A yolk-shell type catalyst, its preparation method and application
By constructing an egg yolk-eggshell type Ni@SiO2 catalyst, the problems of easy sintering and carbon deposition of nickel-based catalysts in alcohol-water reforming reactions were solved, achieving high activity and high stability in alcohol-water reforming hydrogen production.
Patent Information
- Application Number
- CN202211581997.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-09
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-12-09
AI Technical Summary
Traditional nickel-based catalysts are prone to sintering and have poor resistance to carbon deposition in alcohol-water reforming reactions, which leads to a rapid decline in catalyst activity and limits their industrial application prospects.
The Ni@SiO2 catalyst with an egg yolk-eggshell structure improves the activity and stability of nickel-based catalysts by constructing a cavity-containing coating structure and modifying it with additives.
It effectively inhibits catalyst sintering, increases the exposure of nickel metal active sites, improves mass transfer efficiency, and enhances the catalyst's resistance to carbon deposition and high-temperature stability.
Smart Images

Figure BDA0003991665400000081 
Figure BDA0003991665400000091 
Figure BDA0003991665400000131
Abstract
Description
Technical Field
[0001] This application relates to an egg yolk-eggshell type catalyst, its preparation method and application, belonging to the field of alcohol-water reforming hydrogen production technology. Background Technology
[0002] Hydrogen energy is an effective means to address the dual needs of carbon neutrality and economic development. Currently, domestic hydrogen production mainly comes from coal gasification and natural gas reforming. Although the cost is low, the production process involves steam reforming (CO + H2O → CO2 + H2), resulting in high carbon dioxide emissions, reaching 22–35 kg CO2 / kg H2 and 10–16 kg CO2 / kg H2, respectively. Therefore, developing low-carbon emission hydrogen production methods has become a pressing scientific problem for the academic community. Utilizing carbon-neutral biomass energy to produce hydrogen is widely recognized as an effective method with the potential to significantly reduce carbon emissions. In various alcohol solutions prepared from biomass raw materials, methanol, ethanol, and ethylene glycol can react with water vapor under the action of a catalyst to produce a mixture of gases such as CO2, CO, and H2. High-purity hydrogen can then be produced through further separation. Furthermore, each of the three bio-alcohols has its own advantages in hydrogen production. Methanol, lacking C-C bonds, can undergo reforming at low temperatures of 200–300°C; ethanol is non-toxic, easy to store, and easy to transport; and ethylene glycol, as the simplest diol, has low volatility and toxicity. A steam reforming hydrogen production process based on these three alcohols can efficiently produce hydrogen while mitigating the greenhouse effect and reducing organic waste pollution, making it of significant research importance.
[0003] For alcohol-water reforming reactions, the required catalyst should possess excellent CH and CO bond dissociation capabilities, but this often leads to rapid carbon deposition on the catalyst. Furthermore, under high-temperature and complex component reaction conditions, the active metal is prone to sintering and growth, resulting in a rapid decline in catalyst performance. Literature reports indicate that noble metal catalysts such as Pt, Ru, Rh, and Pd exhibit high activity and selectivity in alcohol-water reforming reactions, but their high cost severely limits their industrial application prospects. In contrast, Ni-based catalysts have a relatively low cost (Renewable Sustainable Energy Rev. 2015, 44, 132) and excellent activation performance for CH, CC, and OH bonds, making them a research hotspot. However, for traditional supported Ni-based catalysts, when the metal-support interaction is weak, Ni metal is prone to sintering, or the formation of carbon deposits (usually carbon whiskers) causes Ni to detach from the support, resulting in loss of activity. Conversely, when the metal-support interaction is strong, carbon deposits from the alcohol-water reaction easily accumulate on the Ni surface, rapidly covering active sites, leading to catalyst deactivation and insufficient hydrogen production. Therefore, developing high-temperature resistant and carbon-resistant catalysts suitable for hydrogen production from alcohol-water reforming is key to the widespread application of this technology. Summary of the Invention
[0004] To address the problems of traditional nickel-based catalysts such as easy sintering at high temperatures and poor resistance to carbon deposition, this invention provides a metal@oxide (Ni-M@SiO2-X) catalyst with an egg yolk-eggshell structure and its preparation method. By constructing a cavity-containing coating structure and modifying it with additives, the activity and stability of the nickel-based catalyst in the alcohol-water reforming reaction are significantly improved.
[0005] According to one aspect of this application, a yolk-eggshell type catalyst is provided, the catalyst comprising a metallic Ni core and a SiO2 shell, the metallic Ni core being located inside the SiO2 shell, and a cavity being formed between the metallic Ni core and the SiO2 shell.
[0006] Optionally, the diameter of the Ni core of the catalyst is 30-150 nm, the inner diameter of the SiO2 shell is 5-40 nm larger than that of the Ni core, and the thickness of the SiO2 shell is 5-20 nm.
[0007] Optionally, in the catalyst, the content of metallic Ni accounts for 30 to 90 wt% of the catalyst.
[0008] Optionally, in the catalyst, the content of metallic Ni accounts for any value or a range between two values from 30 wt%, 50 wt%, 70 wt%, 90 wt% of the catalyst.
[0009] Optionally, the catalyst further includes metal M and oxide promoter, wherein the metal M and oxide promoter are supported on the catalyst, specifically the metal M and oxide promoter are supported on the inner and outer surfaces of the SiO2 shell and the metal Ni core;
[0010] Wherein, the metal M is selected from at least one of Co, Fe, Cu, Zn, Ru, Pt, and Pd;
[0011] The oxide additive is selected from at least one of La2O3, ZrO2, MgO, BaO, and CaO.
[0012] Optionally, the content of metal M in the catalyst is 0 to 10 wt% of the catalyst;
[0013] The content of the oxide promoter in the catalyst is 0 to 10 wt%.
[0014] Optionally, the content of metal M in the catalyst is any value or a range between two values from 0 wt%, 1 wt%, 2 wt%, 5 wt%, and 10 wt% of the catalyst.
[0015] Optionally, the content of the oxide promoter in the catalyst is any value or a range between two values, which is 0 wt%, 1 wt%, 3 wt%, 5 wt%, or 10 wt% of the catalyst.
[0016] According to another aspect of this application, a method for preparing the above-mentioned catalyst is provided, comprising the following steps:
[0017] a) Under an inactive atmosphere, a nickel precursor, alcohol solution I, and a surfactant are mixed and reacted to obtain nickel particles.
[0018] b) Add the nickel particles described in step a to a solution containing organosilicon, ammonia and ethanol, and react II to obtain the Ni@SiO2 core-shell precursor;
[0019] c) The Ni@SiO2 core-shell precursor described in step b is calcined in a reducing atmosphere to obtain the Ni@SiO2 catalyst.
[0020] Optionally, before step c, the method further includes:
[0021] b-1: The Ni@SiO2 core-shell precursor described in step b is added to an acidic solution and etched to obtain intermediate product I;
[0022] b-2: Mix the intermediate product I with the metal element precursor, impregnate, and dry.
[0023] Optionally, the nickel precursor is selected from C 10 H 14 NiO4 and / or NiCl2.
[0024] Optionally, the alcohol solution I is selected from at least one of 1,5-pentanediol, glycerol, butanol, and ethylene glycol.
[0025] Optionally, the surfactant is selected from at least one of PVP, P123, and F127.
[0026] Optionally, the organosilicon compound is selected from C4H. 12 O4Si, C8H 20 O4Si, C 21 H 46 At least one of O3Si.
[0027] Optionally, the mass ratio of the nickel precursor, alcohol solution I, and surfactant is 1:40-100:3-10.
[0028] Optionally, the mass ratio of the nickel precursor, alcohol solution I, and surfactant is any value or a range between two values from 1:40:3, 1:47.3:3, 1:48:5, 1:49:5, 1:50:5, and 1:100:10.
[0029] Optionally, the mass ratio of the nickel particles, organosilicon, ammonia, and ethanol is 1:0.20-0.25:7-8:15-20.
[0030] Optionally, the mass ratio of the nickel particles, organosilicon, ammonia, and ethanol is any value or a range between two values from 1:0.20:7:15, 1:0.23:7.6:18, 1:0.24:7.7:19, 1:0.25:7.8:20, 1:0.25:7.9:20, and 1:0.25:8:20.
[0031] Optionally, the conditions for reaction I are: temperature 200-240°C, time 1-4 hours.
[0032] Optionally, the temperature of reaction I is selected from any value or a range between two values from 200℃, 210℃, 220℃, 230℃, and 240℃.
[0033] Optionally, the reaction time I is selected from any value of 1h, 2h, 3h, 4h or a range between two values.
[0034] Optionally, the conditions for reaction II are: temperature 15–30°C, time 1–2 h.
[0035] Optionally, the temperature of reaction II is selected from any value of 15°C, 20°C, 25°C, 30°C, or a range between two values.
[0036] Optionally, the reaction time II is selected from any value of 1h, 1.5h, 2h, or a range between two values.
[0037] Optionally, the calcination conditions are: temperature 300-500℃, time 2-4h.
[0038] Optionally, the roasting temperature is selected from any value or a range between two of 300℃, 350℃, 400℃, 450℃, and 500℃.
[0039] Optionally, the roasting time is selected from any value of 2h, 3h, 4h or a range between two values.
[0040] Optionally, the reducing atmosphere is hydrogen, and the volume concentration of the hydrogen is 10-100%.
[0041] Optionally, the volume concentration of the hydrogen gas is selected from any value of 10%, 30%, 50%, 70%, 100%, or a range between two values.
[0042] Optionally, the acidic solution is selected from nitric acid or hydrochloric acid, and the concentration of the acidic solution is 1 to 1.5 mol / L, expressed as moles of hydrogen ions.
[0043] Optionally, the concentration of the acidic solution is selected from any value of 1 mol / L, 1.25 mol / L, 1.5 mol / L, or a range between two values.
[0044] Optionally, the etching conditions are: temperature 15-30°C, time 5-40 min.
[0045] Optionally, the etching temperature is room temperature, and the etching time is selected from any value of 5 min, 10 min, 20 min, 30 min, 40 min, or a range between two values.
[0046] Optionally, the metal element precursor includes a first component precursor and a second component precursor;
[0047] The first component precursor is selected from a soluble salt containing at least one of Co, Fe, Cu, Zn, Ru, Pt, and Pd;
[0048] The second component precursor is selected from a soluble salt containing at least one of La, Zr, Mg, Ba, and Ca.
[0049] The soluble salt of Co is selected from at least one of Co(NO3)2 and CoCl2;
[0050] The soluble salt of Fe is selected from at least one of Fe(NO3)3 and FeCl3;
[0051] The soluble salt of Cu is selected from at least one of Cu(NO3)2 and CuCl2;
[0052] The soluble salt of Zn is selected from at least one of Zn(NO3)2 and ZnCl2;
[0053] The soluble salt of Pt is selected from at least one of Pt(NO3)2 and PtCl2;
[0054] The soluble salts of Ru are selected from RuCl3 and N4O. 10 At least one of Ru;
[0055] The soluble salt of Pd is selected from at least one of Pd(NO3)2 and PdCl2;
[0056] The soluble salt of La is selected from at least one of La(NO3)2, LaCl3 and La2(SO4)3;
[0057] The soluble salt of Zr is selected from at least one of ZrO(NO3)2 and ZrCl4;
[0058] The soluble salt of Mg is selected from at least one of Mg(NO3)2 and MgCl2;
[0059] The soluble salt of Ba is selected from at least one of Ba(NO3)2 and BaCl2;
[0060] The soluble salt of Ca is selected from at least one of Ca(NO3)2 and CaCl2.
[0061] Optionally, the mass ratio of the intermediate product to the metal element precursor is 1:0 to 0.1, based on the mass of the metal element.
[0062] Optionally, the mass ratio of the intermediate product to the metal element precursor is any value among 0, 1:0.05, 1:0.075, and 1:0.1, or a range between two values.
[0063] Optionally, the immersion temperature is 15–30°C, and the immersion time is 12–24 hours.
[0064] Optionally, the immersion temperature is selected from any value of 15°C, 20°C, 25°C, 30°C, or a range between two values.
[0065] Optionally, the immersion time is selected from any value of 12h, 16h, 18h, 20h, 24h or a range between two values.
[0066] Optionally, the drying temperature is 60–80°C.
[0067] According to another aspect of this application, a reaction for the preparation of hydrogen from an alcohol-water mixture is provided, wherein an aqueous solution of an alcohol is contacted with a catalyst and reacted to obtain a hydrogen-containing mixture.
[0068] The catalyst is selected from the above-described catalysts or the catalysts obtained according to the above preparation method.
[0069] Optionally, the mass ratio of the catalyst to the alcohol is 1:1.5 to 30.
[0070] Optionally, the mass ratio of the catalyst to the alcohol is any value or a range between two values from 1:1.5, 1:5, 1:15, 1:20, and 1:30.
[0071] Optionally, the alcohol is selected from at least one of methanol, ethanol, and ethylene glycol.
[0072] Optionally, the molar ratio of the alcohol to water is 1:1 to 10.
[0073] Optionally, when the alcohol is methanol, the molar ratio of alcohol to water is 1:1 to 3;
[0074] When the alcohol is ethanol, the molar ratio of alcohol to water is 1:3 to 10;
[0075] When the alcohol is ethylene glycol, the molar ratio of alcohol to water is 1:3 to 5.
[0076] The reaction conditions are a temperature of 200–800°C and a pressure of 1–10 bar.
[0077] Optionally, when the alcohol is methanol, the reaction temperature is 200–400°C;
[0078] When the alcohol is ethanol or ethylene glycol, the reaction temperature is 500–800℃.
[0079] The beneficial effects that this application can produce include:
[0080] 1) The yolk-shell type catalyst provided in this application can effectively inhibit catalyst sintering and has a high metal loading compared with traditional supported catalysts, thus giving the catalyst both high activity and high stability.
[0081] 2) Compared with ordinary core-shell structure catalysts, the yolk-shell type catalyst provided in this application has more exposed nickel metal active sites, adjustable metal size, and the cavity between metal and oxide can effectively promote mass transfer while improving the stability of the core-shell structure.
[0082] 3) The yolk-eggshell type catalyst provided in this application can improve the reactivity of metallic Ni through metal doping, and the oxide modification can enhance the synergistic effect of metal promoters and the stability of silica shell, thereby significantly improving the anti-carbon deposition performance and high-temperature stability of the yolk@eggshell structure catalyst. Attached Figure Description
[0083] Figure 1 This is a SEM image of Ni metal from Example 1 of this application;
[0084] Figure 2 HRTEM image of the core-shell structure catalyst prepared in Example 1 of this application;
[0085] Figure 3 The images shown are SEM and HRTEM images of the egg yolk-eggshell catalyst prepared in Example 2 of this application, with the left image being the SEM image and the right image being the HRTEM image. Detailed Implementation
[0086] The present application is described in detail below with reference to the embodiments, but the present application is not limited to these embodiments.
[0087] Unless otherwise specified, all raw materials used in the embodiments of this application were purchased through commercial channels.
[0088] The analysis method in the embodiments of this application is as follows:
[0089] Catalyst morphology was analyzed using scanning electron microscopy (SEM) and transmission electron microscopy (TEM).
[0090] The reaction products were analyzed using gas chromatography (6890N).
[0091] Example 1:
[0092] Preparation of Ni@SiO2 catalysts with core-shell structure
[0093] A nickel precursor (2.1 g) and a surfactant (PVP) were added to a 1,5-pentanediol solution at a mass ratio of 1:5. The mixture was stirred and heated to 200 °C for 4 h under an argon atmosphere, then heated to 240 °C for 1 h. After the solution cooled to room temperature, 100 ml of acetone solution was added, and the mixture was washed repeatedly by centrifugation with ethanol. The resulting nickel nanoparticles were dispersed in an appropriate amount of ethanol solution, and 0.2 ml of C4H4O was added. 12 O4Si, 0.2ml C 21 H 46 O3Si and 4 ml of 7.4 mol / ml ammonia water were stirred at room temperature for 1 h, and then washed repeatedly by centrifugation with ethanol. The catalyst was placed in a vacuum oven and dried at room temperature for 13 h. The dried catalyst was calcined at 500 °C for 2 h under a hydrogen atmosphere to obtain a Ni@SiO2 catalyst with a core-shell structure.
[0094] Example 2:
[0095] Preparation of Ni@SiO2 catalysts with yolk-shell structure
[0096] A nickel precursor (2.1 g) and a surfactant (PVP) were added to a 1,5-pentanediol solution at a mass ratio of 1:5. The mixture was stirred and heated to 200 °C for 4 h under an argon atmosphere, then heated to 240 °C for 1 h. After the solution cooled to room temperature, 100 ml of acetone solution was added, and the mixture was washed repeatedly by centrifugation with ethanol. The resulting nickel nanoparticles were then dispersed in an appropriate amount of ethanol solution, and 0.2 ml of C4H4O was added. 12 O4Si, 0.2ml C 21 H 46O3Si and 4 ml of 7.4 mol / ml ammonia water were stirred at room temperature for 1 h, and then washed repeatedly by centrifugation with ethanol. The obtained active metal nickel@silicon oxide shell catalyst was then dispersed in an appropriate amount of ethanol, and 11 ml of 1.0 mol / L hydrochloric acid solution was added and stirred for 30 min, and then washed repeatedly by centrifugation with ethanol. The catalyst was placed in a vacuum oven and dried at room temperature for 13 h. The dried catalyst was calcined at 500 °C for 2 h under a hydrogen atmosphere to obtain a Ni@SiO2 catalyst with an egg yolk-eggshell structure.
[0097] The catalysts of Examples 1 and 2 were characterized by scanning electron microscopy (SEM) and transmission electron microscopy (TEM) to observe their microstructure.
[0098] according to Figure 1 It is known that nickel nanoparticles exhibit polycrystalline properties, and due to the magnetic interaction between particles, the particles automatically arrange themselves into chains.
[0099] according to Figure 2 It can be seen that after SiO2 lattice modification, the surface of Ni particles is covered with a uniform SiO2 oxide shell.
[0100] according to Figure 3 The HRTEM image shows that after acid treatment, a clear cavity appears between the SiO2 shell and the Ni core of the Ni@SiO2 core-shell catalyst, thus forming an egg yolk-eggshell structure, which maximizes the contact between Ni metal and reactants.
[0101] Example 3:
[0102] Following the method shown in Example 2, the surfactant (PVP) was replaced with one or more mixtures of P123 and F127, and the effects of different surfactants on the active metal size of the catalyst were compared (Table 1).
[0103] Table 1. Comparison of the effects of different types of surfactants on the size of active metals in catalysts.
[0104]
[0105] As shown in Table 1, compared with several surfactant components, PVP and P123 have the best inhibitory effect on Ni particle growth. Moreover, when PVP and P123 are mixed, their synergistic effect can further reduce the size of Ni metal particles. In addition, when the mass ratio of surfactant to metal increases, Ni catalysis is significantly reduced. When the mass ratio of PVP-P123 mixed surfactant to metal Ni reaches 5:1, the size of the active metal of Ni catalyst is reduced to a minimum of 64 nm. Further increasing the mass ratio to 10:1, the reduction in Ni particle size is not significant. Therefore, in the following preparation, a 1:1 mixture of PVP-P123 is preferred as the surfactant, and the mass ratio of surfactant to metal is 5:1.
[0106] Example 4:
[0107] Following the method shown in Example 2, except that the surfactant was replaced with a 1:1 mixture of PVP-P123, a Ni@SiO2 catalyst with an egg yolk-eggshell structure was prepared. The effects of different acid etching conditions on the size of the active metal in the yolk-eggshell catalyst were compared by changing the type, concentration, temperature, and time of the etching active metal acid (Table 2).
[0108] Table 2. Effect of different acid etching conditions on the size of nickel metal with yolk-shell catalyst activity.
[0109]
[0110] As can be seen from Table 2, different acid etching conditions have a significant impact on the size of active nickel metal with egg yolk-eggshell catalyst. As the etching time increases, the metal particle size gradually decreases, but when the etching time is extended to 60 min, the nickel particles are almost completely dissolved. Compared with hydrochloric acid, nitric acid has a faster etching rate and the particle size is more difficult to control. Therefore, hydrochloric acid with a concentration of 1 mol / min and an etching time of 30 min are preferred. The following examples are all preferred etching conditions.
[0111] Example 5:
[0112] Preparation of a 5 wt.% M / Ni@SiO2 catalyst
[0113] The nickel precursor and surfactant (PVP-P123 in a 1:1 ratio) were added to a 1,5-pentanediol solution at a mass ratio of 1:5. The mixture was stirred and heated to 200°C for 4 hours under an argon atmosphere, then heated to 240°C for 1 hour. After cooling to room temperature, 100 ml of acetone solution was added, and the mixture was washed repeatedly by centrifugation with ethanol. The resulting nickel nanoparticles were then dispersed in an appropriate amount of ethanol solution, and 0.2 ml of C4H4O was added. 12 O4Si, 0.2ml C 21 H 46O3Si and 4 ml of 7.4 mol / ml ammonia water were stirred at room temperature for 1 h, and then washed repeatedly by centrifugation with ethanol. The obtained active metal nickel@silicon oxide shell catalyst was then dispersed in an appropriate amount of ethanol, and 11 ml of 1.0 mol / L acid solution was added and stirred for 30 min. After washing repeatedly by centrifugation with ethanol, the catalyst was placed in a vacuum oven and dried at room temperature for 13 h. The dried catalyst was calcined at 500 °C for 2 h under a hydrogen atmosphere to obtain a Ni@SiO2 catalyst with an egg yolk-eggshell structure.
[0114] 1g of Ni@SiO2 catalyst with an egg yolk-eggshell structure was placed in a beaker; 1.3mL of a 40.5mg / mL solution of metal precursors (cobalt, iron, copper, zinc, ruthenium, platinum, and palladium) was measured and added dropwise to the beaker, and stirred evenly until the sample formed viscous droplets, at which point stirring was stopped; after standing for 4h, the sample was placed in a vacuum drying oven and dried at 60℃ under vacuum for 6h; after drying, the catalyst was calcined at 500℃ for 2h under H2 atmosphere to obtain the metal-modified Ni@SiO2 egg yolk-eggshell structure catalyst.
[0115] Example 6:
[0116] Same as Example 5, except that the calcination conditions of the metal-modified Ni@SiO2 yolk-shell structure catalyst were changed. The concentration of hydrogen in the calcination atmosphere (H2 / Ar of 10%, 50%, and 100%), the calcination temperature (300°C, 400°C, and 500°C), and the calcination time (2h and 4h) were also changed.
[0117] Example 7:
[0118] Preparation of Co / Ni@SiO2 catalyst with a loading of X wt.%
[0119] The nickel precursor and surfactant (PVP-P123 in a 1:1 ratio) were added to a 1,5-pentanediol solution at a mass ratio of 1:5. The mixture was stirred and heated to 200°C for 4 hours under an argon atmosphere, then heated to 240°C for 1 hour. After cooling to room temperature, 100 ml of acetone solution was added, and the mixture was washed repeatedly by centrifugation with ethanol. The resulting nickel nanoparticles were then dispersed in an appropriate amount of ethanol solution, and 0.2 ml of C4H4O was added. 12 O4Si, 0.2ml C 21 H 46O3Si and 4 ml of 7.4 mol / ml ammonia water were stirred at room temperature for 1 h, and then washed repeatedly by centrifugation with ethanol. The obtained active metal nickel@silicon oxide shell catalyst was then dispersed in an appropriate amount of ethanol, and 11 ml of 1.0 mol / L acid solution was added and stirred for 30 min. After washing repeatedly by centrifugation with ethanol, the catalyst was placed in a vacuum oven and dried at room temperature for 13 h. The dried catalyst was calcined at 500 °C for 2 h under a hydrogen atmosphere to obtain a Ni@SiO2 catalyst with an egg yolk-eggshell structure.
[0120] 1 g of Ni@SiO2 catalyst with an egg yolk-eggshell structure was placed in a beaker; 1.3 mL of cobalt solution with a concentration of Y g / mL (Table 3) was measured and added dropwise to the beaker. The mixture was stirred until it formed viscous droplets, at which point the stirring was stopped; after standing for 4 h, the sample was placed in a vacuum drying oven and dried at 60 °C for 6 h; after drying, the catalyst was calcined at 500 °C for 2 h under H2 atmosphere to obtain Co-modified Ni@SiO2 egg yolk-eggshell structure catalyst.
[0121] Table 3. Preparation of Ni@SiO2 catalysts modified with different Co contents DD220923I-DL
[0122] Co loading / wt.% <![CDATA[Metal solution concentration / mg·ml -1 > 1 7.8 2 15.7 5 40.5 10 85.5
[0123] Example 8:
[0124] Preparation of a 5Co-Ni@SiO2-5X catalyst (X being La2O3, ZrO2, MgO, BaO, or CaO) with a Co loading of 5 wt.% and a M loading of 5 wt%.
[0125] The nickel precursor and surfactant (PVP-P123 in a 1:1 ratio) were added to a 1,5-pentanediol solution at a mass ratio of 1:5. The mixture was stirred and heated to 200°C for 4 hours under an argon atmosphere, then heated to 240°C for 1 hour. After cooling to room temperature, 100 ml of acetone solution was added, and the mixture was washed repeatedly by centrifugation with ethanol. The resulting nickel nanoparticles were then dispersed in an appropriate amount of ethanol solution, and 0.2 ml of C4H4O was added. 12 O4Si, 0.2ml C 21 H 46 O3Si and 4 ml of 7.4 mol / ml ammonia water were stirred at room temperature for 1 h, and then washed repeatedly by centrifugation with ethanol. The obtained active metal nickel@silicon oxide shell catalyst was then dispersed in an appropriate amount of ethanol, and 11 ml of 1.0 mol / L acid solution was added and stirred for 30 min. After washing repeatedly by centrifugation with ethanol, the catalyst was placed in a vacuum oven and dried at room temperature for 13 h. The dried catalyst was calcined at 500 °C for 2 h under a hydrogen atmosphere to obtain a Ni@SiO2 catalyst with an egg yolk-eggshell structure.
[0126] 1g of Ni@SiO2 catalyst with an egg yolk-eggshell structure was placed in a beaker; 0.5ml of a cobalt solution with a concentration of 105.3mg / ml and a solution containing 0.8ml of a metal precursor (lanthanum, cadmium, magnesium, barium, and calcium) with a concentration of 65.8mg / ml were measured and added dropwise to the beaker. The mixture was stirred until the sample formed viscous droplets, at which point stirring was stopped; after standing for 4h, the sample was placed in a vacuum drying oven and dried at 60℃ under vacuum for 6h; after drying, the catalyst was calcined at 500℃ for 2h under H2 atmosphere to obtain the oxide-modified 5Co-Ni@SiO2-5X egg yolk-eggshell structure catalyst.
[0127] Example 9:
[0128] Preparation of 5Co-Ni@SiO2-YLa2O3 catalysts with different La loadings (Co loading 5 wt.%)
[0129] The nickel precursor and surfactant (PVP-P123 in a 1:1 ratio) were added to a 1,5-pentanediol solution at a mass ratio of 1:5. The mixture was stirred and heated to 200°C for 4 hours under an argon atmosphere, then heated to 240°C for 1 hour. After cooling to room temperature, 100 ml of acetone solution was added, and the mixture was washed repeatedly by centrifugation with ethanol. The resulting nickel nanoparticles were then dispersed in an appropriate amount of ethanol solution, and 0.2 ml of C4H4O was added. 12 O4Si, 0.2ml C 21 H 46 O3Si and 4 ml of 7.4 mol / ml ammonia water were stirred at room temperature for 1 h, and then washed repeatedly by centrifugation with ethanol. The obtained active metal nickel@silicon oxide shell catalyst was then dispersed in an appropriate amount of ethanol, and 11 ml of 1.0 mol / L acid solution was added and stirred for 30 min. After washing repeatedly by centrifugation with ethanol, the catalyst was placed in a vacuum oven and dried at room temperature for 13 h. The dried catalyst was calcined at 500 °C for 2 h under a hydrogen atmosphere to obtain a Ni@SiO2 catalyst with an egg yolk-eggshell structure.
[0130] 1g of Ni@SiO2 catalyst with yolk-shell structure was placed in a beaker; 0.5ml of cobalt solution with a concentration of 105.3mg / ml and 0.8ml of La solution with a concentration of Z mg / ml (Table 4) were measured and added dropwise to the beaker. The mixture was stirred until the sample formed viscous droplets, and then the stirring was stopped. After standing for 4h, the sample was placed in a vacuum drying oven and dried at 60℃ under vacuum for 6h; after drying, the catalyst was calcined at 500℃ for 2h under H2 atmosphere to obtain 5Co-Ni@SiO2-YLa2O3 catalyst.
[0131] Table 4. Preparation of 5Co-Ni@SiO2-YLa2O3 catalysts with different La loadings
[0132] La loading / wt.% <![CDATA[Metal solution concentration / mg·ml -1 > 1 12.6 3 38.6 5 65.8 10 138.9
[0133] Example 10:
[0134] The performance of the catalyst prepared in Example 2 in the ethanol-water steam reforming hydrogen production reaction was evaluated using a fixed-bed reactor. 100 mg of Ni@SiO2 yolk-shell structured catalyst was placed in a stainless steel reaction tube, along with 500 mg of quartz sand. The tube was heated to different reaction temperatures using an electric heater under an inert atmosphere at a heating rate of 10 °C / min. Before the reaction, the tube was purged with N2 for 5 minutes, followed by the introduction of alcohol solutions with different molar ratios. Nitrogen gas was added as an internal standard at a flow rate of 20 mL / min. The reactants were vaporized through an evaporator using a constant flow pump (0.1 mL / min) and passed through the catalyst bed. The reaction was carried out under set temperature and pressure conditions. The gaseous components were directly introduced into a 6890N gas chromatograph directly connected to the reactor for real-time analysis of the yield of each substance in the gas phase reaction. The conversion rate of reactant C2H5OH and the gas selectivity S were calculated. i (i = H2, CO, CO2, CH4).
[0135] The methods for calculating reactant conversion and product selectivity are as follows:
[0136]
[0137]
[0138] Where n pi This refers to the molar concentration of gaseous products in the outlet gas. The gaseous products include H2, CO, CO2, and CH4, and the overall carbon balance of the reaction is above 95%.
[0139] Table 5. Reaction performance test of Ni@SiO2 yolk-shell structure catalyst
[0140]
[0141] The reactants are all in molar ratios
[0142] The ethanol steam reforming reaction is a typical endothermic reaction (C2H5OH + 3H2O = 6H2 + 2CO2). As shown in Table 5, under conditions of a feed flow rate of 0.1 ml / min, a reactant molar ratio of C2H5OH:H2O of 1:3, and a reaction pressure of 1 bar, increasing the reaction temperature to 800℃ gradually increases the ethanol conversion and H2 selectivity. Furthermore, the reactant composition and reaction pressure both significantly affect the catalyst performance; a higher water-to-ethanol ratio and lower reaction pressure result in higher H2 selectivity.
[0143] Example 11:
[0144] Ni@SiO2 yolk-shell structured catalysts containing different types of surfactants (surfactant to nickel mass ratio of 5:1) were prepared according to the preparation steps described in Examples 2 and 4. Their reactivity in ethanol steam reforming for hydrogen production was compared according to the method shown in Example 10 (Table 4). The reaction temperature was 700℃, the pressure was 1 bar, and the reactant composition C2H5OH:H2O molar ratio was 1:10.
[0145] Table 6. Performance Comparison of Ni@SiO2 Yolk-Shell Structure Catalysts Containing Different Types of Surfactants
[0146]
[0147] As can be seen from Table 6, the ethanol conversion rate and H2 selectivity of the catalyst gradually increase as the particle size decreases.
[0148] Example 12:
[0149] Following the method shown in Example 10, the catalyst was replaced with the Ni@SiO2 core-shell structure catalyst prepared in Example 1. The reaction performance of Ni@SiO2 core-shell structure catalyst and Ni@SiO2 yolk-eggshell structure catalyst under different acid etching conditions in ethanol steam reforming for hydrogen production was compared (Table 7). The reaction temperature was 700℃, the pressure was 1 bar, and the molar ratio of reactant C2H5OH:H2O was 1:10.
[0150] Table 7. Performance comparison of Ni@SiO2 core-shell structure and Ni@SiO2 yolk-eggshell structure catalysts
[0151]
[0152] As shown in Table 7, compared with traditional core-shell catalysts, the Ni@SiO2 catalyst with an eggshell structure exhibits superior performance in the ethanol steam reforming hydrogen production reaction. Comparatively, the Ni@SiO2 eggshell structure catalyst etched with 1 mol / min hydrochloric acid for 30 min shows slightly better activity than the catalyst etched for 10 min. Therefore, the preferred etching solution for the reaction is 1 mol / min hydrochloric acid, etched for 30 min to prepare the Ni@SiO2 eggshell structure catalyst.
[0153] Example 13:
[0154] Table 8 compares the performance of Ni@SiO2 yolk-shell structure catalysts impregnated with different metals, following the method shown in Example 10. The reaction temperature was 700℃, the pressure was 1 bar, and the molar ratio of C2H5OH:H2O to the reactants was 1:10.
[0155] Table 8. Performance comparison of Ni@SiO2 yolk-shell structure catalysts with different metal modifications
[0156]
[0157]
[0158] As can be seen from Table 8, the reaction performance of the egg yolk-eggshell structure catalysts modified by active metals Co, Fe, Cu, Zn, Ru, Pt and Pd is improved to a certain extent. Among them, active metals Co and Fe greatly improve the conversion rate of C2H5OH and the selectivity of H2.
[0159] Example 14:
[0160] Catalysts with different calcination temperatures were prepared according to the preparation steps described in Examples 5 and 6, and their performance was compared according to the method shown in Example 10 (Table 9). After optimizing the reaction temperature, the calcination conditions were adjusted to further compare the reaction activity of the catalysts. The reaction temperature was 700°C, the pressure was 1 bar, and the molar ratio of C2H5OH:H2O in the reactants was 1:10.
[0161] Table 9. Comparison of reaction performance of 5 wt.% Co / Ni@SiO2 yolk-shell structure catalysts under different calcination conditions
[0162]
[0163] As shown in Table 9, the 5wt.% Co / Ni@SiO2 egg yolk-eggshell structure catalyst C2H5OH produced under calcination conditions of 500℃ for 2h in a 100% H2 / Ar atmosphere exhibited the highest conversion rate and H2 selectivity, demonstrating the best reaction performance.
[0164] Example 15
[0165] Effects of different Co loadings on the reaction performance of Ni@SiO2 yolk-shell structure catalysts:
[0166] Ni@SiO2 yolk-eggshell structure catalysts with different metal loadings were prepared according to the steps described in Example 7. The different catalysts were evaluated according to the method shown in Example 10, and the reaction performance of Ni@SiO2 yolk-eggshell structure catalysts with different Co loadings was compared (Table 10). The reaction temperature was 700℃, the pressure was 1 bar, and the molar ratio of C2H5OH:H2O in the reactants was 1:10.
[0167] Table 10. Performance comparison of Ni@SiO2 yolk-shell structure catalysts modified with different metal loadings
[0168]
[0169] As shown in Table 10, the conversion rate of C2H5OH first increases and then decreases with increasing loading. Considering all factors, 5wt.% Co / Ni@SiO2 exhibits superior performance.
[0170] Example 16:
[0171] Effects of different 5wt.% Co / Ni@SiO2 yolk-shell structure catalysts modified with different co-metal oxides on reaction performance:
[0172] 5 wt.% Co / Ni@SiO2 yolk-shell structure catalysts modified with different metal oxide promoters were prepared according to the steps described in Example 8. Different catalysts were evaluated according to the method shown in Example 10, and the reaction performance of the 1 wt.% Co / Ni@SiO2 yolk-shell structure catalysts modified with different metal oxide promoters was compared (Table 11). The reaction temperature was 700℃, the pressure was 1 bar, and the molar ratio of C2H5OH:H2O in the reactants was 1:10.
[0173] Table 11. Comparison of performance of 1 wt.% Co / Ni@SiO2 yolk-shell structure catalysts modified with different auxiliary metal oxides
[0174]
[0175]
[0176] Table 11 shows that the performance of the 5 wt.% Co / Ni@SiO2 yolk-shell structure catalysts modified with different auxiliary metal oxides was improved to some extent. All catalysts achieved a C2H5OH conversion rate higher than 90% in the reaction. Among them, the La2O3 and ZrO2-modified 5 wt.% Co / Ni@SiO2 yolk-shell structure catalysts showed higher H2 selectivity, while the La2O3-supported catalyst exhibited superior performance. Therefore, the La2O3-modified catalyst is preferred.
[0177] Example 17:
[0178] Effect of different loadings of La-modified 5wt.% Co / Ni@SiO2 yolk-shell structure catalysts on reaction performance:
[0179] Following the steps described in Example 9, 5 wt.% Ni@SiO2 yolk-shell structure catalysts modified with co-metal oxides of different La loadings were prepared. The different catalysts were evaluated according to the method shown in Example 10, and the reaction performance of the 5 wt.% Co / Ni@SiO2 yolk-shell structure catalysts modified with different co-metal oxide loadings was compared (Table 12). The reaction temperature was 700℃, the pressure was 1 bar, and the reactant composition (C2H5OH:H2O molar ratio) was 1:10.
[0180] Table 12. Performance comparison of 5wt.% Co / Ni@SiO2 yolk-shell structure catalysts modified with different La loadings
[0181]
[0182] As can be seen from Table 12, different loadings of the co-metal oxide have a significant impact on the catalyst's reaction performance. The catalyst modified with 3 wt.% La2O3 has better performance. Therefore, the co-metal oxide with a mass fraction of 3 wt.% La2O3 is preferred for catalyst modification.
[0183] Example 18:
[0184] A fixed-bed reactor was used to evaluate the stability of the catalyst in the ethanol-water steam reforming hydrogen production reaction. 100 mg of the 5Co-Ni@SiO2-3La2O3 yolk-shell structured catalyst was placed in a stainless steel reaction tube, along with 500 mg of quartz sand. The reactor was heated to different reaction temperatures using an electric heater under an inert atmosphere at a heating rate of 10 °C / min. Before the reaction, the reactor was purged with N2 for 5 minutes, followed by the introduction of alcohol solutions with different molar ratios. Nitrogen gas was added as an internal standard at a flow rate of 20 mL / min. The reactants were vaporized through an evaporator using a constant flow pump (0.1 mL / min) and passed through the catalyst bed. The reaction was carried out for 400 min under set temperature and pressure conditions. The gaseous components were directly analyzed in real-time using a 6890N gas chromatograph directly connected to the reactor. The conversion rate of C2H5OH and the gas selectivity (S) were calculated. i (i = H2, CO, CO2, CH4).
[0185] Table 13.5 Stability Tests of Co-Ni@SiO2-3La2O3 Yolk-Shell Structure Catalysts
[0186]
[0187]
[0188] As can be seen from Table 13, the 5Co-Ni@SiO2-3La2O3 reaction exhibits good stability within 300 min, and the reactivity does not show a significant decrease.
[0189] Example 19:
[0190] A fixed-bed reactor was used to evaluate the stability of the catalyst in the ethylene glycol steam reforming hydrogen production reaction. 100 mg of a yolk-shell structured 5Co-Ni@SiO2-3La2O3 catalyst was placed in a stainless steel reaction tube, along with 500 mg of quartz sand. The tube was heated to different reaction temperatures using an electric heater under an inert atmosphere at a rate of 10 °C / min. Before the reaction, the tube was purged with N2 for 5 minutes, followed by the introduction of alcohol solutions with different molar ratios. Nitrogen gas was added as an internal standard at a flow rate of 20 mL / min. The reactants were vaporized through an evaporator using a constant flow pump (0.1 mL / min) and passed through the catalyst bed. The reaction was carried out under set temperature and pressure conditions. The gaseous components were directly fed into a 6890N gas chromatograph connected directly to the reactor for real-time analysis of the yield of each substance in the gas phase reaction. The conversion rate of reactant (CH2OH)2 and the gas selectivity (S) were calculated. i (i = H2, CO, CO2, CH4).
[0191] The methods for calculating reactant conversion and product selectivity are as follows:
[0192]
[0193]
[0194] Where n pi This refers to the molar concentration of gaseous products (including H2, CO, CO2, and CH4) in the outlet gas, with the overall carbon balance of the reaction being above 95%.
[0195] Table 14.5 Reaction performance test of Co-Ni@SiO2-3La2O3 yolk-shell structure catalyst
[0196]
[0197] DD220923I-DL
[0198]
[0199] The reactants are all in molar ratios
[0200] As shown in Table 14, under conditions of a feed flow rate of 0.1 ml / min, a reactant molar ratio of (CH2OH)2:H2O of 1:3, and a reaction pressure of 1 bar, increasing the reaction temperature to 700 °C gradually increases the ethylene glycol conversion and H2 selectivity. Furthermore, the effect of the water-to-ethanol ratio on catalyst performance is discussed; a higher water-to-ethanol ratio, lower reaction pressure, and higher H2 selectivity are observed.
[0201] Example 20:
[0202] A fixed-bed reactor was used to evaluate the stability of the catalyst in the methanol-water steam reforming hydrogen production reaction. 100 mg of a 1Co-Ni@SiO2-3La2O3 yolk-shell structured catalyst was placed in a stainless steel reaction tube, along with 500 mg of quartz sand. The tube was heated to different reaction temperatures using an electric heater under an inert atmosphere at a heating rate of 10 °C / min. Before the reaction, the tube was purged with N2 for 5 minutes, followed by the introduction of alcohol solutions with different molar ratios. Nitrogen gas was added as an internal standard at a flow rate of 20 mL / min. The reactants were vaporized through an evaporator using a constant flow pump (0.1 mL / min) and passed through the catalyst bed. The reaction was carried out under set temperature and pressure conditions. The gaseous components were directly fed into a 6890N gas chromatograph connected directly to the reactor for real-time analysis of the yield of each substance in the gas phase reaction. The conversion rate of CH3OH and the gas selectivity (S) were calculated. i (i = H2, CO, CO2, CH4).
[0203] The methods for calculating reactant conversion and product selectivity are as follows:
[0204]
[0205]
[0206] Where n pi This refers to the molar concentration of gaseous products (including H2, CO, CO2, and CH4) in the outlet gas, with the overall carbon balance of the reaction being above 95%.
[0207] Table 15.1 Reaction performance test of Co-Ni@SiO2-3La2O3 yolk-shell structure catalyst
[0208]
[0209] The reactants are all in molar ratios
[0210] As shown in Table 15, under conditions of a feed flow rate of 0.1 ml / min, a CH3OH:H2O molar ratio of 1:1, and a reaction pressure of 1 bar, increasing the reaction temperature to 300℃ gradually increases the CH3OH conversion and H2 selectivity. Furthermore, the effect of the water-to-alcohol ratio on catalyst performance is discussed; a higher water-to-alcohol ratio, lower reaction pressure, and higher H2 selectivity are observed.
[0211] The above description is merely a few embodiments of this application and is not intended to limit this application in any way. Although this application discloses preferred embodiments as described above, it is not intended to limit this application. Any changes or modifications made by those skilled in the art without departing from the scope of the technical solution of this application using the disclosed technical content are equivalent to equivalent implementation cases and fall within the scope of the technical solution.
Claims
1. A reaction for hydrogen production via alcohol-water reforming, characterized in that, An aqueous solution of alcohol is contacted with a catalyst to react and produce a mixed gas containing hydrogen. The catalyst is an egg yolk-eggshell type catalyst, comprising a metallic Ni core and a SiO2 shell, wherein the metallic Ni core is located inside the SiO2 shell, and there is a cavity between the metallic Ni core and the SiO2 shell; The catalyst further includes metal M and oxide promoter, wherein metal M and oxide promoter are supported on the catalyst; Wherein, the metal M is selected from at least one of Co, Fe, Cu, Zn, Ru, Pt, and Pd; The oxide additive is selected from at least one of La2O3, ZrO2, MgO, BaO, and CaO.
2. The reaction according to claim 1, characterized in that, The mass ratio of the catalyst to the alcohol is 1:1.5~30; The alcohol is selected from at least one of methanol, ethanol, and ethylene glycol; The molar ratio of the alcohol to water is 1:1 to 10; The reaction conditions are a temperature of 200~800℃ and a pressure of 1~10 bar.
3. The reaction according to claim 1, characterized in that, The catalyst has a Ni core with a diameter of 30-150 nm, an inner diameter of SiO2 shell that is 5-40 nm larger than the Ni core, and a shell thickness of 5-20 nm. In the catalyst, the content of metallic Ni accounts for 30 to 90 wt% of the catalyst.
4. The reaction according to claim 1, characterized in that, In the catalyst, the content of metal M accounts for 1~10 wt% of the catalyst. The content of oxide promoter in the catalyst is 1 to 10 wt%.
5. The reaction according to claim 1, characterized in that, The catalyst is prepared by a method comprising the following steps: a) Under an inactive atmosphere, a nickel precursor, alcohol solution I, and a surfactant are mixed and reacted to obtain nickel particles. b) Add the nickel particles described in step a to a solution containing organosilicon, ammonia and ethanol, and react II to obtain the Ni@SiO2 core-shell precursor; b-1: The Ni@SiO2 core-shell precursor described in step b is added to an acidic solution and etched to obtain intermediate product I; b-2: Mix the intermediate product I with the metal element precursor, impregnate, and dry; the metal element precursor includes a first component precursor and a second component precursor; the first component precursor is selected from a soluble salt containing at least one of Co, Fe, Cu, Zn, Ru, Pt, and Pd. The second component precursor is selected from a soluble salt containing at least one of La, Zr, Mg, Ba, and Ca; c) In a reducing atmosphere, the dried product described in step b-2 is calcined to obtain the egg yolk-eggshell type catalyst.
6. The reaction according to claim 5, characterized in that, In the method for preparing the catalyst, the metallic nickel precursor is selected from C 10 H 14 NiO4 and / or NiCl2; The alcohol solution I is selected from at least one of 1,5-pentanediol, glycerol, butanol, and ethylene glycol; The surfactant is selected from at least one of PVP, P123, and F127; The organosilicon compound is selected from C4H. 12 O4Si, C8H 20 O4Si, C 21 H 46 At least one of O3Si.
7. The reaction according to claim 5, characterized in that, In the preparation method of the catalyst, the mass ratio of the nickel precursor, alcohol solution I, and surfactant is 1:40~100:3~10; The mass ratio of the nickel particles, organosilicon, ammonia, and ethanol is 1:0.20~0.25:7~8:15~20; The conditions for reaction I are: temperature 200~240℃, time 1~4h; The conditions for reaction II are: temperature 15~30℃, time 1~2h; The calcination conditions are: temperature 300~500℃, time 2~4h; The reducing atmosphere is hydrogen, and the volume concentration of hydrogen is 10-100%.
8. The reaction according to claim 5, characterized in that, In the method for preparing the catalyst, the acidic solution is selected from nitric acid or hydrochloric acid, and the concentration of the acidic solution is 1~1.5 mol / L, expressed as molar hydrogen ions. The etching conditions are: temperature 15~30℃, time 5~40min; The mass ratio of intermediate product I to the metal element precursor is 1:0.05~0.1, based on the mass of the metal element; The immersion temperature is 15~30℃, and the immersion time is 12~24h; The drying temperature is 60~80℃.