Additive for alkaline etching texturing solution and texturing solution containing the same
By adding pullulan, sodium nitrophenolate, sodium lignosulfonate, and potassium gluconate to the alkaline etching texturing solution, the problems of uneven etching and corrosion resistance of large-size porous single-crystal silicon electrodes are solved, forming a pyramid-shaped microstructure, improving etching uniformity and corrosion resistance, and making it suitable for industrial applications.
Patent Information
- Application Number
- CN202410300757.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-15
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-03-15
AI Technical Summary
The existing chemical etching texturing technology in the photovoltaic industry is not suitable for large-size porous monocrystalline silicon electrodes, resulting in white marks on the surface and around the pores. In addition, IPA is prone to volatilization and failure, and the surface tension cannot be controlled, affecting etching uniformity and corrosion resistance.
Alkaline etching texturing solution additives, including pullulan, sodium nitrophenolate, sodium lignosulfonate, and potassium gluconate, are used to prepare the alkaline etching texturing solution. This forms a pyramid-shaped microstructure, increases the surface area, improves corrosion resistance, and disperses plasma during the dry etching process, ensuring etching uniformity.
It achieves the etching of uniform pyramid-shaped microstructures on the surface of large-size porous single-crystal silicon electrodes, improving etching uniformity and corrosion resistance, and extending service life. At the same time, the additives are environmentally friendly and free of volatiles, making them suitable for industrial applications.
Smart Images

Figure CN118127642B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of semiconductor etching and texturing, and relates to an additive for an alkaline etching and texturing solution for large-size porous electrodes of single-crystal silicon and a texturing solution containing the additive. Background Art
[0002] Wafer etching is divided into wet etching and dry etching. The advantage of wet etching is that the etching rate is quite fast and only chemical methods are used, so the "selectivity" is higher. But the problem is that it can only perform isotropic etching. During wet etching, the wafer is immersed in liquid, and the protected part on the back of the photoresist will also react with the liquid, being quickly dissolved and corroded, with poor accuracy. Dry etching refers to all processes that use gas for etching, that is, after superimposing the photoresist "mold" on the wafer, it is exposed to the etching gas. Dry etching can be divided into plasma etching, sputtering etching and reactive ion etching (RIE, Reactive Ion Etching).
[0003] Dry etching, also known as gas etching, is an etching method widely used in the industry. The wafer material is placed in an etching chamber, and etching gas is input into the etching chamber. The etching of the wafer material can be completed by the etching gas. While the plasma is dry etching the wafer, it will also corrode the gas diverter disk to a certain extent. In the prior art, the surface of the gas diverter disk is etched with acid. After etching, its micromorphology is similar to that of insect eggs, which can improve corrosion resistance to a certain extent.
[0004] At present, the chemical etching technology for texturing in the photovoltaic industry mostly uses a texturing solution made of potassium hydroxide, potassium silicate or IPA (isopropyl alcohol) for photovoltaic silicon wafers. However, this formula is not suitable for large-sized porous monocrystalline silicon electrodes because large-sized porous monocrystalline silicon products have a large surface area and many pores. During the reaction, the pores continuously produce a large number of bubbles, which adhere to the surface and pores of the product. A large amount of potassium silicate cannot be removed or defoamed in time, and white marks will form on the surface and around the pores of the final product, resulting in the product being scrapped. Moreover, IPA is volatile and will become ineffective during use, and it cannot control the surface tension well. Summary of the invention
[0005] In view of this, an object of the present invention is to provide an additive for an alkaline etching texturing solution and a texturing solution containing the additive, which is suitable for large-sized porous single crystal silicon products.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] 1. An additive for an alkaline etching texturing solution, the additive comprising the following components: pullulan, sodium nitrophenolate, sodium lignin sulfonate and potassium gluconate.
[0008] The additives of the alkaline etching texturing solution further include, by weight:
[0009] 0.08-1 part of pullulan;
[0010] 0.001-0.08 parts of sodium nitrophenolate;
[0011] 0.02-0.1 parts of sodium lignin sulfonate;
[0012] 0.01-0.1 parts potassium gluconate.
[0013] The additives of the alkaline etching texturing solution further include, by weight:
[0014] 0.2-0.5 parts of pullulan;
[0015] 0.01-0.06 parts of sodium nitrophenolate;
[0016] 0.02-0.08 parts of sodium lignin sulfonate;
[0017] 0.02-0.05 parts of potassium gluconate.
[0018] 2. Application of any of the above-mentioned additives in alkaline etching and texturing of single crystal silicon.
[0019] 3. An alkaline etching texturing solution comprising any of the additives described above and a solution of an inorganic base.
[0020] Furthermore, in the alkaline etching texturing solution, the inorganic base is selected from potassium hydroxide and / or sodium hydroxide.
[0021] Furthermore, the alkaline etching texturing solution comprises, by mass percentage, 1%-8% potassium hydroxide, 0.08%-1% pullulan, 0.001%-0.08% sodium nitrophenolate, 0.02%-0.1% sodium lignin sulfonate, and 0.01%-0.1% potassium gluconate.
[0022] 4. Application of the alkaline etching texturing solution described in any one of the above items in alkaline etching texturing of single crystal silicon.
[0023] 5. A method for preparing single crystal silicon by alkaline etching and texturing, the specific steps of the preparation method are:
[0024] 1) Grind the single crystal silicon sample, put it into degreasing liquid for cleaning, and then rinse it with pure water;
[0025] 2) After cleaning, the single crystal silicon sample is immersed in 1%-5% alkali solution for 3-5 minutes, and then ultrasonically cleaned with pure water;
[0026] 3) The cleaned single crystal silicon sample in step 2) is subjected to alkaline etching, placed in an alkaline etching texturing solution, etched at 75-85° C. for 30-60 minutes, and finally ultrasonically cleaned with pure water. The alkaline etching texturing solution is calculated by weight:
[0027] 1%-8% inorganic alkali,
[0028] 0.08%-1% pullulan,
[0029] 0.001%-0.08% sodium nitrophenolate,
[0030] 0.02%-0.1% sodium lignin sulfonate,
[0031] 0.01%-0.1% potassium gluconate.
[0032] The beneficial effects of the present invention are as follows: the present invention provides an alkaline etching texturing liquid, which can etch a microstructure similar to a pyramid shape on the micro surface of a single crystal silicon gas diversion disk. The surface is reflective when viewed from the side, which has a velvety effect, and can also be called a velvet surface. The broken layer and the particles and metal ions on the surface of the gas diversion disk product can be removed. The formed velvet surface can increase the surface area of the product, further improve the corrosion resistance during the dry etching process, and increase its service life. It also effectively disperses the plasma in the dry etching process, ensures that the etching gas passes through the wafer evenly, and ensures uniform etching of the wafer material. The alkaline etching texturing liquid of the present invention does not contain organic volatiles, and will not fail during the etching process to cause uneven etching; the amount of additives used is small, and after the etching is completed, the sodium lignin sulfonate and pullulan components can be degraded by microorganisms in a certain period of time, and sodium nitrophenolate can also be hydrolyzed, so the texturing liquid is very environmentally friendly when used in industrial applications, and has good industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to make the purpose, technical solution and beneficial effects of the present invention clearer, the present invention provides the following drawings for illustration:
[0034] Figure 1 Surface image and electron microscope image of the single crystal silicon sample prepared in Example 1.
[0035] Figure 2 Surface image and electron microscope image of the single crystal silicon sample prepared in Example 2.
[0036] Figure 3 Surface image and electron microscope image of the single crystal silicon sample prepared in Example 3.
[0037] Figure 4 Surface image and electron microscope image of the single crystal silicon sample prepared in Example 4.
[0038] Figure 5 Surface image and electron microscope image of the single crystal silicon sample prepared in Comparative Example 1.
[0039] Figure 6 Surface image and electron microscope image of the single crystal silicon sample prepared in Comparative Example 2.
[0040] Figure 7 Surface image and electron microscope image of the single crystal silicon sample prepared in Comparative Example 3.
[0041] Figure 8 Surface image and electron microscope image of the single crystal silicon sample prepared in Comparative Example 4. DETAILED DESCRIPTION
[0042] The preferred embodiment of the present invention will be described clearly and completely below in conjunction with the accompanying drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. The experimental methods for which specific conditions are not specified in the embodiments are usually carried out under conventional conditions or under conditions recommended by the manufacturer.
[0043] The present invention is mainly applied to large-size products of semiconductor single crystal silicon materials. This type of product has a diameter of 300 mm, a number of pores exceeding several thousand, and a pore diameter of about 0.4 mm.
[0044] The concentrations involved in the following examples are in mass percentages, and the solvent involved is pure water. Sodium lignin sulfonate: CAS No.: 8061-51-6; Pullulan: CAS No.: 9057-02-7; Potassium gluconate: CAS No.: 35398-15-3.
[0045] The alkaline etching texturing solution specifically comprises: 1%-8% potassium hydroxide, 0.08%-1% pullulan, 0.001%-0.08% sodium nitrophenolate, 0.02%-0.1% sodium lignin sulfonate, and 0.01%-0.1% potassium gluconate.
[0046] The preferred alkaline etching texturing solution includes: 4%-7% potassium hydroxide, 0.2%-0.5% pullulan, 0.01%-0.06% sodium nitrophenolate, 0.02%-0.08% sodium lignin sulfonate, and 0.02%-0.05% potassium gluconate.
[0047] Example 1
[0048] 1) After grinding the single crystal silicon sample, put it into the degreasing liquid for cleaning for 10-20 minutes, and rinse it with pure water at 40°C;
[0049] 2) After cleaning, the single crystal silicon sample is immersed in 1% alkali solution for 3-5 minutes, and then cleaned again with pure water ultrasound at 60° C. for 5-10 minutes;
[0050] 3) Step 2) The cleaned single crystal silicon sample is subjected to alkaline etching, placed in an alkaline etching liquid, and etched at 80°C for 30
[0051] Minutes, and finally use pure water ultrasound for 5-10 minutes to complete the cleaning;
[0052] The alkaline etching texturing solution specifically includes: 7% potassium hydroxide, 0.5% pullulan, 0.06% sodium nitrophenolate, 0.03% sodium lignin sulfonate, and 0.03% potassium gluconate.
[0053] Degreasing liquid: 3% alkali + 5% surfactant, or other conventional degreasing liquids can be used, such as the cleaning agent for surface degreasing of semiconductor materials in CN113980747B. The degreasing liquid is used for pre-cleaning to further activate the reaction effect of silicon and alkali.
[0054] The surface image and electron microscope image of the single crystal silicon sample obtained by the above preparation method are as follows: Figure 1 As shown by Figure 1 It can be seen that there is no color difference in the appearance of the sample, and the pyramids are balanced in size, with a length and width of about 10μm-15μm, which is within the acceptable range.
[0055] Example 2
[0056] 1) After grinding the single crystal silicon sample, put it into the degreasing liquid for cleaning for 10-20 minutes, and rinse it with pure water at 40°C;
[0057] 2) After cleaning, the single crystal silicon sample is immersed in 1% alkali solution for 3-5 minutes, and then cleaned again with pure water ultrasound at 60° C. for 5-10 minutes;
[0058] 3) Step 2) The cleaned single crystal silicon sample is subjected to alkaline etching, placed in an alkaline etching liquid, and etched at 80°C for 30
[0059] Minutes, and finally use pure water ultrasound for 5-10 minutes to complete the cleaning;
[0060] The alkaline etching texturing solution specifically includes: 5% potassium hydroxide, 0.4% pullulan, 0.02% sodium nitrophenolate, 0.03% sodium lignin sulfonate, and 0.02% potassium gluconate.
[0061] The surface image and electron microscope image of the single crystal silicon sample obtained by the above preparation method are as follows: Figure 2As shown by Figure 2 It can be seen that there is no color difference in the appearance of the sample, and the size of the pyramids is balanced and within an acceptable range.
[0062] Example 3
[0063] 1) After grinding the single crystal silicon sample, put it into the degreasing liquid for cleaning for 10-20 minutes, and rinse it with pure water at 40°C;
[0064] 2) After cleaning, the single crystal silicon sample is immersed in 1% alkali solution for 3-5 minutes, and then cleaned again with pure water ultrasound at 60° C. for 5-10 minutes;
[0065] 3) The cleaned single crystal silicon sample in step 2) is subjected to alkaline etching, placed in an alkaline etching texturing solution, etched at 75-85° C. for 30 minutes, and finally cleaned with pure water ultrasound for 5-10 minutes;
[0066] The alkaline etching texturing solution specifically includes: 4% potassium hydroxide, 0.2% pullulan, 0.01% sodium nitrophenolate, 0.05% sodium lignin sulfonate, and 0.02% potassium gluconate.
[0067] The surface image and electron microscope image of the single crystal silicon sample obtained by the above preparation method are as follows: Figure 3 As shown by Figure 3 It can be seen that the sample appearance has no color difference, and the pyramid size is balanced and within the acceptable range. In this embodiment, three samples were used to test the etching conditions at 75° C., 80° C., and 85° C., and the results were all acceptable.
[0068] Example 4
[0069] 1) After grinding the single crystal silicon sample, put it into the degreasing liquid for cleaning for 10-20 minutes, and rinse it with pure water at 40°C;
[0070] 2) After cleaning, the single crystal silicon sample is immersed in 1% alkali solution for 3-5 minutes, and then cleaned again with pure water ultrasound at 60° C. for 5-10 minutes;
[0071] 3) The cleaned single crystal silicon sample in step 2) is subjected to alkaline etching, placed in an alkaline etching texturing solution, etched at 80° C. for 30 minutes, and finally cleaned with pure water ultrasound for 5-10 minutes;
[0072] The alkaline etching texturing solution specifically includes: 6% potassium hydroxide, 0.3% pullulan, 0.05% sodium nitrophenolate, 0.04% sodium lignin sulfonate, and 0.03% potassium gluconate.
[0073] The surface image and electron microscope image of the single crystal silicon sample obtained by the above preparation method are as follows: Figure 4 As shown by Figure 4It can be seen that the sample appearance has no color difference, and the pyramid size is balanced and within the acceptable range. In this embodiment, three samples were used to test the etching conditions at 75° C., 80° C., and 85° C., and the results were all acceptable.
[0074] In addition, the potassium hydroxide in other embodiments may also be replaced by sodium hydroxide, and the etching effect is similar to that of the above embodiment, which will not be described in detail here.
[0075] Comparative Example 1
[0076] The difference from Example 1 is that the components and mass fraction of the alkaline etching texturing solution in this example are different, and the rest are the same as Example 1.
[0077] The alkaline etching texturing solution specifically includes: 8% potassium hydroxide, 0.1% sodium nitrophenolate, 0.03% sodium lignin sulfonate, and 0.01% potassium gluconate.
[0078] The surface image and electron microscope image of the single crystal silicon sample obtained by the above preparation method are as follows: Figure 5 As shown by Figure 5 It can be seen that the surface of the sample has a slight color difference, the pyramid velvet surface has not grown evenly, and the distribution is uneven.
[0079] Comparative Example 2
[0080] The difference from Example 1 is that the components and mass fraction of the alkaline etching texturing solution in this example are different, and the rest are the same as Example 1.
[0081] The alkaline etching texturing solution specifically includes: 10% potassium hydroxide, 0.5% pullulan, 0.1% sodium lignin sulfonate, and 0.03% potassium gluconate.
[0082] The surface image and electron microscope image of the single crystal silicon sample obtained by the above preparation method are as follows: Figure 6 As shown by Figure 6 It can be seen that there is no halo around the holes on the surface of the sample product, no white spots, and no obvious pyramid suede on the surface.
[0083] Comparative Example 3
[0084] The difference from Example 1 is that the components and mass fraction of the alkaline etching texturing solution in this example are different, and the rest are the same as Example 1.
[0085] The alkaline etching texturing solution specifically includes: 7% potassium hydroxide, 0.5% pullulan, 0.04% sodium nitrophenolate, and 0.01% potassium gluconate.
[0086] The surface image and electron microscope image of the single crystal silicon sample obtained by the above preparation method are as follows: Figure 7 As shown by Figure 7It can be seen that the suede on the surface of the sample is not fully grown in some parts.
[0087] Comparative Example 4
[0088] The difference from Example 1 is that the components and mass fraction of the alkaline etching texturing solution in this example are different, and the rest are the same as Example 1.
[0089] The alkaline etching texturing solution specifically includes: 3% potassium hydroxide, 0.3% pullulan, 0.02% sodium nitrophenolate, and 0.02% sodium lignin sulfonate.
[0090] The surface image and electron microscope image of the single crystal silicon sample obtained by the above preparation method are as follows: Figure 8 As shown by Figure 8 It can be seen that there is chromatic aberration caused by halos around the holes on the surface of the sample, and the golden tower is very small.
[0091] Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made in form and details without departing from the scope defined by the claims of the present invention.
Claims
1. An additive for alkaline etching texturing solution, characterized in that: The additive comprises the following components in parts by weight: 0.08-1 part of pullulan; 0.001-0.08 parts of sodium nitrophenolate; 0.02-0.1 parts of sodium lignin sulfonate; 0.01-0.1 parts potassium gluconate.
2. The additive for alkaline etching texturing solution according to claim 1, characterized in that: The additive comprises the following components in parts by weight: 0.2-0.5 parts of pullulan; 0.01-0.06 parts of sodium nitrophenolate; 0.02-0.08 parts of sodium lignin sulfonate; 0.02-0.05 parts of potassium gluconate.
3. Use of the additive according to any one of claims 1 to 2 in alkaline etching and texturing of single crystal silicon.
4. An alkaline etching texturing solution, characterized in that: A solution comprising the additive according to any one of claims 1 to 2 and an inorganic base.
5. The alkaline etching texturing solution according to claim 4, characterized in that: The inorganic base is selected from potassium hydroxide and / or sodium hydroxide.
6. The alkaline etching texturing solution according to claim 4, characterized in that: Calculated by mass percentage, the alkaline etching texturing solution contains: 1%-8% potassium hydroxide, 0.08%-1% pullulan, 0.001%-0.08% sodium nitrophenolate, 0.02%-0.1% sodium lignin sulfonate, and 0.01%-0.1% potassium gluconate.
7. Use of the alkaline etching texturing solution described in any one of claims 4 to 6 in alkaline etching texturing of single crystal silicon.
8. A method for preparing single crystal silicon by alkaline etching texturing, characterized in that: The specific steps of the preparation method are: 1) Grind the single crystal silicon sample, put it into degreasing liquid for cleaning, and then rinse it with pure water; 2) After cleaning, the single crystal silicon sample is immersed in 1%-5% alkali solution for 3-5 minutes, and then ultrasonically cleaned with pure water; 3) The cleaned single crystal silicon sample of step 2) is subjected to alkaline etching, placed in an alkaline etching texturing solution, etched at 75-85°C for 30-60 minutes, and finally ultrasonically cleaned with pure water. The alkaline etching texturing solution is the alkaline etching texturing solution described in any one of claims 4-6.
9. The method for preparing single crystal silicon alkaline etching texturing according to claim 8, characterized in that: Calculated by mass percentage, the alkaline etching texturing solution contains: 1%-8% potassium hydroxide, 0.08%-1% pullulan, 0.001%-0.08% sodium nitrophenolate, 0.02%-0.1% sodium lignin sulfonate, and 0.01%-0.1% potassium gluconate.