A chalcogenide quantum dot nanoporous glass and its preparation method

By combining sol-gel method and chemical vapor deposition with digital light processing 3D printing technology, the problems of difficult molding and poor stability of chalcogenide quantum dot glass devices have been solved, realizing the fabrication of high-precision complex-shaped chalcogenide quantum dot glass devices and improving the transparency and stability of the devices.

CN118125719BActive Publication Date: 2026-11-17SHANGHAI INST OF OPTICS & FINE MECHANICS CHINESE ACAD OF SCI
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410214328.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-27
Publication Date
2026-11-17
Estimated Expiration
2044-02-27

AI Technical Summary

Technical Problem

Existing technologies make it difficult to form chalcogenide quantum dot glass devices with high precision. Furthermore, chalcogenide quantum dots have poor stability, complex preparation processes, low transparency, and limited application range.

Method used

Chalcogenide quantum dot glass materials were prepared by a combination of sol-gel method and chemical vapor deposition. Quantum dots were then grown in situ within the pores of the mesoporous glass using digital light processing 3D printing. Fluorescent dyes were used to absorb ultraviolet light to reduce over-curing and achieve high-precision printing.

Benefits of technology

The fabrication of high-precision, complex-shaped chalcogenide quantum dot glass devices has been achieved, improving the stability and transparency of chalcogenide quantum dots and expanding their application scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118125719B_ABST
    Figure CN118125719B_ABST
Patent Text Reader

Abstract

This invention discloses a method for in-situ growth of PbS / CdS quantum dots in photopolymerized 3D printed microporous glass and its application, wherein the microporous glass is composed of (Al2O3). x -(SiO2) y -(PbS / CdS) z Where x = 2 - 10, x + y = 100, z = 0.2 - 1; a silica sol suitable for photopolymerization 3D printing was developed, which printed a silica hydrogel. After drying and sintering, a silica glass with a microporous structure was obtained. Chalcogenide quantum dots were then grown in situ inside the micropores using chemical vapor deposition to obtain chalcogenide quantum dot photofunctionalized microporous glass devices. This preparation method solves the problems of poor stability and reusability of free chalcogenide quantum dots and high-precision molding of chalcogenide quantum dot photofunctional devices. It has the advantages of no mold required, free geometric design, easy composition design, economic applicability, and reusability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the fields of semiconductor nanomaterial preparation technology and additive manufacturing, specifically relating to additive manufacturing technology for chalcogenide quantum dot mesoporous glass based on sol-gel, photopolymerization 3D printing and chemical vapor deposition methods. Background Technology

[0002] Quantum dot materials, as an emerging nanoscale material, possess unique photoelectric and catalytic properties, and have broad application potential in display technology, biomedical imaging, and photocatalysis. Chalcogenide quantum dots, due to their high quantum yield and narrow fluorescence emission peak, are considered to have broad application prospects in information and optical communication. Common methods for preparing chalcogenide quantum dots include thermal injection, hydrothermal methods, and microemulsion methods, typically producing colloidal quantum dots. However, their stability is greatly affected by external environmental conditions such as oxidation and hydrolysis. This invention utilizes chemical vapor deposition to achieve stable and rapid growth of chalcogenide quantum dots.

[0003] Mesoporous glass is a type of glass with an average pore size ranging from 2 to 50 nm. Due to its high specific surface area and regularly ordered pore structure, it has wide applications in sensing and information, catalysis, adsorption separation, and biomedicine. The stable pore structure within mesoporous glass provides confinement and a stable external environment for the growth of quantum dots. It also prevents chalcogenide quantum dots from contacting oxygen in the air, slowing down oxidation and increasing their lifespan. The sol-gel method uses metal alkoxides to undergo hydrolysis and condensation reactions in a liquid phase to form a stable sol. This method offers advantages such as low preparation temperature and the ability to uniformly add raw materials at the molecular level. Using the sol-gel method to prepare mesoporous glass facilitates the adjustment of glass composition and manufacturing methods.

[0004] Digital light processing 3D printing (DLP), as a type of additive manufacturing, has advantages such as fast forming speed, high precision, and ease of fabricating complex-shaped components. By combining the sol-gel method with digital light processing 3D printing, it is possible to fabricate complex-shaped mesoporous glass, solving the problems of complex forming difficulties of quantum dot devices and the stability of quantum dots.

[0005] However, to date, there has been no research on photopolymerization 3D printing of mesoporous glass devices grown in situ from chalcogenide quantum dots. For example, CN111825333B discloses a method for 3D printing glass devices, but this method uses silica particles as the silicon source in the glass to prepare glass ink. The sintering process requires heating to 1260℃. The sintered glass has no mesoporous structure and has low transparency, limiting its application range in optical communication. CN116874182A discloses a method for 3D printing nanoporous glass ink and additive manufacturing of transparent nanoporous glass materials, but it does not show the confinement effect of nanopores on quantum dot growth. The ink prepared by this method is prone to over-curing during actual use, resulting in low printing accuracy. CN105693096B discloses a method for preparing a chalcogenide quantum dot and phosphate mesoporous glass composite, but the prepared quantum dot phosphate glass composite belongs to the phosphate glass system. There are no reports on 3D printing chalcogenide quantum dot glass devices based on aluminosilicate glass systems. The quantum dot glass prepared by this method needs to be processed into applicable glass devices, which is a complex process. Currently, there are still no reports on 3D printing chalcogenide quantum dot glass devices. Summary of the Invention

[0006] This invention provides a sol-gel method combined with chemical vapor deposition (CVD) to prepare chalcogenide quantum dot glass materials, and a method for growing chalcogenide quantum dots in glass materials prepared using digital light processing 3D printing. More specifically, it provides a photopolymerizable glass slurry suitable for preparing chalcogenide quantum dot light-emitting devices, and a method for in-situ growth of chalcogenide quantum dots in mesoporous glass devices with freely designed three-dimensional complex structures using CVD, aided by computer modeling software. The method provided by this invention solves the problems of difficulty in forming high-precision quantum dot glass devices and poor stability of colloidal chalcogenide quantum dots.

[0007] To achieve the objectives of the invention described above, the present invention provides the following technical solution:

[0008] This invention provides a chalcogenide quantum dot nanoporous glass, characterized in that the glass composition is (Al2O3). x -(SiO2) y -(PbS / CdS) z Where x = 2-10, x+y = 100, z = 0.2-1; the glass material is formed by digital light processing 3D printing, and is obtained by aging, drying and degreasing; the quantum dot growth principle is chemical vapor deposition.

[0009] This invention provides a method for preparing chalcogenide quantum dot nanoporous glass, comprising the following steps:

[0010] First, a glass paste is prepared, which is suitable for preparing chalcogenide quantum dot light-emitting glass devices and can be used for photopolymerization printing; the glass prepared by this paste has the general formula (Al2O3). x -(SiO2) y -(PbS / CdS) z Where x = 2-10, x+y = 100, z = 0.2-1, after selecting the values ​​of x / y / z, the raw materials are weighed according to the content ratio of Al, Pb, Cd, and Si elements in the general formula, and the glass sol that can be photocured and printed is prepared by stepwise stirring, which is the glass slurry; the raw materials include pore-forming agents, salts that make up quantum dots, deionized water, acid solutions, organosilicon compounds, photoinitiators, silane coupling agents, polycondensation catalysts, and fluorescent dye solutions;

[0011] Secondly, 3D printing is used to obtain photocurable wet gels, including software modeling, photocuring printing, washing the printed parts, and aging and curing the printed parts. The printing process involves using computer 3D modeling software to create a spatial structure model suitable for printing, slicing the model file and importing it into the printer, and using ultraviolet light to cure the glass ink layer by layer to obtain a photocurable wet gel with a special complex shape.

[0012] Next, the wet gel undergoes drying and heat treatment processes, including aging, graded drying, vacuum drying, and degreasing. The aging process is carried out in a sealed container, maintaining stable water and ethanol vapor pressure, and allowing the sample to stand for 24 to 48 hours. The graded drying process is carried out in a sealed container, which is then transferred to an oven. Based on the different solvent contents in different gel components, a multi-stage drying temperature ranging from 30°C to 100°C is set, and the sample is kept at each temperature for 24 hours. During vacuum drying, the sample is placed in an open container and then placed in a vacuum drying oven, where it is vacuum dried at 100°C for 12 hours. The degreasing and sintering process is carried out in a muffle furnace. Based on the different organic matter content in the dry gel, a heating rate ranging from 0.1°C / min to 1.5°C / min is set. The sample is heated from room temperature to 300°C to 400°C and held at this temperature for 2 to 12 hours. Then, the temperature is raised to 650°C to 800°C and held for 2 to 12 hours. After heating is stopped, the sample is cooled to room temperature with the furnace and then removed to obtain 3D printed glass with complex shapes and mesoporous structures.

[0013] Finally, quantum dots are grown in situ within the pores of the mesoporous glass, including vacuuming, introducing hydrogen sulfide gas, growing chalcogenide quantum dots via chemical vapor deposition, and rinsing with inert gas. During the vacuuming process, the mesoporous glass is placed in a tube furnace, and a mechanical pump is used to remove air from the furnace. Once the vacuum stabilizes, a molecular pump is used, and the air extraction is stopped after the vacuum stabilizes. During the introduction of hydrogen sulfide gas, a gas pressure reducing valve is used to slowly introduce hydrogen sulfide gas to atmospheric pressure. During the chemical vapor deposition process for growing chalcogenide quantum dots, the ambient temperature is controlled within the range of 25°C to 100°C, depending on the material, and the mixture is left to stand for 12 to 48 hours to achieve confined growth of chalcogenide quantum dots. The inert gas rinsing process involves slowly introducing helium gas into the tube furnace using a gas pressure reducing valve, rinsing for 30 to 60 minutes, and then removing the sample to obtain a 3D-printed complex structure mesoporous glass device with in-situ grown chalcogenide quantum dots.

[0014] Compared with the prior art, the present invention has achieved the following beneficial results:

[0015] This invention utilizes the sol-gel method to prepare photocurable 3D printing glass ink. While sol-gel method-prepared glass inks are colorless and transparent, they are prone to over-curing during DLP printing, reducing printing accuracy. This invention, for the first time, absorbs scattered ultraviolet light during printing by adding a fluorescent dye, significantly reducing over-curing and greatly improving printing accuracy.

[0016] This invention utilizes the sol-gel method to synthesize sulfur quantum dots, specifically CdS / PbS quantum dots. The required Cd and Pb elements are introduced into the system in the form of hydrated metal salts. Compared to commonly used methods for preparing sulfide quantum dots, such as hot injection and water precipitation, introducing the necessary metal elements into the silica sol preparation process and combining it with chemical vapor deposition for quantum dot growth makes it easier to adjust the metal salt content and avoids metal waste. During the addition of Cd / Pb elements to the sol, the hydrolysis and condensation of tetraethyl orthosilicate easily lead to the precipitation of complexes. This invention, for the first time, solves the problem of the difficulty in adding Cd / Pb ions into the silica sol-gel system by adjusting the pH of the sol and adding an alkaline catalyst.

[0017] This invention utilizes chemical vapor deposition to grow quantum dots in situ within the pores of mesoporous glass at a reaction temperature of 25-60℃. Compared to common methods for preparing sulfide quantum dots, such as hot injection and hydrothermal precipitation, this method is more environmentally friendly and energy-efficient. Due to the use of a gaseous sulfur source (hydrogen sulfide gas), the quantum dot growth is more uniform, and the impact on the transmittance of glass devices is significantly reduced.

[0018] This invention utilizes 3D printing combined with quantum dot materials to achieve integrated fabrication of complex-shaped chalcogenide quantum dot glass devices. The fabrication success rate is high, no molds are required, and free geometric space can be formed, thus expanding the application scenarios of chalcogenide quantum dot glass devices. Attached Figure Description

[0019] Figure 1 This is a schematic diagram of the digital light processing 3D printing process;

[0020] Figure 2 This is a schematic diagram of the PbS quantum dot growth process. Detailed Implementation

[0021] To provide a more concise description, some of the quantitative expressions given herein are not modified by the term "approximately". It should be understood that, whether or not the term "approximately" is explicitly used, each quantity given herein is intended to refer to an actual given value, and also to an approximation of such given values ​​that can be reasonably inferred by one of ordinary skill in the art, including approximations of such given values ​​caused by experimental and / or measurement conditions.

[0022] The main steps of the 3D printing preparation method for in-situ growth of chalcogenide quantum dots in mesoporous glass in this invention include:

[0023] 1. Dissolve the pore-forming agent and the salts that make up the quantum dots in water to obtain an aqueous solution, and adjust the pH value using an acid solution;

[0024] 2. Dissolve the organosilicon compound in an alcohol solvent to obtain an alcohol solution, then add it to an aqueous solution and stir until the organosilicon compound is completely hydrolyzed and transparent to obtain a silica sol;

[0025] 3. Dissolve the photoinitiator in the silane coupling agent to obtain a photosensitive solution. Add the photosensitive solution dropwise to the silica sol obtained in the previous step, add the polycondensation catalyst, add the fluorescent dye solution, and stir to obtain a silica sol that can be cured by ultraviolet light.

[0026] 4. Use 3D modeling software to create a 3D model, slice the model file, and then import it into the printer;

[0027] 5. Place the UV-curable silica sol obtained in step 3 into the material box, set the printing parameters, and print layer by layer to obtain a wet gel with a complex shape.

[0028] 6. After curing the wet gel with a UV lamp, slowly remove it, place it in a sealed bag for aging, and then dry it in stages and under vacuum to obtain a dry gel. After degreasing and removing organic matter in a muffle furnace, the dry gel yields a transparent glass with a mesoporous structure.

[0029] 7. Hydrogen sulfide gas is introduced into the mesoporous glass in a tube furnace, and after standing for a period of time, 3D printed mesoporous glass devices with in-situ grown chalcogenide quantum dots are obtained.

[0030] The present invention will be further illustrated below with reference to specific embodiments. It is important to note that these embodiments are for illustrative purposes only and should not be construed as limiting the scope of protection of the invention. Those skilled in the art can make non-essential improvements and adjustments based on the above description of the invention. Test methods in the following embodiments that do not specify specific conditions are generally performed under conventional conditions or as recommended by the manufacturer. Unless otherwise stated, all percentages and parts are by weight.

[0031] The sources, names, and specifications of the experimental materials or instruments used in the embodiments of this invention are shown in the table below:

[0032]

[0033] Table 1: Experimental materials and instruments used in this invention. Data from each test case in the embodiments of this invention are shown in the following table:

[0034]

[0035]

[0036] Table 2: Data list of each test case in Examples 1-6

[0037] Example 1:

[0038] S1. Ink preparation: according to stoichiometric ratio (Al2O3) x -(SiO2) y -(CdS) z Where x = 2, y = 98, z = 0.2, and aluminum lactate (C9H) with an equal molar ratio of aluminum is accurately weighed. 150.2354 g of AlO9 and 0.0426 g of cadmium acetate dihydrate (C4H6CdO4·2H2O) were dissolved in 2 ml of deionized water to obtain an aqueous solution. 6 mol / L dilute nitric acid was prepared, and the pH of the aqueous solution was adjusted to 4 using the dilute nitric acid. Then, 8.1665 g of tetraethyl orthosilicate was weighed and dissolved in 6 ml of ethanol to obtain an alcoholic solution. The solution was added to water and stirred at 500 r / min until clear to obtain silica sol. Weigh out 0.07g of photoinitiator propyl 3-(trimethoxysilyl)acrylate and 1.5g of silane coupling agent propyl 3-(trimethoxysilyl)acrylate. Dissolve the photoinitiator in the silane coupling agent to obtain a photosensitive solution. Add the photosensitive solution dropwise to the silica sol, then add 1.5ml of 1mol / L ammonium acetate (C2H7NO2) solution. Stir at 500r / min for 15 minutes to obtain a UV-curable silica sol, which is the photocurable glass ink for printing. Prepare a 1mg / ml solution of 6g rhodamine in ethanol as a fluorescent dye solution, and add 1ml of the fluorescent dye solution to the ink.

[0039] S2. Preparation of mesoporous glass: A 3D model is created using 3D modeling software. After the model file is sliced, it is imported into the MAX X27 UV printer manufactured by Asiga. Ink is placed into the cartridge, and the printer emits ultraviolet light of the sliced ​​pattern to the bottom of the transparent cartridge. The sol is cured onto the printing platform. As the printing platform rises, the layers are printed and stacked to obtain a three-dimensional wet gel.

[0040] To age the wet gel, place it in a sealed container at room temperature, keeping the vapor pressure of water and ethanol stable, and let it stand for 3 days.

[0041] During the gradient drying process, the aged wet gel is placed in a flat container such as a petri dish or filter paper, and the container is placed in an oven. The temperature is increased in increments of 10°C within the range of 30 to 100°C, and the temperature is maintained for 16 hours for each 10°C increase to obtain the dry gel.

[0042] In the degreasing process, the dry gel was placed on the corundum crucible lid and placed in a muffle furnace. The temperature was increased to 300°C at a heating rate of 0.1°C / min and held for 2 hours. Subsequently, in the sintering process, the temperature was increased to 700°C at a heating rate of 0.5°C / min and held for 2 hours. The mixture was then cooled to room temperature in the furnace to obtain a microporous glass structure.

[0043] Growth of S3.CdS quantum dots: A mesoporous glass was placed in a crucible, which was then placed in a tube furnace. Air was removed using a mechanical pump to achieve a vacuum level of 1*10⁻⁶. -3 After passing through H2S gas at kPa, the glass was allowed to stand at 25℃ for 12 hours to obtain a mesoporous glass with CdS quantum dots grown in situ within a mesoporous structure.

[0044] Test Example 1: Ink Transparency

[0045] Test sample: Ink prepared in Example 1

[0046] Test equipment: UV-Vis spectrophotometer (Cary 60, Agilent, USA)

[0047] Test range: 300-850nm;

[0048] The ink prepared in Example 1 had a light transmittance of 86.6% within the test range.

[0049] Test Example 2: Viscosity Test

[0050] Test sample: Ink prepared in Example 1

[0051] Test equipment: Rotational rheometer (MCR 502e, Anton Paar, Austria)

[0052] Test conditions: 25℃, shear rate measurement range: 1-1500s -1 .

[0053] The viscosity of the ink prepared in Example 1 is 3.5 cP / 10s.

[0054] Test Example 3: Thermogravimetric-Differential Thermal Testing

[0055] Test sample: Dry gel prepared in Example 1

[0056] Testing equipment: TG / DTA analyzer (EXSTAR 7300, SII, Japan)

[0057] Test conditions: Measurement temperature range: 50-1100℃, heating rate: 5℃ / min.

[0058] The dry gel prepared in Example 1 showed a weight loss peak at around 340°C, and the inorganic content was 85.5 wt%.

[0059] Test Example 4: Pore Size Analysis of Mesoporous Glass

[0060] Test sample: Mesoporous glass prepared in Example 1

[0061] Test equipment: Surface area and pore size analyzer (Micromeritics ASAP 2460, Shanghai); Adsorbed gas: nitrogen; Degassing temperature: 200℃; Degassing time: 8h.

[0062] The glass prepared in Example 1 exhibits a typical adsorption-desorption curve pattern for mesoporous materials, with a specific surface area of ​​430 m². 2 / g, with an average pore size of 5.5nm.

[0063] Test Example 5: Glass Composition Test

[0064] Test sample: Mesoporous glass prepared in Example 1

[0065] Test equipment: Transmission electron microscope (HEOL-2010, USA); Energy dispersive X-ray spectroscopy (EDS) detector (Oxford Instruments, UK).

[0066] The mesoporous glass prepared in Example 1 has an Al2O3-SiO2 composition and uniform elemental distribution.

[0067] Test Example 6: Fluorescence Spectroscopy of Quantum Dots

[0068] Test sample: In-situ grown CdS quantum dot mesoporous glass prepared in Example 1

[0069] Test equipment: Steady-state / transient fluorescence spectrometer (Edinburgh, FLS 980, UK)

[0070] Test conditions: excitation light source wavelength: 350nm; test range: 400-800nm; sampling interval: 1nm; repeated sampling: 5 times.

[0071] The in-situ grown CdS quantum dot mesoporous glass prepared in Example 1 showed a broad fluorescence emission peak at 457 nm, proving the formation of CdS quantum dots.

[0072] Example 2:

[0073] S1. Ink preparation: according to stoichiometric ratio (Al2O3) x -(SiO2) y -(CdS) z Where x = 5, y = 95, z = 0.5, and equal amounts of aluminum lactate (C9H2O) are accurately weighed. 150.5884 g of AlO9 and 0.0533 g of cadmium acetate dihydrate (C4H6CdO4·2H2O) were dissolved in 4 ml of deionized water to obtain an aqueous solution. A 6 mol / L dilute nitric acid solution was prepared, and the pH of the aqueous solution was adjusted to 3 using the dilute nitric acid. Then, 7.9165 g of tetraethyl orthosilicate was weighed and dissolved in 6 ml of isopropanol to obtain an alcoholic solution. The solution was added to water and stirred at 500 r / min until clear to obtain a silica sol. Weigh out 0.07 g of photoinitiator ethyl 2,4,6-trimethylbenzoylphenylphosphonate and 1.5 g of silane coupling agent (3-glycidylpropoxy)trimethoxysilane. Dissolve the photoinitiator in the silane coupling agent to obtain a photosensitive solution. Add the photosensitive solution dropwise to the silica sol, then add 1.5 ml of 1 mol / L ammonium acetate (C2H7NO2) solution. Stir at 500 rpm for 15 minutes to obtain a UV-curable silica sol, which is the photocurable glass ink for printing. Prepare a 1 mg / ml Rhodamine B ethanol solution as a fluorescent dye solution, and add 1 ml of the fluorescent dye solution to the ink.

[0074] S2. Preparation of mesoporous glass: A 3D model is created using 3D modeling software. After the model file is sliced, it is imported into the MAX X27 UV printer manufactured by Asiga. Ink is placed into the cartridge, and the printer emits ultraviolet light of the sliced ​​pattern to the bottom of the transparent cartridge. The sol is cured onto the printing platform. As the printing platform rises, the layers are printed and stacked to obtain a three-dimensional wet gel.

[0075] The wet gel was aged by placing it in a sealed container at room temperature, keeping the vapor pressure of water and ethanol stable, and letting it stand for 4 days.

[0076] During the gradient drying process, the aged wet gel is placed in a flat container such as a petri dish or filter paper, and the container is placed in an oven. The temperature is increased in increments of 10°C within the range of 30 to 100°C, and the temperature is maintained for 20 hours for each 10°C increase to obtain the dry gel.

[0077] In the degreasing process, the dry gel was placed on a corundum crucible lid and placed in a muffle furnace. The temperature was increased to 300°C at a heating rate of 0.3°C / min and held for 16 hours. Subsequently, in the sintering process, the temperature was increased to 700°C at a heating rate of 0.5°C / min and held for 16 hours. The mixture was then cooled to room temperature in the furnace to obtain a microporous glass structure.

[0078] Growth of S3.CdS quantum dots: A mesoporous glass was placed in a crucible, which was then placed in a tube furnace. Air was removed using a mechanical pump to achieve a vacuum level of 1*10⁻⁶. -3 After passing through H2S gas at kPa, the glass was allowed to stand at 60℃ for 12 hours to obtain a mesoporous glass with CdS quantum dots grown in situ within a mesoporous structure.

[0079] Test Example 7: Ink Transparency

[0080] Test sample: Ink prepared in Example 2

[0081] Test equipment: UV-Vis spectrophotometer (Cary 60, Agilent, USA)

[0082] Test range: 300-850nm;

[0083] The ink prepared in Example 2 had a light transmittance of 85.1% within the test range.

[0084] Test Example 8: Viscosity Test

[0085] Test sample: Ink prepared in Example 2

[0086] Test equipment: Rotational rheometer (MCR 502e, Anton Paar, Austria)

[0087] Test conditions: 25℃, shear rate measurement range: 1-1500s -1 .

[0088] The viscosity of the ink prepared in Example 2 is 3.7 cP / 10s.

[0089] Test Example 9: Thermogravimetric-Differential Thermal Testing

[0090] Test sample: Dry gel prepared in Example 2

[0091] Testing equipment: TG / DTA analyzer (EXSTAR 7300, SII, Japan)

[0092] Test conditions: Measurement temperature range: 50-1100℃, heating rate: 5℃ / min.

[0093] The dry gel prepared in Example 2 showed a weight loss peak at around 340°C, and the inorganic content was 83.2 wt%.

[0094] Test Example 10: Pore Size Analysis of Mesoporous Glass

[0095] Test sample: Mesoporous glass prepared in Example 2

[0096] Test equipment: Surface area and pore size analyzer (Micromeritics ASAP 2460, Shanghai); Adsorbed gas: nitrogen; Degassing temperature: 200℃; Degassing time: 8h.

[0097] The glass prepared in Example 2 exhibits a typical adsorption-desorption curve pattern for mesoporous materials, with a specific surface area of ​​493 m². 2 / g, with an average pore size of 7.7nm.

[0098] Test Example 11: Glass Composition Test

[0099] Test sample: Mesoporous glass prepared in Example 2

[0100] Test equipment: Transmission electron microscope (HEOL-2010, USA); Energy dispersive X-ray spectroscopy (EDS) detector (Oxford Instruments, UK).

[0101] The mesoporous glass prepared in Example 2 has an Al2O3-SiO2 composition and uniform elemental distribution.

[0102] Test Example 12: Fluorescence Spectroscopy of Quantum Dots

[0103] Test sample: In-situ grown CdS quantum dot mesoporous glass prepared in Example 2

[0104] Test equipment: Steady-state / transient fluorescence spectrometer (Edinburgh, FLS 980, UK)

[0105] Test conditions: excitation light source wavelength: 350nm; test range: 400-800nm; sampling interval: 1nm; repeated sampling: 5 times.

[0106] The in-situ grown CdS quantum dot mesoporous glass prepared in Example 2 showed a broad fluorescence emission peak at 461 nm, proving the formation of CdS quantum dots.

[0107] Example 3:

[0108] S1. Ink preparation: according to stoichiometric ratio (Al2O3) x -(SiO2) y -(CdS) z Where x = 10, y = 90, z = 0.5, equal amounts of aluminum lactate (C9H) are accurately weighed. 151.1768 g of AlO9 and 0.0533 g of cadmium acetate dihydrate (C4H6CdO4·2H2O) were dissolved in 8 ml of deionized water to obtain an aqueous solution. A 6 mol / L dilute nitric acid solution was prepared, and the pH of the aqueous solution was adjusted to 1 using the dilute nitric acid. Then, 7.4999 g of tetraethyl orthosilicate was weighed and dissolved in 6 ml of methanol to obtain an alcoholic solution. The solution was added to water and stirred at 500 r / min until clear to obtain a silica sol. Weigh out 0.07 g of photoinitiator diacylphosphine oxide 819 and 1.5 g of silane coupling agent 3-aminopropyltrimethoxysilane. Dissolve the photoinitiator in the silane coupling agent to obtain a photosensitive solution. Add the photosensitive solution dropwise to the silica sol, then add 1.5 ml of 1 mol / L formamide (CH3NO) solution. Stir at 500 rpm for 15 minutes to obtain a UV-curable silica sol, which is the photocurable glass ink for printing. Prepare a 1 mg / ml methyl orange aqueous solution as a fluorescent dye solution, and add 1 ml of the fluorescent dye solution to the ink.

[0109] S2. Preparation of mesoporous glass: A 3D model is created using 3D modeling software. After the model file is sliced, it is imported into the MAX X27 UV printer manufactured by Asiga. Ink is placed into the cartridge, and the printer emits ultraviolet light of the sliced ​​pattern to the bottom of the transparent cartridge. The sol is cured onto the printing platform. As the printing platform rises, the layers are printed and stacked to obtain a three-dimensional wet gel.

[0110] The wet gel was aged by placing it in a sealed container at room temperature, keeping the vapor pressure of water and ethanol stable, and letting it stand for 5 days.

[0111] During the gradient drying process, the aged wet gel is placed in a flat container such as a petri dish or filter paper, and the container is placed in an oven. The temperature is increased in increments of 10°C within the range of 30 to 100°C, and the temperature is maintained for 24 hours for each 10°C increase to obtain the dry gel.

[0112] In the degreasing process, the dry gel was placed on a corundum crucible lid and placed in a muffle furnace. The temperature was increased to 300°C at a rate of 0.5°C / min and held for 24 hours. Subsequently, in the sintering process, the temperature was increased to 700°C at a rate of 0.5°C / min and held for 24 hours. The mixture was then cooled to room temperature in the furnace to obtain a microporous glass structure.

[0113] Growth of S3.CdS quantum dots: A mesoporous glass was placed in a crucible, which was then placed in a tube furnace. Air was removed using a mechanical pump to achieve a vacuum level of 1*10⁻⁶. -3 After passing through H2S gas at kPa, the glass was allowed to stand at 100℃ for 12 hours to obtain a mesoporous glass with CdS quantum dots grown in situ within a mesoporous structure.

[0114] Test Example 13: Ink Transparency

[0115] Test sample: Ink prepared in Example 3

[0116] Test equipment: UV-Vis spectrophotometer (Cary 60, Agilent, USA)

[0117] Test range: 300-850nm;

[0118] The ink prepared in Example 3 had a light transmittance of 83.7% within the test range.

[0119] Test Example 14: Viscosity Test

[0120] Test sample: Ink prepared in Example 3

[0121] Test equipment: Rotational rheometer (MCR 502e, Anton Paar, Austria)

[0122] Test conditions: 25℃, shear rate measurement range: 1-1500s -1 .

[0123] The viscosity of the ink prepared in Example 3 is 4.1 cP / 10s.

[0124] Test Example 15: Thermogravimetric-Differential Thermal Testing

[0125] Test sample: Dry gel prepared in Example 3

[0126] Testing equipment: TG / DTA analyzer (EXSTAR 7300, SII, Japan)

[0127] Test conditions: Measurement temperature range: 50-1100℃, heating rate: 5℃ / min.

[0128] The dry gel prepared in Example 3 showed a weight loss peak at around 340°C, with an inorganic content of 81.9 wt%.

[0129] Test Example 16: Pore Size Analysis of Mesoporous Glass

[0130] Test sample: Mesoporous glass prepared in Example 3

[0131] Test equipment: Surface area and pore size analyzer (Micromeritics ASAP 2460, Shanghai); Adsorbed gas: nitrogen; Degassing temperature: 200℃; Degassing time: 8h.

[0132] The glass prepared in Example 3 exhibits a typical adsorption-desorption curve pattern for mesoporous materials, with a specific surface area of ​​510 m². 2 / g, with an average pore size of 9.7nm.

[0133] Test Example 17: Glass Composition Test

[0134] Test sample: Mesoporous glass prepared in Example 3

[0135] Test equipment: Transmission electron microscope (HEOL-2010, USA); Energy dispersive X-ray spectroscopy (EDS) detector (Oxford Instruments, UK).

[0136] The mesoporous glass prepared in Example 3 has an Al2O3-SiO2 composition and a uniform elemental distribution.

[0137] Test Example 18: Fluorescence Spectroscopy of Quantum Dots

[0138] Test sample: In-situ grown CdS quantum dot mesoporous glass prepared in Example 3

[0139] Test equipment: Steady-state / transient fluorescence spectrometer (Edinburgh, FLS 980, UK)

[0140] Test conditions: excitation light source wavelength: 350nm; test range: 400-800nm; sampling interval: 1nm; repeated sampling: 5 times.

[0141] The in-situ grown CdS quantum dot mesoporous glass prepared in Example 3 showed a broad fluorescence emission peak at 469 nm, proving the formation of CdS quantum dots.

[0142] Example 4:

[0143] S1. Ink preparation: according to stoichiometric ratio (Al2O3) x -(SiO2) y -(PbS) z Where x = 2, y = 98, z = 1, and equal amounts of aluminum element in aluminum lactate (C9H) are accurately weighed. 150.2354 g of AlO9 and 0.1517 g of lead acetate trihydrate (PbC4H6O4·3H2O) containing an equal amount of lead were dissolved in 2 ml of deionized water to obtain an aqueous solution. A 6 mol / L dilute hydrochloric acid solution was prepared, and the pH of the aqueous solution was adjusted to 4 using the dilute hydrochloric acid. Then, 8.1665 g of tetraethyl orthosilicate was weighed and dissolved in 6 ml of ethanol to obtain an alcoholic solution. The solution was then added to water and stirred at 500 r / min until clear to obtain a silica sol. Weigh out 0.07g of photoinitiator propyl 3-(trimethoxysilyl)acrylate and 1.5g of silane coupling agent propyl 3-(trimethoxysilyl)acrylate. Dissolve the photoinitiator in the silane coupling agent to obtain a photosensitive solution. Add the photosensitive solution dropwise to the silica sol, then add 1.5ml of 1mol / L ammonium acetate (C2H7NO2) solution. Stir at 500r / min for 15 minutes to obtain a UV-curable silica sol, which is the photocurable glass ink for printing. Prepare a 1mg / ml solution of 6g rhodamine in ethanol as a fluorescent dye solution, and add 1ml of the fluorescent dye solution to the ink.

[0144] S2. Preparation of mesoporous glass: A 3D model is created using 3D modeling software. After the model file is sliced, it is imported into the MAX X27 UV printer manufactured by Asiga. Ink is placed into the cartridge, and the printer emits ultraviolet light of the sliced ​​pattern to the bottom of the transparent cartridge. The sol is cured onto the printing platform. As the printing platform rises, the layers are printed and stacked to obtain a three-dimensional wet gel.

[0145] To age the wet gel, place it in a sealed container at room temperature, keeping the vapor pressure of water and ethanol stable, and let it stand for 3 days.

[0146] During the gradient drying process, the aged wet gel is placed in a flat container such as a petri dish or filter paper, and the container is placed in an oven. The temperature is increased in increments of 10°C within the range of 30 to 100°C, and the temperature is maintained for 16 hours for each 10°C increase to obtain the dry gel.

[0147] In the degreasing process, the dry gel was placed on the corundum crucible lid and placed in a muffle furnace. The temperature was increased to 300°C at a heating rate of 0.1°C / min and held for 2 hours. Subsequently, in the sintering process, the temperature was increased to 700°C at a heating rate of 0.5°C / min and held for 2 hours. The mixture was then cooled to room temperature in the furnace to obtain a microporous glass structure.

[0148] Growth of S3.CdS quantum dots: A mesoporous glass was placed in a crucible, which was then placed in a tube furnace. Air was removed using a mechanical pump to achieve a vacuum level of 1*10⁻⁶. -3 After passing through H2S gas at kPa, the glass was allowed to stand at 25℃ for 48 hours to obtain a mesoporous glass with PbS quantum dots grown in situ within a mesoporous structure.

[0149] Test Example 19: Ink Transparency

[0150] Test sample: Ink prepared in Example 4

[0151] Test equipment: UV-Vis spectrophotometer (Cary 60, Agilent, USA)

[0152] Test range: 300-850nm;

[0153] The ink prepared in Example 4 had a light transmittance of 91.2% within the test range.

[0154] Test Example 20: Viscosity Test

[0155] Test sample: Ink prepared in Example 4

[0156] Test equipment: Rotational rheometer (MCR 502e, Anton Paar, Austria)

[0157] Test conditions: 25℃, shear rate measurement range: 1-1500s -1 .

[0158] The viscosity of the ink prepared in Example 4 is 3.5 cP / 10s.

[0159] Test Example 21: Thermogravimetric-Differential Thermal Testing

[0160] Test sample: Dry gel prepared in Example 4

[0161] Testing equipment: TG / DTA analyzer (EXSTAR 7300, SII, Japan)

[0162] Test conditions: Measurement temperature range: 50-1100℃, heating rate: 5℃ / min.

[0163] The dry gel prepared in Example 4 showed a weight loss peak at around 340°C, with an inorganic content of 85.6 wt%.

[0164] Test Example 22: Pore Size Analysis of Mesoporous Glass

[0165] Test sample: Mesoporous glass prepared in Example 4

[0166] Test equipment: Surface area and pore size analyzer (Micromeritics ASAP 2460, Shanghai); Adsorbed gas: nitrogen; Degassing temperature: 200℃; Degassing time: 8h.

[0167] The glass prepared in Example 4 exhibits a typical adsorption-desorption curve pattern for mesoporous materials, with a specific surface area of ​​433 m². 2 / g, with an average pore size of 5.1nm.

[0168] Test Example 23: Glass Composition Test

[0169] Test sample: Mesoporous glass prepared in Example 4

[0170] Test equipment: Transmission electron microscope (HEOL-2010, USA); Energy dispersive X-ray spectroscopy (EDS) detector (Oxford Instruments, UK).

[0171] The mesoporous glass prepared in Example 4 has an Al2O3-SiO2 composition and a uniform elemental distribution.

[0172] Test Example 24: Fluorescence Spectroscopy of Quantum Dots

[0173] Test sample: In-situ grown PbS quantum dot mesoporous glass prepared in Example 4

[0174] Test equipment: Steady-state / transient fluorescence spectrometer (Edinburgh, FLS 980, UK)

[0175] Test conditions: excitation light source wavelength: 900nm; test range: 950-1600nm; sampling interval: 1nm; repeated sampling: 5 times.

[0176] The in-situ grown PbS quantum dot mesoporous glass prepared in Example 4 showed a broad fluorescence emission peak at 1121 nm, proving the formation of PbS quantum dots.

[0177] Example 5:

[0178] S1. Ink preparation: according to stoichiometric ratio (Al2O3) x -(SiO2) y -(PbS) z Where x = 5, y = 95, z = 1, and equal amounts of aluminum lactate (C9H) are accurately weighed. 150.5884 g of AlO9 and 0.1517 g of lead acetate trihydrate (PbC4H6O4·3H2O) containing an equal amount of lead were dissolved in 4 ml of deionized water to obtain an aqueous solution. A 6 mol / L dilute hydrochloric acid solution was prepared, and the pH of the aqueous solution was adjusted to 3 using dilute nitric acid. Then, 7.9165 g of tetraethyl orthosilicate was weighed and dissolved in 6 ml of isopropanol to obtain an alcoholic solution. The solution was then added to water and stirred at 500 r / min until clear to obtain a silica sol. Weigh out 0.07 g of photoinitiator ethyl 2,4,6-trimethylbenzoylphenylphosphonate and 1.5 g of silane coupling agent (3-glycidylpropoxy)trimethoxysilane. Dissolve the photoinitiator in the silane coupling agent to obtain a photosensitive solution. Add the photosensitive solution dropwise to the silica sol, then add 1.5 ml of 1 mol / L ammonium acetate (C2H7NO2) solution. Stir at 500 rpm for 15 minutes to obtain a UV-curable silica sol, which is the photocurable glass ink for printing. Prepare a 1 mg / ml Rhodamine B ethanol solution as a fluorescent dye solution, and add 1 ml of the fluorescent dye solution to the ink.

[0179] S2. Preparation of mesoporous glass: A 3D model is created using 3D modeling software. After the model file is sliced, it is imported into the MAX X27 UV printer manufactured by Asiga. Ink is placed into the cartridge, and the printer emits ultraviolet light of the sliced ​​pattern to the bottom of the transparent cartridge. The sol is cured onto the printing platform. As the printing platform rises, the layers are printed and stacked to obtain a three-dimensional wet gel.

[0180] The wet gel was aged by placing it in a sealed container at room temperature, keeping the vapor pressure of water and ethanol stable, and letting it stand for 4 days.

[0181] During the gradient drying process, the aged wet gel is placed in a flat container such as a petri dish or filter paper, and the container is placed in an oven. The temperature is increased in increments of 10°C within the range of 30 to 100°C, and the temperature is maintained for 20 hours for each 10°C increase to obtain the dry gel.

[0182] In the degreasing process, the dry gel was placed on a corundum crucible lid and placed in a muffle furnace. The temperature was increased to 300°C at a heating rate of 0.3°C / min and held for 16 hours. Subsequently, in the sintering process, the temperature was increased to 700°C at a heating rate of 0.5°C / min and held for 16 hours. The mixture was then cooled to room temperature in the furnace to obtain a microporous glass structure.

[0183] Growth of S3.CdS quantum dots: A mesoporous glass was placed in a crucible, which was then placed in a tube furnace. Air was removed using a mechanical pump to achieve a vacuum level of 1*10⁻⁶. -3 After passing through H2S gas at kPa, the glass was allowed to stand at 60℃ for 48 hours to obtain a mesoporous glass with PbS quantum dots grown in situ within a mesoporous structure.

[0184] Test Example 25: Ink Transparency

[0185] Test sample: Ink prepared in Example 5

[0186] Test equipment: UV-Vis spectrophotometer (Cary 60, Agilent, USA)

[0187] Test range: 300-850nm;

[0188] The ink prepared in Example 5 had a light transmittance of 86.7% within the test range.

[0189] Test Example 26: Viscosity Test

[0190] Test sample: Ink prepared in Example 5

[0191] Test equipment: Rotational rheometer (MCR 502e, Anton Paar, Austria)

[0192] Test conditions: 25℃, shear rate measurement range: 1-1500s -1 .

[0193] The viscosity of the ink prepared in Example 5 is 3.8 cP / 10s.

[0194] Test Example 27: Thermogravimetric-Differential Thermal Testing

[0195] Test sample: Dry gel prepared in Example 5

[0196] Testing equipment: TG / DTA analyzer (EXSTAR 7300, SII, Japan)

[0197] Test conditions: Measurement temperature range: 50-1100℃, heating rate: 5℃ / min.

[0198] The dry gel prepared in Example 5 showed a weight loss peak at around 340°C, with an inorganic content of 83.9 wt%.

[0199] Test Example 28: Pore Size Analysis of Mesoporous Glass

[0200] Test sample: Mesoporous glass prepared in Example 5

[0201] Test equipment: Surface area and pore size analyzer (Micromeritics ASAP 2460, Shanghai); Adsorbed gas: nitrogen; Degassing temperature: 200℃; Degassing time: 8h.

[0202] The glass prepared in Example 5 exhibits a typical adsorption-desorption curve pattern for mesoporous materials, with a specific surface area of ​​499 m². 2 / g, with an average pore size of 7.9nm.

[0203] Test Example 29: Glass Composition Test

[0204] Test sample: Mesoporous glass prepared in Example 5

[0205] Test equipment: Transmission electron microscope (HEOL-2010, USA); Energy dispersive X-ray spectroscopy (EDS) detector (Oxford Instruments, UK).

[0206] The mesoporous glass prepared in Example 5 has an Al2O3-SiO2 composition and a uniform elemental distribution.

[0207] Test Example 30: Fluorescence Spectroscopy of Quantum Dots

[0208] Test sample: In-situ grown PbS quantum dot mesoporous glass prepared in Example 5

[0209] Test equipment: Steady-state / transient fluorescence spectrometer (Edinburgh, FLS 980, UK)

[0210] Test conditions: excitation light source wavelength: 900nm; test range: 950-1600nm; sampling interval: 1nm; repeated sampling: 5 times.

[0211] The in-situ grown PbS quantum dot mesoporous glass prepared in Example 4 showed a broad fluorescence emission peak at 1125 nm, proving the formation of PbS quantum dots.

[0212] Example 6:

[0213] S1. Ink preparation: according to stoichiometric ratio (Al2O3) x -(SiO2) y -(PbS) z Where x = 10, y = 90, z = 1, equal amounts of aluminum lactate (C9H) are accurately weighed. 151.1768 g of AlO9 and 0.1517 g of lead acetate trihydrate (PbC4H6O4·3H2O) containing an equal amount of lead were dissolved in 8 ml of deionized water to obtain an aqueous solution. A 6 mol / L dilute hydrochloric acid solution was prepared, and the pH of the aqueous solution was adjusted to 1 using the dilute hydrochloric acid. Then, 7.4999 g of tetraethyl orthosilicate was weighed and dissolved in 6 ml of methanol to obtain an alcoholic solution. The solution was added to water and stirred at 500 r / min until clear to obtain a silica sol. Weigh out 0.07 g of photoinitiator diacylphosphine oxide 819 and 1.5 g of silane coupling agent 3-aminopropyltrimethoxysilane. Dissolve the photoinitiator in the silane coupling agent to obtain a photosensitive solution. Add the photosensitive solution dropwise to the silica sol, then add 1.5 ml of 1 mol / L formamide (CH3NO) solution. Stir at 500 rpm for 15 minutes to obtain a UV-curable silica sol, which is the photocurable glass ink for printing. Prepare a 1 mg / ml methyl orange aqueous solution as a fluorescent dye solution, and add 1 ml of the fluorescent dye solution to the ink.

[0214] S2. Preparation of mesoporous glass: A 3D model is created using 3D modeling software. After the model file is sliced, it is imported into the MAX X27 UV printer manufactured by Asiga. Ink is placed into the cartridge, and the printer emits ultraviolet light of the sliced ​​pattern to the bottom of the transparent cartridge. The sol is cured onto the printing platform. As the printing platform rises, the layers are printed and stacked to obtain a three-dimensional wet gel.

[0215] The wet gel was aged by placing it in a sealed container at room temperature, keeping the vapor pressure of water and ethanol stable, and letting it stand for 5 days.

[0216] During the gradient drying process, the aged wet gel is placed in a flat container such as a petri dish or filter paper, and the container is placed in an oven. The temperature is increased in increments of 10°C within the range of 30 to 100°C, and the temperature is maintained for 24 hours for each 10°C increase to obtain the dry gel.

[0217] In the degreasing process, the dry gel was placed on a corundum crucible lid and placed in a muffle furnace. The temperature was increased to 300°C at a rate of 0.5°C / min and held for 24 hours. Subsequently, in the sintering process, the temperature was increased to 700°C at a rate of 0.5°C / min and held for 24 hours. The mixture was then cooled to room temperature in the furnace to obtain a microporous glass structure.

[0218] Growth of S3.CdS quantum dots: A mesoporous glass was placed in a crucible, which was then placed in a tube furnace. Air was removed using a mechanical pump to achieve a vacuum level of 1*10⁻⁶. -3 After passing through H2S gas at kPa, the glass was allowed to stand at 100℃ for 48 hours to obtain a mesoporous glass with PbS quantum dots grown in situ within a mesoporous structure.

[0219] Test Example 31: Ink Transparency

[0220] Test sample: Ink prepared in Example 6

[0221] Test equipment: UV-Vis spectrophotometer (Cary 60, Agilent, USA)

[0222] Test range: 300-850nm;

[0223] The ink prepared in Example 6 had a light transmittance of 85.3% within the test range.

[0224] Test Example 32: Viscosity Test

[0225] Test sample: Ink prepared in Example 6

[0226] Test equipment: Rotational rheometer (MCR 502e, Anton Paar, Austria)

[0227] Test conditions: 25℃, shear rate measurement range: 1-1500s -1 .

[0228] The viscosity of the ink prepared in Example 6 is 4.2 cP / 10s.

[0229] Test Example 33: Thermogravimetric-Differential Thermal Testing

[0230] Test sample: Dry gel prepared in Example 6

[0231] Testing equipment: TG / DTA analyzer (EXSTAR 7300, SII, Japan)

[0232] Test conditions: Measurement temperature range: 50-1100℃, heating rate: 5℃ / min.

[0233] The dry gel prepared in Example 6 showed a weight loss peak at around 340°C, with an inorganic content of 82.1 wt%.

[0234] Test Example 34: Pore Size Analysis of Mesoporous Glass

[0235] Test sample: Mesoporous glass prepared in Example 6

[0236] Test equipment: Surface area and pore size analyzer (Micromeritics ASAP 2460, Shanghai); Adsorbed gas: nitrogen; Degassing temperature: 200℃; Degassing time: 8h.

[0237] The glass prepared in Example 6 exhibits a typical adsorption-desorption curve pattern for mesoporous materials, with a specific surface area of ​​521 m². 2 / g, with an average pore size of 10.3nm.

[0238] Test Example 35: Glass Composition Test

[0239] Test sample: Mesoporous glass prepared in Example 6

[0240] Test equipment: Transmission electron microscope (HEOL-2010, USA); Energy dispersive X-ray spectroscopy (EDS) detector (Oxford Instruments, UK).

[0241] The mesoporous glass prepared in Example 6 has an Al2O3-SiO2 composition and a uniform elemental distribution.

[0242] Test Example 36: Fluorescence Spectroscopy of Quantum Dots

[0243] Test sample: In-situ grown PbS quantum dot mesoporous glass prepared in Example 6

[0244] Test equipment: Steady-state / transient fluorescence spectrometer (Edinburgh, FLS 980, UK)

[0245] Test conditions: excitation light source wavelength: 900nm; test range: 950-1600nm; sampling interval: 1nm; repeated sampling: 5 times.

[0246] The in-situ grown PbS quantum dot mesoporous glass prepared in Example 6 showed a broad fluorescence emission peak at 1132 nm, proving the formation of PbS quantum dots.

[0247] The above-described embodiments are merely examples of several implementations of the present invention, and their descriptions are quite specific. However, these embodiments should not be construed as limiting the scope of the present invention. It should be noted that those skilled in the art can make several modifications without departing from the concept of the present invention, and these modifications all fall within the scope of protection of the present invention. The scope of protection of the present invention should be determined by the appended claims.

Claims

1. A method for preparing chalcogenide quantum dot nanoporous glass, characterized in that, The glass molar composition is (Al2O3). x -(SiO2) y -(PbS / CdS) z Where x = 2~10, x+y = 100, z = 0.2~1, the method includes the following steps: S1: Dissolve the pore-forming agent and the salts that make up the quantum dots in water to obtain an aqueous solution. Adjust the pH of the aqueous solution to 1-4 using an acid solution. The pore-forming agent used is aluminum lactate. S2. The silicone organic compound is miscible with an alcohol solvent to obtain an alcohol solution, which is then added to an aqueous solution and stirred to obtain a silica sol; S3. Dissolve the photoinitiator in a silane coupling agent to obtain a photosensitive solution. Add the photosensitive solution dropwise to the silica sol obtained in step S2, add the polycondensation catalyst, add the fluorescent dye solution, and stir to obtain a UV-curable silica sol. The polycondensation catalyst is one or a mixture of two or more of ammonium acetate and formamide. S4. Use 3D printing to solidify the silica sol onto the printing platform to obtain a three-dimensional wet gel. S5. Place the gel obtained from step S4 in a sealed container at room temperature, keep the vapor pressure of water and ethanol stable, and let it stand for 3 to 5 days. For the gradient drying process, place the wet gel in a petri dish or filter paper, put the petri dish or filter paper in an oven, and heat it in increments of 10°C within the range of 30 to 100°C. Hold the temperature for 16 to 24 hours for each 10°C increase to obtain the dry gel. S6. Place the dry gel on the corundum crucible lid, put it into a muffle furnace, and heat it to 300℃ at a heating rate of 0.1~0.5℃ / min, and hold it for 2-24 hours; then the sintering process is as follows: heat it to 700℃ at a heating rate of 0.5℃ / min, hold it for 2-24 hours, and cool it to room temperature with the furnace to obtain microporous glass. S7. Place the mesoporous glass in a tube furnace and react it with hydrogen sulfide gas to obtain nanoporous glass with in-situ growth of sulfide quantum dots in a microporous structure.

2. The method for preparing a chalcogenide quantum dot nanoporous glass according to claim 1, characterized in that, In step S1, the salt solution that forms the quantum dots is either cadmium acetate or lead acetate, and the acid solution is either dilute nitric acid or dilute hydrochloric acid or a mixture of two of them.

3. The method for preparing a chalcogenide quantum dot nanoporous glass according to claim 1, characterized in that, In step S2, the organosilicon is one or a mixture of two of tetrahexyl orthosilicate (TEOS) and tetramethoxysilane (TMOS), and the alcohol solvent is one or a mixture of two or more of ethanol, isopropanol, and methanol.

4. The method for preparing a chalcogenide quantum dot nanoporous glass according to claim 1, characterized in that, In step S3, the photoinitiator is one or a mixture of two or more of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide (TPO), ethyl 2,4,6-trimethylbenzoylphenylphosphonate (TPO-L), and diacylphosphine oxide 819 (BBDMP); the silane coupling agent is one or a mixture of two or more of 3-(trimethoxysilyl)propyl acrylate (APTMS), (3-glycidylpropoxy)trimethoxysilane, and 3-aminopropyltrimethoxysilane; and the fluorescent dye solution is one or a mixture of two or more of Rhodamine B ethanol solution, Rhodamine 6G ethanol solution, and methyl orange aqueous solution.

5. The method for preparing a chalcogenide quantum dot nanoporous glass according to claim 1, characterized in that, The growth process of chalcogenide quantum dots in step S7 is as follows: place mesoporous glass in a crucible, place the crucible in a tube furnace, evacuate the furnace with a mechanical pump, introduce H2S gas, and let it stand at 25°C to 100°C for 12-48 hours.

Citation Information

Patent Citations

  • Chalcogenide quantum dots and phosphate mesoporous glass composites and their preparation methods

    CN105693096B

  • A glass slurry, its preparation method, and a method for 3D printing glass devices.

    CN111825333B

  • Preparation method of transparent nanopore glass ink and method for additive manufacturing of transparent nanopore glass material by using transparent nanopore glass ink

    CN116874182A

  • Gas phase preparation method for growing chalcogenide quantum dots in nanopore inorganic glass

    CN117623644A