A high-strength rollable magnesium alloy and its preparation method

By adding Ca and trace amounts of Ce and La elements to magnesium alloys and employing specific smelting and rolling processes, the problem of poor rolling performance of AZ91 magnesium alloys has been solved, achieving a combination of high strength and good plasticity, making it suitable for industrial production.

CN118147500BActive Publication Date: 2026-11-10SHANGHAI INST OF TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410301250.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-15
Publication Date
2026-11-10
Estimated Expiration
2044-03-15

AI Technical Summary

Technical Problem

The existing AZ91 magnesium alloy has poor rolling performance, making it difficult to achieve a combination of high strength and good plasticity, and there are problems with uneven deformation during casting and extrusion.

Method used

High-strength rollable magnesium alloys are prepared by adding small amounts of Ca and trace amounts of Ce and La elements to magnesium alloys, combined with specific smelting and rolling processes. The specific processes include smelting, casting, multi-pass rolling, and annealing.

Benefits of technology

High room temperature strength and plasticity of magnesium alloys have been achieved, with room temperature tensile strength reaching 290-310 MPa, yield strength 180-210 MPa, and elongation 10-17%, and the process is simple and easy to industrialize.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention relates to a high-strength rollable magnesium alloy and its preparation method. The magnesium alloy has the following mass percentage composition: Al: 8.5-9.5%, Zn: 0.60-1.5%, Ca: 0.15-0.3%, Ce: 0.01-0.3%, La: 0.001-0.008%, with impurities of Si <0.02%, Fe <0.05%, Cu <0.003%, and the balance being Mg. This magnesium alloy can be rolled on a magnesium alloy sheet rolling mill. After annealing, its room temperature tensile strength is 290-310 MPa, its yield strength is 180-210 MPa, and its elongation is 10-17%. The room temperature mechanical properties of this magnesium alloy are higher than those of the commercially available AZ91 alloy in both extruded and die-cast states. This method for preparing high-strength rollable magnesium alloy material has the advantages of simple melt treatment, good rolling processing performance, high room temperature mechanical properties, and low cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a high-strength rollable magnesium alloy and its preparation method, belonging to the field of metallic materials. Background Technology

[0002] Magnesium alloys are currently the lightest metallic structural materials used in practical applications, possessing advantages such as high specific stiffness and strength, strong electromagnetic shielding and vibration resistance, excellent machinability, and good damping properties. Therefore, they are widely used in aerospace, automotive, and 3C products. Due to their close-packed structure, magnesium alloys have poor room-temperature forming properties. Currently, AZ series alloys are among the most widely used commercial magnesium alloy series. This is because a small number of magnesium alloys, such as AZ31 and AZ61, can be formed by rolling, but these two alloys have relatively low strength. AZ91 magnesium alloy has higher strength; the widely used cast magnesium alloy AZ91 has a maximum tensile strength of 280 MPa, while the highest strength American standard cast magnesium alloy ZK61 only reaches a maximum tensile strength of 310 MPa. AZ91 magnesium alloy not only has high strength but also good corrosion resistance. AZ series alloys are mainly composed of α-Mg matrix and β-Mg matrix. 17 Al 12 Phase composition, β-Mg in the alloy 17 Al 12 The phase precipitates below 380℃, but due to the high aluminum content of AZ91, β-Mg... 17 Al 12 The phase distribution changes from a dispersed granular distribution to a discontinuous network distribution, which leads to a decrease in the plasticity of the material.

[0003] Rare earth elements can improve the properties of magnesium alloys. Liu Liang et al. [Reference 1: Special Casting and Nonferrous Alloys, 2018, 38(12): 1374-1378] added 0.5-1.0 wt.% Ce to AZ91 alloy and found that the addition of Ce can improve the grain nucleation efficiency and inhibit its growth, thereby achieving the effect of refining the grains.

[0004] Hu Yong et al. [Reference 2: Journal of Materials Heat Treatment, 2014, 35(4): 121-126] added Ce to AZ91 magnesium alloy, resulting in the formation of fine Al4Ce phase, thereby improving the wear resistance, mechanical properties and corrosion resistance of magnesium alloy.

[0005] Dong Yixuan [Reference 3: Master's thesis, Shandong University of Science and Technology, 2020] studied the influence of Ce on the microstructure and mechanical properties of die-cast AZ91 magnesium alloy.

[0006] Wu Anru [Reference 4: Special Casting and Nonferrous Alloys, 2019, Vol.39, No.3, 247-251] studied the effects of rare earth Ce on the grain size and interdendritic compound distribution of as-cast AZ91 magnesium alloy. He found that 0.2 wt.% Ce can refine the grain size of AZ91 alloy and increase the age hardening rate of AZ91 extruded sheet, but 0.5 wt.% Ce reduces the age hardening rate of AZ91 extruded sheet.

[0007] Adding a small amount of alkaline earth element Ca to AZ series alloys can improve the microstructure and enhance their mechanical and formability. Feng et al. [Reference 5: Rare Metal Materials and Engineering, 2015, 44(001): 41-47] found that the addition of Ca can improve the high-temperature performance of magnesium alloys and effectively prevent ignition and oxidation of magnesium alloys during melting. The Al2Ca phase formed by Ca makes β-Mg 17 Al 12 The phase size is significantly reduced, improving the microstructure of AZ91D magnesium alloy.

[0008] Xiao Ran [Reference 6: Master's Thesis, Shanghai Jiao Tong University, 2020] studied the influence of Ca on the microstructure and mechanical properties of AZ91-Ce magnesium alloy in rheological extrusion casting. AZ91-1Ce-xCa (x=0, 1.0, 2.0, 3.0wt%) was produced by gravity casting, die casting, and rheological extrusion casting. AZ91-xCe (x=0, 0.2, 0.5, 0.7, 1.0wt%) magnesium alloy was developed using the extrusion method. The alloy composition was 9.0% Al, 1% Zn, and 0.3% Mn.

[0009] Nie Zhongkui [Reference 7: Master's Thesis, Chongqing University, 2022] studied the effects of 0, 0.4, 0.8 and 1.2 wt.% Ca content and 0.4 wt.% Ce content on the microstructure and properties of AZ91 magnesium alloy, and analyzed the influence of Ca on the microstructure and properties of as-cast, as-cast at different cooling rates and extruded AZ91-0.4Ce-xCa alloy.

[0010] Yang Fan [Reference 8: Doctoral dissertation of Northeastern University, 2018.] studied the effects of Y and Ca on the high-temperature oxidation of AZ91 magnesium alloy and found that 1.5 wt% Ca had the most obvious effect on refining the alloy microstructure, while when the Ca content was 2.0 wt.%, the microstructure was coarsened.

[0011] Chen et al. [Reference 9: Effects of the addition of Ca and Sb on the microstructure and mechanical properties of AZ91 magnesium[J]. Materials Science and Engineering:A,2013,587(10):262-267.] studied the effects of Ca and Sb on the microstructure and mechanical properties of AZ91 magnesium alloy and found that the addition of more than 1.0 wt.% Ca to AZ91 magnesium alloy deteriorated its mechanical properties and also caused severe hot tearing of the alloy.

[0012] Analysis of existing patents and literature reveals that current methods for improving the plasticity of high-strength, corrosion-resistant magnesium alloys primarily involve using industrial-grade AZ91 magnesium alloy ingots as the master alloy. After preheating the ingot to a specific temperature range, rare earth elements and calcium (Ca) are added for modification. These modified AZ91 magnesium alloys mainly focus on the research and development of cast and extruded magnesium alloys, with less research on rolling. However, cast and extruded magnesium alloys, due to factors such as the types and quantities of alloying elements, process parameters, and die design, exhibit the characteristic uneven deformation distribution across the cross-section inherent in extrusion deformation; that is, the microstructure of hot-extruded alloys is typically non-uniform. This significantly limits the application of AZ91. Secondly, research has found that adding Mn to magnesium alloys has almost no effect on tensile strength but does affect plasticity. Therefore, using AZ91 as the master alloy and modifying it by adding rare earth elements, Ca, and other elements cannot achieve the desired high-strength, well-plasticized magnesium alloy. Therefore, based on the characteristics of Al, Zn, Ca, and rare earth elements, it is necessary to formulate a new magnesium alloy composition to achieve a new high-strength magnesium alloy suitable for rolling. Summary of the Invention

[0013] The purpose of this invention is to address the poor rolling performance of existing AZ91 magnesium alloys by providing a high-strength rollable magnesium alloy containing Ca, Ce, and La, and its preparation method. The magnesium alloy manufactured using this invention exhibits high room temperature strength and is easy to cast and roll. The features of this invention are: ① By adding a small amount of alloying element Ca and trace amounts of rare earth elements Ce and La to the alloy, the room temperature plasticity is improved, achieving the purpose of strengthening without significantly increasing the alloy cost. The metallic element Ca has flame-retardant properties, refines the alloy microstructure, and can also improve the high-temperature performance of the alloy.

[0014] To achieve the above objectives, the technical solution of the present invention is: a high-strength rollable magnesium alloy, wherein the mass percentage composition of the magnesium alloy is Al: 8.5-9.5%, Zn: 0.60-1.5%, Ca: 0.15-0.3%, Ce: 0.01-0.3%, La: 0.001-0.008%, impurity elements Si < 0.02%, Fe < 0.05%, Cu < 0.003%, and the balance is Mg.

[0015] A method for preparing a high-strength rollable magnesium alloy involves selecting industrial-grade pure Mg ingots or pure Mg powder and master alloys of MgAl, MgZn, MgCe, MgLa, and MgCa, mixing them according to the mass percentage composition of the magnesium alloy, placing them in a furnace, heating and melting them under a CO2+SF6 protective gas atmosphere, raising the melting temperature to above 710℃, and ensuring the magnesium alloy mixture is completely melted between 710 and 780℃. The melt is then stirred and mixed evenly, allowed to stand for 30 minutes, and then cooled to 680-700℃. Surface slag is removed, and the mixture is then cast.

[0016] First, the surface of the magnesium alloy ingot is planed clean to remove smelting marks. Then, the planed ingot is sent into a heating furnace and heated to a temperature between 380 and 450°C. After holding at this temperature until the temperature inside and outside the ingot is the same, it is sent into a magnesium alloy hot rolling mill for multi-pass rolling of the sheet metal with a total reduction rate of 80 to 90%. The rolled sheet metal is then annealed at a temperature of 320 to 360°C for 30 to 60 minutes.

[0017] The magnesium alloy has a room temperature tensile strength of 290–310 MPa, a yield strength of 180–210 MPa, and an elongation of 10–17%.

[0018] The beneficial effects of this invention are:

[0019] The magnesium alloy of the present invention has a room temperature tensile strength, yield strength, and elongation of 290–310 MPa, 180–2100 MPa, and 10–17%, respectively. Under the same processing conditions, the magnesium alloy of the present invention has improved room temperature strength and toughness indicators (tensile strength 230 MPa, yield strength 140 MPa, elongation 3%) compared to the AZ91 alloy.

[0020] The magnesium alloy manufactured using this invention exhibits high room temperature strength and is easy to cast and roll. The features of this invention are: ① By adding a small amount of alloying element Ca and trace amounts of rare earth elements Ce and La to the alloy, its room temperature plasticity is improved, achieving the goal of strengthening without significantly increasing the alloy cost. Metallic element Ca has flame-retardant properties, refines the alloy microstructure, and can also improve the alloy's high-temperature performance. Rare earth elements Ce and La can improve the plastic processing properties of magnesium alloys and are inexpensive. Secondly, the smelting and rolling process of this alloy is simple and easy to implement for industrial production. Detailed Implementation

[0021] The present invention discloses a high-strength rollable magnesium alloy, wherein the alloy has the following mass percentage composition: Al: 8.5-9.5%, Zn: 0.60-1.5%, Ca: 0.15-0.3%, Ce: 0.01-0.3%, La: 0.001-0.008%, impurity elements Si < 0.02%, Fe < 0.05%, Cu < 0.003%, and the balance being Mg.

[0022] The high-strength rollable magnesium alloy preparation method of the present invention involves selecting industrial pure Mg ingots or pure Mg powder and intermediate alloys such as MgAl, MgZn, MgCe, MgLa and MgCa, and mixing them according to the mass percentage composition of the alloys. The mixture is then placed in a furnace and heated to melt under a CO2+SF6 protective gas. The melting temperature is raised to above 710°C, and the magnesium alloy mixture is completely melted between 710 and 780°C. The melt is stirred and mixed evenly, allowed to stand for 30 minutes, and then cooled to 680-700°C. Surface slag is removed, and the mixture is then cast.

[0023] First, the surface of the magnesium alloy ingot is planed clean to remove smelting marks. Then, the planed ingot is sent into a heating furnace and heated to a temperature between 380 and 450°C. After holding at this temperature until the temperature inside and outside the ingot is the same, it is sent into a conventional magnesium alloy hot rolling mill for multi-pass rolling of the sheet metal with a total reduction rate of 80 to 90%. The rolled sheet metal is then annealed at a temperature of 320 to 360°C for 30 to 60 minutes.

[0024] The magnesium alloy has a room temperature tensile strength of 290–310 MPa, a yield strength of 180–210 MPa, and an elongation of 10–17%.

[0025] Case Study: Industrial pure magnesium ingots are mixed with appropriate amounts of intermediate alloys such as MgAl, MgZn, MgCe, MgLa and MgCa and placed in a furnace. The mixture is heated and melted under a protective gas at a temperature of 780°C. After complete melting, the mixture is stirred and stirred evenly. The mixture is left to stand for 30 minutes, then cooled to 680°C. The surface slag is removed, and the mixture is die-cast to a thickness of 10 mm.

[0026] The composition of the obtained castings is shown in the table below (by mass percentage):

[0027] Mg Al Zn Ca Ce La Other impurities 89.71 9.0 1.0 0.25 0.10 0.001 margin

[0028] Magnesium alloy ingots are heated to around 450℃ and held until the internal and external temperatures are uniform before being fed into a conventional hot-rolling mill for magnesium alloys. This allows for multi-pass rolling of the sheet metal, resulting in a final rolled thickness of 1mm. The rolled sheet metal is then annealed at 330℃ for 30 minutes. Tensile test specimens are prepared from the sheet metal, and the room temperature properties are measured to be σ. s=310MPa, σ b =204MPa, elongation 14%.

Claims

1. A high-strength rollable magnesium alloy, characterized in that: The magnesium alloy has the following mass percentage composition: Al: 8.5~9.5%, Zn: 0.60~1.5%, Ca: 0.15~0.3%, Ce: 0.01~0.3%, La: 0.001~0.008%, impurity elements Si<0.02%, Fe<0.05%, Cu<0.003%, with the balance being Mg; the room temperature tensile strength of the magnesium alloy is 290~310MPa, the yield strength is 180~210MPa, and the elongation is 10~17%.

2. A method for preparing the high-strength rollable magnesium alloy according to claim 1, characterized in that: Industrial-grade pure Mg ingots or pure Mg powder are selected and mixed with MgAl, MgZn, MgCe, MgLa and MgCa master alloys according to the weight percentage of the magnesium alloy composition. The mixture is then placed in a furnace and heated to melt under CO2+SF6 protective gas. The melting temperature is raised to above 710℃, and the magnesium alloy is completely melted between 710~780℃. The melt is stirred and mixed evenly, and allowed to stand for 30 minutes. Then, the temperature is lowered to 680~700℃, the surface slag is removed, and the mixture is cast.

3. The method for preparing high-strength rollable magnesium alloy according to claim 2, characterized in that: First, the surface of the magnesium alloy ingot is planed clean to remove smelting marks. Then, the planed ingot is sent into a heating furnace and heated to a temperature between 380 and 450°C. After holding at this temperature until the temperature inside and outside the ingot is the same, it is sent into a magnesium alloy hot rolling mill for multi-pass rolling of the sheet metal with a total reduction rate of 80 to 90%. The rolled sheet metal is then annealed at a temperature of 320 to 360°C for 30 to 60 minutes.

Citation Information

Patent Citations

  • Creep-resistant Mg-Al wrought magnesium alloy and preparation method thereof

    CN115652158A