Cobalt-based superalloys with excellent high-temperature strength and their manufacturing method

By adding Ta, Ti, Cr, Mo and B elements to cobalt-based superalloys and using solid solution and aging heat treatment processes, a stable γ′ phase structure is formed, which solves the problem of insufficient high-temperature strength of cobalt-based superalloys and achieves excellent yield strength and oxidation resistance at high temperatures, making it suitable for high-end aerospace equipment.

CN118147490BActive Publication Date: 2026-11-17SHENYANG RES INST OF FOUNDRY
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410166756.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-06
Publication Date
2026-11-17
Estimated Expiration
2044-02-06

AI Technical Summary

Technical Problem

Existing cobalt-based superalloys have insufficient strength and low creep performance under high temperature conditions, which cannot meet the requirements of key hot-end components in advanced aerospace equipment.

Method used

By adopting the Co-Ni-Al-W alloy system and adding Ta, Ti, Cr, Mo and B elements, combined with solid solution and aging heat treatment processes, a stable γ′ phase structure is formed, the size and morphology of the γ′ phase are optimized, and the high-temperature strength and oxidation resistance of the alloy are improved.

Benefits of technology

It achieves a yield strength of ≥800MPa at high temperatures, exhibits good alloy microstructure stability, and possesses excellent high-temperature strength and oxidation resistance, making it suitable for key hot-end components in high-end aerospace equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118147490B_ABST
    Figure CN118147490B_ABST
Patent Text Reader

Abstract

This invention provides a cobalt-based superalloy with excellent high-temperature strength, whose chemical composition, by mass percentage, includes the following components: C: 0.02–0.06%, Ni: 22.0–30.0%, Al: 2.0–4.0%, Ti: 4.0–5.0%, Cr: 5.0–8.0%, Mo: 2.0–3.0%, Ta: 4.0–6.0%, W: 8.0–10.0%, B: 0.01–0.03%, with the remainder being Co and unavoidable impurities. This invention significantly improves the high-temperature strength of the alloy and ensures good oxidation resistance. This invention also includes a method for preparing the aforementioned cobalt-based superalloy with excellent high-temperature strength, comprising the following steps: Step 1, smelting in a vacuum electromagnetic induction melting furnace with protective casting throughout the process to obtain a cobalt-based superalloy ingot; Step 2, precision casting to obtain equiaxed crystal sample parts; Step 3, solution treatment and aging heat treatment to obtain the cobalt-based superalloy with excellent high-temperature strength. The alloy of this invention has a high yield and good high-temperature structural stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of high-temperature alloy material design and preparation technology, and in particular to a cobalt-based high-temperature alloy with excellent high-temperature strength and its manufacturing method. Background Technology

[0002] In the field of high-temperature alloy material design, preparation, and application technology, among the three major high-temperature alloy systems currently in practical use—iron-based, nickel-based, and cobalt-based—traditional cobalt-based high-temperature alloys use Co-Ni-Cr as the matrix, adding a large amount of W-based solid solution strengthening elements for solid solution strengthening, and using carbide precipitation strengthening. Therefore, cobalt-based high-temperature alloys have high melting temperatures, excellent oxidation and corrosion resistance, flat creep rupture curves (LM curves), good resistance to thermal fatigue, and good weldability, making them very suitable for manufacturing key components such as turbine guide vanes for aero-engines.

[0003] However, due to the lack of a γ′ phase strengthening mechanism, the engineering applications of traditional cobalt-based superalloys relying solely on solid solution strengthening and carbide strengthening are severely limited at higher temperatures (>800℃). In recent years, researchers have discovered the γ′-Co3(Al,W) phase in Co-Al-W based alloy systems, with a γ′ dissolution temperature reaching 990℃, approximately 250℃ higher than γ′-Co3Ti and Co3Ta. This suggests that γ′ phase-strengthened cobalt-based superalloy systems hold promise for achieving a combination of high temperature resistance and high environmental resistance. At the European High-Temperature Alloys Conference held in France in 2014, γ′ phase-strengthened cobalt-based superalloys were listed as one of the seven major trends in the future development of high-temperature alloy materials technology.

[0004] With the continuous development of aero-engines and ground-based gas turbines, the requirements for the environmental resistance and temperature resistance of their key hot-end components are becoming increasingly stringent. γ′ phase-strengthened cobalt-based superalloys have advantages over nickel-based superalloys in terms of hot corrosion resistance and melting temperature. To promote the development of this type of alloy, alloy design and optimization methods that comprehensively consider multiple key engineering application indicators such as microstructure stability, mechanical properties, and density are needed. This will accelerate the engineering application process of cobalt-based superalloys and provide material support for the independent development of key hot-end components in my country's aerospace, energy, and transportation sectors. γ′ phase-strengthened cobalt-based superalloys not only have a higher melting temperature than nickel-based superalloys but also retain the good wear resistance and thermal fatigue resistance of traditional cobalt-based superalloys, making them a high-potential high-temperature structural material.

[0005] In the prior art, invention patent CN113699414B proposes a γ′ phase-reinforced cobalt-based superalloy with excellent high-temperature tensile properties. The alloy composition of this patent contains Ti: 1–3 wt.%, B: 0.005–0.01 wt.%, W: 2–6 wt.%, and Zr: 0.05–0.2 wt.%, and employs a heat treatment process of solution treatment + first-stage aging + second-stage aging. However, the final alloy has a yield strength of less than 700 MPa at 800℃, thus failing to meet the higher requirements of key hot-end components in advanced aerospace equipment.

[0006] Patent CN108385010B discloses a low-density, high-structural-stability cobalt-based superalloy and its preparation method. The alloy composition contains Y, Ce, or La: 0.01–1 at.%, Fe: 0–4 at.%, Hf: 0.01–1 at.%, and Nb: 0–4 at.%. The heat treatment process involves solution treatment + first-stage aging + second-stage aging. The final alloy maintains a two-phase microstructure of γ′ and γ at 700℃, with a room temperature Vickers hardness of 468 HV. However, the alloy exhibits insufficient strength at high temperatures (800℃).

[0007] Based on the current state of technology, the microstructure of cobalt-based superalloys used under high-temperature conditions is mainly composed of carbides, γ′ and γ phases. These alloys suffer from problems such as insufficient high-temperature strength and low creep performance during use. This is because the γ′ phase coarsens and its volume fraction decreases under high-temperature conditions, resulting in a significant reduction in high-temperature strength.

[0008] Currently, achieving superior high-temperature strength in high-performance cobalt-based superalloys is a critical technical challenge that urgently needs to be addressed in high-end aerospace high-temperature structural materials. Summary of the Invention

[0009] This invention provides a cobalt-based superalloy with excellent high-temperature strength and its preparation method.

[0010] The technical solution of this invention is as follows:

[0011] The key technology of cobalt-based superalloys with excellent high-temperature strength is that their chemical composition, by mass percentage, includes the following components: C: 0.02–0.06%, Ni: 22.0–30.0%, Al: 2.0–4.0%, Ti: 4.0–5.0%, Cr: 5.0–8.0%, Mo: 2.0–3.0%, Ta: 4.0–6.0%, W: 8.0–10.0%, B: 0.01–0.03%, with the remainder being Co and unavoidable impurities.

[0012] This invention also claims protection for a method for preparing a cobalt-based superalloy with excellent high-temperature strength as described above, the key technology of which includes the following steps:

[0013] Step 1: Smelt the cobalt-based high-temperature alloy in a vacuum electromagnetic induction melting furnace according to the chemical composition requirements of the alloy with excellent high-temperature strength, and cast it under full protection throughout the process to finally obtain the cobalt-based high-temperature alloy ingot.

[0014] In step 1, the raw materials used are pure Ni, pure Al, pure W, pure Ta, pure Ti and pure Co, each with a purity of not less than 99.9%; the high-temperature refining technical parameters include: power of 15-25kW, melting temperature of 1470-1550℃, and holding time of 25-35min.

[0015] Step 2: The riser of the master alloy ingot is removed by wire cutting. At the same time, the surface of the alloy ingot is polished to remove the surface iron oxide scale. Then, the alloy ingot is melted under argon protection and precision casting is performed to obtain equiaxed crystal sample parts.

[0016] Step 3: Perform solution treatment and aging heat treatment on the sample to obtain the cobalt-based high-temperature alloy with excellent high-temperature strength;

[0017] The heat treatment process includes: solution treatment, with a solution temperature of 1180-1210℃ and a holding time of 4-8 hours, and an average cooling rate of 4-10℃ / s after exiting the furnace; and aging treatment, with an aging temperature of 880-920℃ and a holding time of 15-20 hours, and an average cooling rate of 4-10℃ / s after exiting the furnace.

[0018] Further optimization requirements are:

[0019] In step 2, the induction power supply of the vacuum electromagnetic induction melting furnace generates an electromagnetic stirring effect while induction heating the cobalt-based high-temperature alloy melt, which makes the alloy elements in the melt more uniformly distributed and reduces macroscopic segregation.

[0020] The casting temperature is 1450–1500℃, and the melting and holding time is 25–35 minutes.

[0021] During the entire process of casting the alloy ingot into a test piece under full protection, it is required to control [O] < 25 ppm, [N] < 10 ppm, and [S] < 10 ppm.

[0022] Other relevant descriptions of this invention are supplemented as follows:

[0023] This invention involves extensive and systematic experimental research on several aspects, including alloy element content, precision casting control, optimization and parameter selection of solution treatment and aging heat treatment processes, and microstructure control. Ultimately, it determined the alloy element ratios and preparation schemes that meet the objectives of this invention. During the precision casting process, the alloy is thoroughly melted, and the casting process ensures uniform filling of the alloy melt while controlling the cooling rate to effectively control grain size. The heat treatment process for the alloy is solution treatment followed by aging heat treatment, resulting in the formation of a γ′ phase with a content exceeding 60%. The formed γ′ phase exhibits high thermal stability and mechanical properties: firstly, the γ′ phase in the alloy does not undergo phase transformation under high-temperature conditions, exhibiting high thermal stability; secondly, the presence of a large amount of γ′ phase significantly improves the alloy's yield strength during high-temperature deformation through interaction with dislocations.

[0024] The mechanism of action of each alloy component in the high-strength cobalt-based superalloy prepared by this invention is as follows (where the percentage symbol % represents mass percentage):

[0025] Ni: Increasing the Ni content can expand the γ′+γ two-phase region, increase the volume fraction of the γ′ phase, and raise the dissolution temperature of the γ′ phase, thus reducing the lattice parameters and mismatch of the γ / γ′ two-phase. However, excessively high Ni content can lead to χ-D0 19 The precipitation of the γ′ phase and the decrease in the volume fraction of the γ′ phase mean that the Ni content in this invention is controlled at 22.0% to 30.0%.

[0026] W: Adding W can not only enhance the high-temperature strength and oxidation resistance of cobalt-based alloys, but also form a γ′ phase with Co with an L12 structure, which improves the stability and dissolution temperature of the γ′ phase. However, excessive W content will increase the density of the alloy. Therefore, the W content in this invention is controlled at 8.0 to 10.0%.

[0027] Al: Adding Al can form the L12 structure γ′-Co3(Al,W) phase with Co and W, while improving the alloy's oxidation resistance and preventing oxygen from continuing to diffuse into the alloy, thus controlling the Al content at 2.0-4.0%.

[0028] Ti: By adding Ti, the volume fraction of the γ′ phase is increased, the dissolution temperature of the γ′ phase is increased, and the strength of the alloy is further improved. Therefore, the preferred Ti content is 4.0 to 5.0%.

[0029] Ta: Ta can increase the dissolution temperature of the γ′ phase in the alloy, effectively improve the stability of the γ′ phase, and increase the volume fraction of the γ′ phase, thereby improving the high-temperature strength of the alloy. Therefore, the preferred Ta content is 4.0 to 6.0%.

[0030] Cr: Adding Cr can form a Cr2O3 protective layer on the alloy surface, which significantly improves the oxidation resistance and corrosion resistance. However, the addition of Cr lowers the dissolution temperature of the γ′ phase, and excessive addition of Cr can also destroy the microstructure of γ′+γ. Therefore, the Cr content in this invention is controlled at 5.0-8.0%.

[0031] Mo: Adding Mo can increase the volume fraction of the γ′-Co3(Al,W) phase, but it will increase the size of the γ′ phase. However, although replacing W with Mo can reduce the segregation of Al during solidification and reduce the alloy density, it also lowers the dissolution temperature of the γ′ phase and reduces the mismatch between the γ / γ′ phases. After solution treatment and aging, the alloy is prone to precipitating the μ phase, which leads to a decrease in the high-temperature hardness and strength of the alloy. Therefore, the Mo content in this invention is controlled at 2.0-3.0%.

[0032] C: Adding carbon can improve the casting properties of the alloy, and C is an important grain boundary strengthening element; however, excessive C will lead to the formation of carbides at the grain boundaries, which will deteriorate its mechanical properties. Therefore, the preferred C content is 0.25 to 1.0 wt.%.

[0033] B: Adding boron (B) can improve the grain boundary strength of high-temperature alloys and reduce nitrogen (M). 23 C6 aggregates at grain boundaries, reducing the grain boundary diffusion coefficient and thus enhancing grain boundary bonding. Therefore, the boron content is controlled between 0.01% and 0.03%.

[0034] The beneficial effects of this invention are as follows:

[0035] 1. To improve the high-temperature performance of cobalt-based superalloys, the high-strength cobalt-based superalloy of this invention adopts a Co-Ni-Al-W alloy system with added elements such as Ta, Ti, Cr, Mo, and B. This alloy design can form a stable γ′ phase, significantly improving the high-temperature strength of the alloy while ensuring good oxidation resistance. By optimizing the solution treatment and aging heat treatment process, the size, morphology, and internal element enrichment of the γ′ phase are controlled, improving the thermal stability and volume fraction of the γ′ phase. Finally, a multiphase microstructure of γ′ phase and γ matrix phase with a content of more than 60 vol.% is obtained, ensuring that the alloy has excellent high-temperature yield strength.

[0036] 2. In order to solve the problem of insufficient high-temperature strength of cobalt-based superalloys, the present invention provides a method for preparing cobalt-based superalloys with excellent high-temperature strength, which can obtain high-strength cobalt-based superalloys (800℃, yield strength ≥800MPa).

[0037] 3. The chemical composition of the cobalt-based high-temperature alloy with excellent high-temperature strength designed in this invention, combined with its preparation method, enables the production of cobalt-based high-temperature alloys with high temperature and high strength, and the alloy has a high yield and good high-temperature structural stability. Attached Figure Description

[0038] Figure 1 This is the γ′ phase morphology of alloy 1 in Example 1 of the present invention. Detailed Implementation

[0039] The present invention will be further described below with reference to the embodiments and accompanying drawings, but is not limited thereto.

[0040] The chemical composition of the cobalt-based superalloys with excellent high-temperature strength in Examples 1-6 is shown in Table 1, the smelting process is shown in Table 2, the heat treatment process is shown in Table 3, and the high-temperature strength is shown in Table 4.

[0041] Table 1. Alloy chemical composition of embodiments of the present invention

[0042] Example Ni Al W Ti Ta Cr Mo C B 1 30 3.2 8.3 4.5 5.6 5.8 2.1 0.02 0.02 2 28.6 3.8 10.0 4.1 6.0 8.0 2.5 0.04 0.03 3 22.0 2.0 9.0 5.0 4.9 5.0 3.0 0.06 0.01 4 24.8 4.0 8.0 4.0 4.0 6.3 2.0 0.05 0.02 5 26.4 2.5 9.6 4.2 4.5 7.3 2.3 0.03 0.03 6 27.1 2.7 8.7 4.8 5.2 7.8 2.7 0.03 0.02

[0043] Table 2 Alloy smelting process of the present invention embodiments

[0044]

[0045] Table 3 Alloy heat treatment process of the embodiments of the present invention

[0046]

[0047] Table 4 High-temperature strength of alloys in the embodiments of the present invention

[0048] Example 800℃, yield strength / MPa 1 808 2 815 3 814 4 820 5 819 6 826

[0049] Example 7

[0050] Cobalt-based superalloys with excellent high-temperature strength have the following chemical composition by mass percentage:

[0051] C: 0.02–0.06%, Ni: 22.0–30.0%, Al: 2.0–4.0%, Ti: 4.0–5.0%, Cr: 5.0–8.0%, Mo: 2.0–3.0%, Ta: 4.0–6.0%, W: 8.0–10.0%, B: 0.01–0.03%, with the remainder being Co and unavoidable impurities.

[0052] Example 8

[0053] The preparation method of the cobalt-based superalloy with excellent high-temperature strength as described in Example 7 includes the following steps:

[0054] Step 1: Smelt the cobalt-based high-temperature alloy in a vacuum electromagnetic induction melting furnace according to the chemical composition requirements of the alloy with excellent high-temperature strength, and cast it under full protection throughout the process to finally obtain the cobalt-based high-temperature alloy ingot.

[0055] In step 1, the raw materials used are pure Ni, pure Al, pure W, pure Ta, pure Ti and pure Co, each with a purity of not less than 99.9%; the high-temperature refining technical parameters include: power of 15-25kW, melting temperature of 1470-1550℃, and holding time of 25-35min.

[0056] Step 2: The riser of the master alloy ingot is removed by wire cutting. At the same time, the surface of the alloy ingot is polished to remove the surface iron oxide scale. Then, the alloy ingot is melted under argon protection and precision casting is performed to obtain equiaxed crystal sample parts.

[0057] In step 2, the induction power supply of the vacuum electromagnetic induction melting furnace generates an electromagnetic stirring effect while induction heating the cobalt-based high-temperature alloy melt, which makes the alloy elements in the melt more uniformly distributed and reduces macroscopic segregation.

[0058] The casting temperature is 1450–1500℃, and the melting and holding time is 25–35 minutes.

[0059] During the entire process of casting the alloy ingot into a test piece under full protection, it is required to control [O] < 25 ppm, [N] < 10 ppm, and [S] < 10 ppm.

[0060] Step 3: Perform solution treatment and aging heat treatment on the sample to obtain the cobalt-based high-temperature alloy with excellent high-temperature strength;

[0061] The heat treatment process includes: solution treatment, with a solution temperature of 1180-1210℃ and a holding time of 4-8 hours, and an average cooling rate of 4-10℃ / s after exiting the furnace; and aging treatment, with an aging temperature of 880-920℃ and a holding time of 15-20 hours, and an average cooling rate of 4-10℃ / s after exiting the furnace.

Claims

1. A method for preparing a cobalt-based superalloy with excellent high-temperature strength, characterized in that: The chemical composition of the cobalt-based superalloy includes the following components by mass percentage: C: 0.02~0.06%, Ni: 22.0~30.0%, Al: 2.0~4.0%, Ti: 4.0~5.0%, Cr: 5.0~8.0%, Mo: 2.0~3.0%, Ta: 4.0~6.0%, W: 8.0~10.0%, B: 0.01~0.03%, with the remainder being Co and unavoidable impurities; The preparation method of the cobalt-based superalloy with excellent high-temperature strength includes the following steps: Step 1: Melt the cobalt-based high-temperature alloy in a vacuum electromagnetic induction melting furnace according to the chemical composition requirements of the alloy with excellent high-temperature strength, and cast it under full protection throughout the process to finally obtain the cobalt-based high-temperature alloy ingot. In step 1, the high-temperature refining technical parameters include: power of 15~25 kW; melting temperature of 1470~1550 ℃; and holding time of 25~35 min. Step 2: The riser of the master alloy ingot is removed by wire cutting. At the same time, the surface of the alloy ingot is polished to remove the surface iron oxide scale. Then, the alloy ingot is melted under argon protection and precision casting is performed to obtain equiaxed crystal sample parts. Step 3: The sample is subjected to solution treatment and aging heat treatment to obtain a cobalt-based superalloy with excellent high-temperature strength; The heat treatment process includes: solution treatment, with a solution temperature of 1180~1210 ℃, holding for 4~8 h, and an average cooling rate of 4~10 ℃ / s after exiting the furnace; and aging treatment, with an aging temperature of 880~920 ℃, holding for 15~20 h, and an average cooling rate of 4~10 ℃ / s after exiting the furnace.

2. The method for preparing the cobalt-based superalloy with excellent high-temperature strength according to claim 1, characterized in that: In step 2, the induction power supply of the vacuum electromagnetic induction melting furnace generates an electromagnetic stirring effect while induction heating the cobalt-based high-temperature alloy melt, which makes the alloy elements in the melt more uniformly distributed and reduces macroscopic segregation. The casting temperature is 1450~1500 ℃, and the melting and holding time is 25~35 min; During the entire process of casting the alloy ingot into a test piece under protective conditions, the [O] content must be controlled to be less than 25 ppm, [N] less than 10 ppm, and [S] less than 10 ppm.

Citation Information

Patent Citations

  • A low-density, high-structural-stability cobalt-based superalloy and its preparation method

    CN108385010B

  • A γ′ phase-reinforced cobalt-based superalloy with excellent high-temperature tensile properties

    CN113699414B

  • Cobalt-based high-temperature alloy for additive manufacturing, preparation method and application thereof, and additive manufacturing product

    CN111455221A