utilization. Attached Figure Description

[0017] Figure 1This is a schematic diagram of an intensive ultra-high strength hot-rolled coil continuous heat treatment line in an embodiment of the present invention.

[0018] Figure 2 This is a simplified structural diagram of the quenching machine in an embodiment of the present invention.

[0019] Figure 3 This is a simplified layout diagram of the quenching machine in an embodiment of the present invention.

[0020] In the diagram: 1. Uncoiler; 2. Steel strip; 3. Shearing machine #1; 4. Straightening machine; 5. Shearing machine #2; 6. Shot blasting machine; 7. Heating furnace; 8. Quenching machine; 9. Plate shaper; 10. Laser cutting machine; 11. Stacker; 12. Vacuum suction cup crane; 20. Group 1 pinch roller conveyor; 21. Flat nozzle group; 22. Slit nozzle group; 23. Round hole nozzle group; 24-26. Groups 2 to 4 pinch roller conveyors; L1-L5. Upper flat nozzle group segmented water tank; L6-L10. Lower flat nozzle group segmented water tank; L11-L15. Upper slit nozzle group segmented water tank; L16-L20. Lower slit nozzle group segmented water tank; L21. Upper round hole nozzle group water tank; L22. Lower round hole nozzle group water tank. Detailed Implementation

[0021] The present invention will be further described below with reference to the accompanying drawings and embodiments.

[0022] Example 1 This embodiment discloses an intensive continuous heat treatment line for ultra-high strength hot-rolled coils, such as... Figure 1 As shown, the process includes an uncoiler 1, a shearing machine 3, a straightener 4, a shearing machine 5, a shot blasting machine 6, a heating furnace 7, a quenching machine 8, a shaper 9, a laser cutter 10, and a stacker 11 arranged sequentially along the processing path. The overall process flow is as follows: For ultra-high strength hot-rolled coils with a thickness of 3mm to 25mm, the coils are first fed to the uncoiler 1, which automatically uncoils them. The steel strip 2 head is cut off by the shearing machine 3, and then passes through the straightener 4 for straightening, the shot blasting machine 6 for shot blasting, and then enters the heating furnace 7. After the steel strip 2 is heated to the predetermined temperature in the heating furnace 7, it enters the quenching machine 8 for quenching. Then, the shaper 9 detects the shape of the quenched steel strip 2, and the laser cutter 10 cuts the continuously moving steel strip 2 to length. The cut steel strip 2 then enters the stacker 11 for stacking and unloading.

[0023] Regarding the functions of shear machine #2 (5) and vacuum suction cup hanger #12: like Figure 1As shown, the #2 shearing machine 5 is located between the straightening machine 4 and the shot blasting machine 6. The vacuum suction cup crane 12 is in the waiting position at the exit of the shot blasting machine 6. Under normal circumstances, the steel strip 2 passes through the #2 shearing machine 5 without being cut. In an emergency, after the steel strip 2 is straightened by the straightening machine 4, the #2 shearing machine 5 can cut the steel strip 2 to a fixed length. After the fixed-length cut steel strip 2 is shot blasted by the shot blasting machine 6, it is stacked and unloaded by the vacuum suction cup crane 12.

[0024] Regarding heating furnace 7 and its function: Heating furnace 7 is a continuous atmosphere protection heating furnace. It adopts a roller bottom structure with heating from top and bottom. Its combustion system includes burners, radiant tubes and control valves, metering devices and safety shut-off devices. It is indirectly heated by self-preheating burners installed in the radiant tubes.

[0025] In this embodiment, the maximum furnace temperature of the heating furnace 7 is 1100°C, and it operates under a nitrogen protective atmosphere. The heating furnace 7 is 100 meters long, and the upper and lower areas of the steel strip passing through the line are separate temperature control areas. It is divided into 20 segments and 40 temperature control areas along the length of the furnace.

[0026] During operation, the steel strip 2 passes through the heating furnace 7 at a constant speed (the speed is not adjustable and is generally less than 40 m / min; in this embodiment, it is 6–40 m / min). The combustion system of the heating furnace 7 controls the burners to heat the steel strip 2 according to the thickness of the steel strip 2 and the running speed, ensuring that the temperature of the steel strip 2 reaches above the austenitizing temperature, which is the quenching temperature, after passing through the heating furnace 7 at a constant speed. The steel strip 2 adopts a constant speed running and continuous heating method, which shortens the heating and heat equalization time, improves production efficiency, and shortens the production line length.

[0027] The outlet of the heating furnace 7 and the first set of pinch roller conveyors 20 of the quenching machine 8 are tightly connected, with the spacing maintained within 1000mm. This ensures that the steel strip 2 is heated to the austenitizing temperature at a uniform speed through the heating furnace 7 and immediately enters the quenching machine 8 after exiting the furnace, avoiding temperature drop during the process and ensuring that the temperature of the steel strip 2 is maintained above Ac3 by 30℃.

[0028] Regarding the quenching machine 8 and its function: like Figure 2As shown, the quenching machine 8 is equipped with several sets of pinch rollers and various symmetrical cooling nozzles along its line. The cooling nozzles include a flat nozzle group 21, a slit nozzle group 22, and a round hole nozzle group 23. The high-temperature zone at the front adopts "flat nozzle group 21 + slit nozzle group 22", and the low-temperature zone at the middle and rear adopts the round hole nozzle group 23. During quenching, the flat nozzle group 21 and slit nozzle group 22 in the high-temperature zone rapidly cool the steel strip 2 to below the Ms point, with a cooling rate of 60-120℃ / s. The round hole nozzle group 23 in the low-temperature zone reduces the cooling rate, allowing the steel strip 2 to complete the martensitic phase transformation, with a cooling rate of 40-80℃ / s, and cools the steel strip 2 to room temperature, ensuring that there is no quenching backheating phenomenon.

[0029] In this embodiment, the water supply pressure of each section of cooling nozzles (flat nozzle group 21, slit nozzle group 22, and round hole nozzle group 23) is 6-9 bar; the angle between the jet flow of the flat nozzle group 21 and the direction of movement of the steel belt 2 is 10°-60°, the angle between the jet flow of the slit nozzle group 22 and the direction of movement of the steel belt 2 is 5°-30°, the slit size of the slit nozzle group 22 on the upper surface of the steel belt is 1.5-3 mm, the slit size of the slit nozzle group 22 on the lower surface of the steel belt is 2.0-3.5 mm, and the slit nozzle group 22 on the upper surface is 0.1-0.4 mm smaller than the slit nozzle group 22 on the lower surface, and the angle between the jet flow of the round hole nozzle group 23 and the direction of movement of the steel belt 2 is 20°-80°.

[0030] Because the width of steel strip 2 ranges from 1000 to 2000 mm, heat transfer varies in different areas along the width of steel strip 2. To avoid issues such as poor plate shape, substandard surface quality, and uneven performance, such as... Figure 3 As shown, the flat nozzle group 21 and the slit nozzle group 22 in the high-temperature zone are both segmented along the width direction of the steel strip 2, generally divided into 3 to 5 segments, symmetrically distributed on the left and right sides and top and bottom. The width of the middle segment is 800 mm, and the length of each segment on the left and right sides is 200 to 450 mm. The water flow rate of each segment can be independently adjusted to achieve adjustable and controllable water cooling speed in the length and width directions of the steel strip 2. The round hole nozzle in the low-temperature zone is not segmented along the width direction of the steel strip.

[0031] In this embodiment, both the flat nozzle assembly 21 and the slit nozzle assembly 22 in the high-temperature zone are divided into 5 segments along the width of the steel strip 2. The lengths of each segment are 200mm, 400mm, 800mm, 400mm, and 200mm, respectively, with a middle width of 800mm. The segments are symmetrically distributed on the left and right sides and top and bottom, and the water flow rate of each segment can be independently adjusted. Figure 3As shown, L1-L5 are segmented water tanks for upper flat nozzle groups, L6-L10 are segmented water tanks for lower flat nozzle groups, L11-L15 are segmented water tanks for upper slit nozzle groups, L16-L20 are segmented water tanks for lower slit nozzle groups, L21 is a water tank for upper round hole nozzle groups, and L22 is a water tank for lower round hole nozzle groups.

[0032] For different steel grades and specifications, corresponding upper and lower flow control is set. The flow ratio of the upper and lower symmetrical nozzles is set according to the product specifications. The setting range for each section in the high temperature zone is 0.65 to 0.90, and the setting range for each section in the low temperature zone is 0.80 to 0.95.

[0033] The quenching machine 8 is equipped with a hot air dryer at the tail end, which can dry the moisture on the outer surface of the steel strip 2.

[0034] The second to fourth sets of pinch roller conveyors (24-26) of the quenching machine 8 use grooved rollers with annular grooves on their surfaces. The first set of pinch roller conveyors 20 and other roller conveyors use flat rollers. The grooved rollers are used to constrain the deformation of the steel strip 2 after the nozzles have cooled, and at the same time, to guide the cooling water sprayed from the nozzles quickly and orderly in the forward direction of the steel strip 2, so as to achieve uniform and orderly quenching and reduce the uneven cooling of the surface of the steel strip 2 by the cooling water after heat exchange. The flat rollers are used to constrain the deformation of the steel strip 2 after cooling, and at the same time, to block the remaining cooling water after heat exchange on the surface of the steel strip 2 along the forward direction of the steel strip 2 from the nozzles, so as to prevent the cooling water from continuing to flow into the low-pressure cooling zone of the quenching machine along the forward direction of the steel strip 2, thus realizing the flow rate zone control.

[0035] A certain hot-rolled ultra-high-strength steel was quenched after heating using the process parameters shown in Table 1. Table 1 lists the relevant equipment layout and parameters. The cooling rates of hot-rolled ultra-high-strength steel of different thicknesses differ above and below the martensitic transformation initiation temperature, with the cooling rate above the initiation temperature being lower than that below. In this embodiment, the steel strip 2 has dimensions of 12*2000*6000mm and a running speed of 16m / min. During the quenching process of the 12mm hot-rolled ultra-high-strength steel, the cooling rates above and below the martensitic transformation initiation temperature are 62℃ / s and 115℃ / s, respectively. After quenching, the tensile strength of the steel plate reaches 1650MPa.

[0036] Table 1 Process Parameters

[0037] Regarding plate shaper 9, laser cutting machine 10, and stacker crane 11: The shape measuring instrument 9 detects the shape of the quenched steel strip 2 and feeds back the relevant shape information to the control system of the quenching machine 8, which is used to adjust the water flow rate of each group and section of nozzles in real time. After the steel strip 2 passes through the shape measuring instrument 9, the cutting head of the laser cutting machine 10 moves along the roller conveyor with the steel strip 2 and simultaneously cuts the quenched steel strip 2 into length laterally. Then the steel strip 2 enters the stacker 11 for stacking and marking. After the stacked plates are bundled, they are hoisted off the line and sent to the finished product warehouse.

[0038] This invention addresses the issue of hot-rolled steel coils not being cut into plates after uncoiling, straightening, and shot blasting. The steel strip 2 continuously enters the heating furnace for quenching, and the cooling rate can be controlled by adjusting the cooling water flow rate. This allows for quenching of steel strips 2 with different thicknesses ranging from 3mm to 25mm. The quenched high-strength steel is then cross-cut and stacked, achieving a "coil-plate" production mode with high production line utilization efficiency. In this invention, the quenching machine 8 integrates multiple cooling nozzles, which are segmented and controllable along the width of the steel strip 2. This ensures symmetrical and controllable heat exchange in different areas along the width of the steel strip 2, avoiding issues such as poor plate shape, substandard surface quality, and uneven performance. It enables continuous quenching of hot-rolled steel coils of different thicknesses, solving the production interval problem inherent in traditional ultra-high-strength steel single-plate heat treatment, shortening the production line length, and improving production efficiency and equipment utilization.

[0039] The embodiments described above are some, but not all, of the embodiments of this application. The detailed description of the embodiments of this application is not intended to limit the scope of the claimed application, but merely to illustrate selected embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of this application without inventive effort are within the scope of protection of this application.

Claims

1. A process method for an intensive continuous heat treatment line for ultra-high strength hot-rolled coils, characterized in that: The processing line includes an uncoiler, a No. 1 shear, a straightener, a No. 2 shear, a shot blasting machine, a heating furnace, a quenching machine, a strip shaper, a laser cutting machine, and a stacker, arranged sequentially along the processing path. The heating furnace is a continuous atmosphere-protected heating furnace with a roller bottom structure for heating from both the top and bottom. It is divided into several temperature control zones along the length of the furnace, and the upper and lower areas of the steel strip passing through the line are separate temperature control zones. The quenching machine is equipped with several sets of pinch rollers and various symmetrical cooling nozzles. The high-temperature zone at the front uses flat nozzle groups and slit nozzle groups, while the low-temperature zone in the middle and rear uses round hole nozzle groups. Both the flat nozzle groups and slit nozzle groups are segmented along the width of the steel strip and are symmetrically distributed on the left and right sides and top and bottom. The water flow rate of each segment is independently adjustable. The round hole nozzles are not segmented along the width of the steel strip. For ultra-high strength hot-rolled coils with thicknesses ranging from 3mm to 25mm, the strip is first fed to an uncoiler, which automatically uncoils the coil. The strip head is then cut off by a shearing machine (No. 1), followed by straightening by a straightening machine and shot blasting by a shot blasting machine before entering the heating furnace. The strip passes through the heating furnace at a uniform speed of 6–40 m / min. The heating furnace controls the heating of the strip according to its thickness and speed, ensuring that the temperature reaches above the austenitizing temperature after passing through the furnace at a uniform speed. Immediately after exiting the furnace, the strip enters a quenching machine, ensuring its temperature remains above Ac3 by 30°C. During quenching in the quenching machine, the flat nozzle group and slit nozzle group in the high-temperature zone rapidly cool the strip to below the Ms point at a cooling rate of 60–120°C / s. The round-hole nozzle group in the low-temperature zone reduces the cooling rate, allowing the strip to cool further. The martensitic transformation is completed at a cooling rate of 40–80 °C / s, and the steel strip is cooled to room temperature to ensure no quenching backheating. The flow rate of the cooling nozzles and the flow ratio between the upper and lower sides are controlled according to the steel grade and specifications of the steel strip. The flow ratio between the upper and lower sides in each section of the high-temperature zone is 0.65–0.90, and the flow ratio between the upper and lower sides in each section of the low-temperature zone is 0.80–0.

95. Then, the shape meter detects the shape of the quenched steel strip and feeds back the relevant shape information to the quenching machine control system for real-time adjustment of the flow rate of each group and section of the cooling nozzles. After the steel strip passes through the shape meter, the cutting head of the laser cutting machine moves along the roller conveyor with the steel strip and simultaneously performs a fixed-length transverse cut on the quenched steel strip. Finally, the steel strip enters the stacker for stacking and marking. After the stacked plates are bundled, they are hoisted off the line and sent to the finished product warehouse.

2. The process for an intensive ultra-high strength hot-rolled coil continuous heat treatment line according to claim 1, characterized in that: A waiting position for a vacuum suction cup is set at the exit of the shot blasting machine. Under normal circumstances, the steel strip passes through the No. 2 shearing machine without being cut. In an emergency, after the steel strip is straightened by the straightening machine, the No. 2 shearing machine cuts the steel strip to a fixed length. After being shot blasted by the shot blasting machine, the steel strip is stacked and removed from the production line by the vacuum suction cup.

3. The process method of the intensive ultra-high strength hot-rolled coil continuous heat treatment line as described in claim 1, characterized in that: The combustion system of the heating furnace includes burners, radiant tubes and control valves, metering devices and safety shut-off devices, and provides indirect heating through self-preheating burners installed inside the radiant tubes.

4. The process method of the intensive ultra-high strength hot-rolled coil continuous heat treatment line as described in claim 1, characterized in that: The outlet of the heating furnace and the first set of pinch rollers of the quenching machine are connected in a compact manner, with the distance between them kept within 1000mm.

5. The process method of the intensive ultra-high strength hot-rolled coil continuous heat treatment line as described in claim 1, characterized in that: The water supply pressure of each section of the cooling nozzle is 6 to 9 bar.

6. The process method of the intensive ultra-high strength hot-rolled coil continuous heat treatment line as described in claim 1, characterized in that: The angle between the jet stream of the flat nozzle group and the direction of steel belt movement is 10° to 60°. The angle between the jet stream of the slit nozzle group and the direction of steel belt movement is 5° to 30°. The slit size of the slit nozzle group on the upper surface of the steel belt is 1.5 to 3 mm, and the slit size of the slit nozzle group on the lower surface of the steel belt is 2.0 to 3.5 mm. The slit size of the slit nozzle group on the upper surface is 0.1 to 0.4 mm smaller than that of the slit nozzle group on the lower surface. The angle between the jet stream of the round hole nozzle group and the direction of steel belt movement is 20° to 80°.

7. The process method of the intensive ultra-high strength hot-rolled coil continuous heat treatment line as described in claim 1, characterized in that: Both the flat nozzle assembly and the slit nozzle assembly are divided into 3 to 5 sections along the width of the steel strip, with the middle section being 800 mm wide and the left and right side sections being 200 to 450 mm long.

8. The process method of the intensive ultra-high strength hot-rolled coil continuous heat treatment line as described in claim 1, characterized in that: The tail end of the quenching machine is equipped with a hot air dryer for blowing away moisture from the outer surface of the steel strip.

9. The process method of the intensive ultra-high strength hot-rolled coil continuous heat treatment line as described in claim 1, characterized in that: The second to fourth sets of pinch rollers of the quenching machine use grooved rollers with annular grooves on the surface. The first set of pinch rollers and other rollers use flat rollers.

Citation Information

Patent Citations

  • Quenching production line and production method

    CN117187503A