A method for quantitatively characterizing the inhomogeneity of amorphous alloys
By acquiring the force curve point by point on the surface of the amorphous alloy sample and using the fitting model, the problem of difficulty in characterizing the inhomogeneity in the existing technology is solved, the direct and accurate quantitative characterization of the inhomogeneity of the amorphous alloy is achieved, and the Test range improves accuracy and repeatability of results.
Patent Information
- Application Number
- CN202410314031.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-19
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-03-19
AI Technical Summary
Existing technology is difficult to effectively quantify, directly and accurately characterize the inhomogeneity of amorphous alloys. The scanning range is limited and cannot fully reflect the internal structure information of the material.
By obtaining force curve information point by point on the surface of the amorphous alloy sample, using the Derjaguin-Muller-Toporov model to fit the modulus value, and fitting the modulus-probability density diagram with a Gaussian function to obtain the full width at half peak to determine the inhomogeneity. Achieve quantitative characterization.
It achieves direct and accurate quantitative characterization of the inhomogeneity of amorphous alloys, expands the test area, ensures the accuracy and repeatability of data, and can more intuitively reflect the degree of inhomogeneity of different samples.
Smart Images

Figure CN118169352B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of amorphous alloy characterization, and in particular to a method for quantitatively characterizing the inhomogeneity of an amorphous alloy. Background Art
[0002] The information disclosed in the background of the invention is only intended to enhance the understanding of the overall background of the invention and should not be necessarily regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Amorphous alloy, also known as metallic glass, is a new type of metal material. Unlike traditional crystalline alloys that have long-range ordered atomic structure characteristics, amorphous alloys do not have long-range translational order and are a disordered structure under a non-equilibrium system. At the same time, unlike the completely uniform disordered system such as ideal gas, amorphous alloys have intrinsic inhomogeneity, which manifests as short-range order and medium-range order structural characteristics. In other words, the intrinsic structural inhomogeneity properties are hidden in the long-range disorder characteristics of amorphous alloys. The inhomogeneity characteristics of amorphous alloys are closely related to the physical properties of the material. It is of great scientific and application significance to establish the correspondence between the structure and performance of amorphous alloys based on the inhomogeneity characteristics.
[0004] In order to deeply understand the inhomogeneity characteristics of amorphous alloys, the first task is to characterize their inhomogeneity. The current inhomogeneity characterization methods are still immature. For example, the scanning range of high-energy transmission electron microscopy to characterize inhomogeneity characteristics is limited to tens of nanometers, and the phase inhomogeneity distribution obtained by amplitude modulation mode atomic force microscopy cannot directly represent the inhomogeneous structure of amorphous samples.
[0005] Therefore, how to provide a method that can quantitatively, directly and accurately characterize the inhomogeneous structure of amorphous alloys is an urgent problem to be solved. Summary of the invention
[0006] In view of this, the present invention provides a method for quantitatively characterizing the inhomogeneity of amorphous alloys. The present invention directly obtains force curve information on the sample surface and simultaneously performs a large-scale point-by-point scanning on the selected area, thereby ultimately obtaining a quantitative, direct and accurate amorphous alloy inhomogeneous structural distribution map.
[0007] The present invention provides a method for quantitatively characterizing the inhomogeneity of an amorphous alloy, comprising the following steps:
[0008] Control the nanoprobe to scan point by point in the area to be scanned of the amorphous alloy sample to generate a pressure-displacement curve for each point;
[0009] The pressure-displacement curve is fitted using the Derjaguin-Muller-Toporov model to obtain the modulus value corresponding to each point;
[0010] Performing statistical analysis on the modulus value, fitting the modulus-probability density graph using a Gaussian function, and obtaining the full width at half maximum of the fitting curve;
[0011] The inhomogeneity of the amorphous alloy sample was judged based on the full width at half maximum.
[0012] In the present invention, the larger the half-maximum full width, the more dispersed the modulus distribution in the scanned area, that is, the greater the degree of inhomogeneity, so the purpose of quantitatively characterizing the inhomogeneity of the amorphous alloy can be achieved by comparing the half-maximum full width values.
[0013] In the present invention, there is no special limitation on the shape of the area to be scanned. For example, a rectangle, a square, a circle, etc. may be selected. For easier scanning, the area to be scanned in the present invention is preferably a square.
[0014] Preferably, before the step of controlling the nanoprobe to scan point by point in the area to be scanned of the amorphous alloy sample, the step of fixing the amorphous alloy sample to keep the upper surface of the amorphous alloy sample horizontal is also included. Before scanning the amorphous alloy sample, the present invention needs to ensure that the upper surface of the amorphous alloy sample is flat and free of pollution. For example, the amorphous alloy sample can be pre-treated by surface polishing, ultrasonic cleaning, etc.
[0015] Furthermore, the method of fixing the amorphous alloy sample includes fixing by air pressure adsorption, fixing by spring clips or fixing by magnetic attraction.
[0016] Preferably, before the step of controlling the nanoprobe to scan point by point in the area to be scanned of the amorphous alloy sample, the method further includes the steps of setting the scanning resolution and setting the maximum pressure value. The scanning resolution is the number of points scanned by the nanoprobe in the area to be scanned, which can be set by the user and can be selected from 64, 128, 256, 512, etc. The maximum pressure value is the turning point of the nanoprobe's pressing-withdrawal.
[0017] Furthermore, the process of controlling the nanoprobe to scan point by point in the area to be scanned of the amorphous alloy sample is as follows: controlling the nanoprobe to press into the sample, and withdrawing from the sample surface after reaching the maximum pressure value, thereby completing the scanning of one point; after adjusting the position of the nanoprobe, repeating the steps of "pressing into the sample, and withdrawing from the sample surface after reaching the maximum pressure value" until the scanning of all points in the area to be scanned is completed.
[0018] Preferably, the nanoprobe is controlled by a pressure-displacement control system, which includes a pressure-displacement sensor and a pressure-displacement controller; wherein the pressure-displacement sensor is used to record and feedback the pressure and relative displacement value between the nanoprobe and the amorphous alloy sample in real time; and the pressure-displacement controller is used to adjust the position of the nanoprobe to complete the scanning of all points in the area to be scanned.
[0019] Furthermore, the upper end of the nanoprobe is connected to a pressure-displacement sensor.
[0020] Preferably, the fitting of the pressure-displacement curve using the Derjaguin-Muller-Toporov model is specifically to fit the pressure-displacement curve of the stage of evacuating the sample surface after reaching the maximum pressure value using the Derjaguin-Muller-Toporov model.
[0021] Furthermore, the fitting formula is:
[0022]
[0023] Where h is the distance between the amorphous alloy sample and the nanoprobe, F is the pressure, R is the radius of curvature of the nanoprobe tip, and E is r is the reduced modulus; the modulus value E of the amorphous alloy sample is further obtained by the following formula:
[0024]
[0025] Where v is the Poisson’s ratio of the amorphous alloy sample, E s and v s are the modulus and Poisson's ratio of the nanoprobe, respectively.
[0026] Preferably, the determination coefficient R of the fitting curve obtained by fitting the modulus-probability density graph using a Gaussian function is 2 >0.95. The determination coefficient R of the fitting curve 2 It reflects the quality of the fit, thus determining the accuracy of the judgment of the unevenness of the modulus distribution. 2 The closer it is to 1, the higher the fitting quality.
[0027] Compared with the prior art, the present invention has achieved the following beneficial effects:
[0028] (1) The method for quantitatively characterizing the inhomogeneity of amorphous alloys provided by the present invention can characterize the inhomogeneity by directly obtaining the pressure-displacement curve information between the amorphous alloy and the nanoprobe, which can more directly and accurately reflect the internal structure information of the amorphous sample, and it is also easier to quantitatively evaluate the degree of inhomogeneity of different samples without processing complex and nonlinear measurement signals;
[0029] (2) The point-by-point scanning method in the method provided by the present invention helps to expand the test area and can observe and characterize the inhomogeneity of amorphous alloys on a large scale, rather than being limited to a tiny area of tens of nanometers or even a few nanometers, thereby ensuring the accuracy and repeatability of the data results. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The drawings constituting part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their description are used to explain the present invention and do not constitute an improper limitation of the present invention. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative work.
[0031] Figure 1 1. It is a front view and a top view of a schematic diagram of the structure of a device for quantitatively characterizing the inhomogeneity of an amorphous alloy according to Example 1 of the present invention;
[0032] Figure 2 is the pressure-displacement curve obtained in Example 2 of the present invention;
[0033] Figure 3 are modulus distribution diagrams of the areas to be scanned in Examples 2 and 3 of the present invention, wherein (a) Example 2, (b) Example 3;
[0034] Figure 4 2 are probability density statistical analysis results (scatter points) and Gaussian fitting result diagrams (solid lines) of Example 2 and Example 3 of the present invention; wherein, (a) Example 2; (b) Example 3;
[0035] In the figure, 1, sample support platform; 2, amorphous alloy sample; 301, nanoprobe; 302, pressure-displacement sensor; 303, pressure-displacement controller; 201, area to be scanned. DETAILED DESCRIPTION
[0036] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0037] The technical solution of the present invention is further described below in conjunction with specific embodiments. In the following embodiments, the amorphous alloy sample is a lanthanum-based amorphous alloy sample.
[0038] Example 1
[0039] This embodiment provides a device for quantitatively characterizing the inhomogeneity of an amorphous alloy. Figure 1 The device specifically comprises: a sample carrier 1, an amorphous alloy sample 2, a nanoprobe 301, a pressure-displacement sensor 302 and a pressure-displacement controller 303; wherein the amorphous alloy sample 2 is fixed on the sample carrier 1; the upper end of the nanoprobe 301 is connected to the pressure-displacement sensor 302, and the lower end is in good contact with the amorphous alloy sample 2; Figure 3 The top view in FIG. 2 shows the area 201 to be scanned.
[0040] The pressure-displacement sensor 302 and the pressure-displacement controller 303 together constitute a pressure-displacement control system. On the one hand, the pressure between the nanoprobe 301 and the amorphous alloy sample 2 is controlled by the pressure-displacement controller 303. On the other hand, the pressure-displacement sensor 302 is used to feedback the pressure value in real time and record the pressure value and displacement value of the whole process.
[0041] Example 2
[0042] This embodiment provides a method for quantitatively characterizing the inhomogeneity of an amorphous alloy. The following operation is based on the device of Embodiment 1 and specifically includes the following steps:
[0043] (1) Polishing and ultrasonic cleaning are performed on the surface of the amorphous alloy sample 2 to ensure that the surface is flat and free of contaminants. The amorphous alloy sample 2 is fixed on the sample support table 1 by magnetic attraction, and the upper surface of the amorphous alloy sample 2 to be tested is kept horizontal;
[0044] (2) The area to be scanned 201 on the amorphous alloy sample 2 is selected as a square area to be scanned 201 of 500*500 nm, and the scanning resolution is set to 256, and the maximum pressure value is set to 190 nN;
[0045] (3) Scanning the first point from the upper left corner of the area to be scanned 201, and controlling the nanoprobe 301 to gradually approach the amorphous alloy sample 2 through the pressure-displacement control system. After contacting the amorphous alloy sample 2, the pressure-displacement controller 303 gradually increases the pressure, and the tip of the nanoprobe 301 causes a certain degree of deformation on the upper surface of the amorphous alloy sample 2. After reaching the maximum pressure value, the pressure-displacement controller 303 withdraws the probe and leaves the sample surface, and finally completes a "press-withdraw" process;
[0046] (4) During the “press-in-withdraw” process, the pressure-displacement sensor 302 records and feeds back the pressure and relative displacement between the nanoprobe 301 and the amorphous alloy sample 2 in real time, generating a corresponding pressure-displacement curve, such as Figure 2 As shown;
[0047] (5) Scan the entire area to be scanned 201 line by line, repeating the “press-and-withdraw” process for each point until the test of area A is completed;
[0048] (6) The pressure-displacement curve results corresponding to each point are extracted, and the Derjaguin-Muller-Toporov (DMT) model is used to fit the withdrawal segment to obtain the modulus value corresponding to each point. The fitting formula is shown as follows:
[0049]
[0050] Where h is the distance between the amorphous alloy sample 2 and the nanoprobe 301, F is the pressure, and R is the radius of curvature of the tip of the nanoprobe 301. The reduced modulus E can be obtained by fitting: r The modulus value E of the amorphous alloy sample 2 is further obtained by the following formula:
[0051]
[0052] Where v is the Poisson's ratio of amorphous alloy sample 2, E s and v s are the modulus and Poisson's ratio of the nanoprobe 301 , respectively.
[0053] The modulus value corresponding to each point is used to obtain the modulus distribution diagram of the area to be scanned 201, such as Figure 3 As shown in (a), it can be seen that the amorphous alloy sample 2 in this embodiment has obvious structural inhomogeneity.
[0054] (7) Perform statistical analysis on the modulus value corresponding to each point, and use Gaussian function to fit the modulus value-probability density map to obtain the corresponding half-maximum full width, such as Figure 4 As shown in (a), the full width at half maximum of region A is 18.9 GPa, R 2 is 0.99, which has a high fitting quality.
[0055] Example 3
[0056] Compared with the embodiment 2, the difference is that the area 201 to be scanned in this embodiment is area B.
[0057] In this embodiment, the modulus value corresponding to each point is obtained to obtain the modulus distribution diagram of the area to be scanned 201 as shown in Figure 3 The modulus distribution diagram can be used to qualitatively determine the degree of inhomogeneity, and it can be seen that the amorphous alloy sample 2 in this embodiment has obvious structural inhomogeneity, but its degree of inhomogeneity is smaller than that of region A in embodiment 2.
[0058] This embodiment uses a Gaussian function to fit the modulus value-probability density diagram to obtain the corresponding half-maximum full width, such as Figure 4 As shown in (b), the full width at half maximum of region B is 13.8 GPa, R 2 The half-peak full width of region B is less than that of region A, indicating that the degree of inhomogeneity in region B is less than that in region A from a quantitative point of view.
[0059] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for quantitatively characterizing the inhomogeneity of an amorphous alloy, characterized in that: The steps include: Control the nanoprobe to scan point by point in the area to be scanned of the amorphous alloy sample to generate a pressure-displacement curve for each point; The pressure-displacement curve is fitted using the Derjaguin-Muller-Toporov model to obtain the modulus value corresponding to each point; Performing statistical analysis on the modulus value, fitting the modulus-probability density graph using a Gaussian function, and obtaining the full width at half maximum of the fitting curve; The inhomogeneity of the amorphous alloy sample was determined based on the full width at half maximum value; The fitting of the pressure-displacement curve using the Derjaguin-Muller-Toporov model specifically includes fitting the pressure-displacement curve of the stage of evacuating the sample surface after reaching the maximum pressure value using the Derjaguin-Muller-Toporov model; The formula for fitting the pressure-displacement curve of the stage of evacuating the sample surface after reaching the maximum pressure value using the Derjaguin-Muller-Toporov model is: Where h is the distance between the amorphous alloy sample and the nanoprobe, F is the pressure, R is the radius of curvature of the nanoprobe tip, and E is r is the reduced modulus; the modulus value E of the amorphous alloy sample is further obtained by the following formula: Where v is the Poisson’s ratio of the amorphous alloy sample, E s and v s are the modulus and Poisson’s ratio of the nanoprobe, respectively; The determination coefficient R of the fitting curve obtained by fitting the modulus-probability density graph using the Gaussian function 2 >0.
95.
2. The method according to claim 1, characterized in that Before the step of controlling the nanoprobe to scan point by point in the area to be scanned of the amorphous alloy sample, the method also includes the step of fixing the amorphous alloy sample to keep the upper surface of the amorphous alloy sample horizontal.
3. The method according to claim 2, characterized in that The method of fixing the amorphous alloy sample includes air pressure adsorption fixation, spring clamp fixation or magnetic attraction fixation.
4. The method according to claim 1, characterized in that Before the step of controlling the nanoprobe to scan point by point in the area to be scanned of the amorphous alloy sample, the step of setting the scanning resolution and setting the maximum pressure value is also included.
5. The method according to claim 4, characterized in that The process of controlling the nanoprobe to scan point by point in the area to be scanned of the amorphous alloy sample is as follows: controlling the nanoprobe to press into the sample, and withdraw from the sample surface after reaching the maximum pressure value, thereby completing the scanning of one point; after adjusting the position of the nanoprobe, repeating the steps of "pressing into the sample, and withdrawing from the sample surface after reaching the maximum pressure value" until the scanning of all points in the area to be scanned is completed.
6. The method according to claim 1, characterized in that The nanoprobe is controlled by a pressure-displacement control system, which includes a pressure-displacement sensor and a pressure-displacement controller.
7. The method according to claim 6, characterized in that The upper end of the nanoprobe is connected to a pressure-displacement sensor.